Treatment method for purifying texture of ox horn button
The treatment of horn buttons through specific chemical treatment liquid solves the problem of unclean texture of horn buttons on the surface and easy to whiten and dirty, achieving the effect of not whitening and not bleaching, improving the added value of the product and market competitiveness, and avoiding spraying of paint Environmental protection issues dealt with.
Patent Information
- Application Number
- CN202411123296.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
The existing horn button production process leads to grayish white and greasy substances on the surface of the product. The overall color and photometric texture are not clean enough, and it is easy to turn white and dirty after machine washing and drying, which cannot meet the customer's needs for not being white or matte. Dealing with environmental protection problems and affecting nature.
Use specific chemical treatment liquids, including citric acid, sodium dodecylbenzenesulfonate and acetic acid, to chemically treat the dry-throwing horn buttons, remove surface impurities and oils, and form a cuticle layer to ensure that the product is It will not turn white or bleach after machine washing and dry cleaning.
The overall surface of the horn button is not gray or dirty, and does not matte, which improves the clean color and texture, meets customer needs, avoids the environmental protection problems and natural influence of paint treatment, and improves the added value of the product and market competitiveness. .
Smart Images

Figure BDA0004997607610000021 
Figure BDA0004997607610000041 
Figure BDA0004997607610000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of natural horn button production, relates to the application of a treatment liquid in the preparation of horn buttons and a treatment method for horn buttons, and in particular to a treatment method for purifying the texture of natural horn buttons. Background Art
[0002] Buttons are the fasteners used to connect the two sides of clothes. Their original function was to connect the front of clothes. Now they have gradually developed into something more artistic and decorative in addition to maintaining their original functions. They are also a representative of personalization and multifunctionality of clothing.
[0003] The existing process flow of horn buttons is: blank → sorting → button making → water roller polishing → water rinsing → drying → dry polishing → inspection and packaging. The currently produced horns are directly dry polished after drying and then inspected before shipment. However, the overall appearance and eye holes of the horns will have grayish white and greasy substances on the surface, and the overall color and light texture are not clean enough. After the finished horn buttons are machine washed, dry cleaned, and ironed on the garment, the overall surface will turn white and dirty, and the light will also turn dull. In addition, many brand customers have put forward the use requirements that buttons should not turn dull, white, or dirty when the garment is machine washed or dry cleaned.
[0004] With the strong demand of customers for the quality of horn buttons, although the existing technology also uses spray painting to achieve a treatment process that does not turn white, dirty or matte, it can no longer meet customer expectations. The naturalness of the product does not reflect the essential characteristics of natural materials, and there are also corresponding environmental problems.
[0005] Therefore, how to develop a horn button production process to solve the above-mentioned technical problems existing in the existing process has become one of the urgent issues to be solved by cutting-edge R&D companies and many researchers in the industry. Summary of the invention
[0006] In view of this, the technical problem to be solved by the present invention is to provide an application of a treatment liquid in the preparation of horn buttons and a treatment method for horn buttons, in particular, a treatment method for purifying the texture of natural horn buttons. The treatment method provided by the present invention can achieve the effect that the surface of the horn buttons is not white, dirty, or matte, and can not only achieve color cleanliness and texture improvement, meet the improvement of customer demand for the use of horn products, but also improve the added value of the products, achieve rapid product delivery, and win more customers' orders for horn buttons.
[0007] The present invention provides application of a treatment liquid in preparing horn buttons;
[0008] The treatment liquid, measured by weight, comprises:
[0009]
[0010] Preferably, the acid comprises acetic acid;
[0011] The horn buttons include natural horn buttons.
[0012] Preferably, the application specifically includes improving the surface texture of horn buttons and horn and / or purification.
[0013] Preferably, the preparation of the horn buttons is specifically, after the horn buttons are dry-polished and / or dry-rolled, chemically treating the horn buttons with a treatment liquid;
[0014] The application includes application in forming a stratum corneum on the horn surface of horn buttons.
[0015] Preferably, the application includes cleaning impurities and oil on horn buttons;
[0016] The horn buttons are specifically ordinary horn buttons or laser-processed horn buttons.
[0017] The present invention provides a method for processing horn buttons, comprising the following steps:
[0018] The semi-finished ox-horn button product after dry polishing and / or dry rolling is placed in a chemical treatment liquid for soaking to obtain an ox-horn button;
[0019] The chemical treatment liquid includes the treatment liquid in the application described in any one of the above technical solutions.
[0020] Preferably, before the dry rolling step, the ox horn button blanks are further subjected to one or more steps of sorting, button making, water rolling polishing, cleaning and drying;
[0021] The pH value of the chemical treatment solution is 3-5.
[0022] Preferably, before the dry rolling step, the ox horn button blanks are also subjected to the steps of sorting, button making, water rolling polishing, cleaning and drying in sequence;
[0023] The chemical treatment liquid is specifically obtained by mixing treatment liquid components;
[0024] The mixing time is 2 to 3 minutes.
[0025] Preferably, the soaking time is 2 to 8 minutes;
[0026] The soaking step also includes a cleaning step;
[0027] The processing method can be used to process finished horn buttons.
[0028] Preferably, the horn buttons include horn buttons with natural horn surfaces and horn buttons with natural horn surfaces and laser-treated surfaces;
[0029] The laser marks on the surface of the horn button after laser treatment are yellow laser marks;
[0030] After the yellow laser mark is treated again with a chemical treatment liquid, a laser mark with the same color as the surface matrix of the horn is obtained.
[0031] The present invention provides the use of a treatment liquid in the preparation of ox-horn buttons; the treatment liquid, measured by mass, includes 3 to 6 parts by weight of citric acid, 2 to 5 parts by weight of sodium dodecylbenzene sulfonate, 1 to 2 parts by weight of acid, and 90 to 92 parts by weight of water. Compared with the prior art, the existing ox-horn buttons have white, dirty and greasy appearance on the overall surface and holes, and the color cleanliness and texture are not pure enough. After the buttons are placed in a washing machine on the garment for continuous machine washing and dry cleaning, the overall color of the surface will turn white and dirty, and the original brightness will also become dull. Downstream application companies have put forward the use requirements that the buttons cannot be dull and cannot turn white and dirty after multiple machine washing and dry cleaning. The present invention specially designs a chemical treatment liquid with a specific composition and formula for use in the preparation of ox-horn buttons. The present invention also provides a processing method with specific steps, which processes the ox-horn buttons after dry polishing, and can not only remove the auxiliary materials added during the button shaping punching, water roller polishing and dry polishing, as well as the dirt and oil attached to the button surface, but also participate in the comprehensive reaction of the main components such as protein contained in the ox-horn material itself, so that the color of the button surface is clearer and the color is more obvious, and no adhesion remains. At the same time, a layer of cuticle is formed, so that the buttons will never turn dull and dirty after being used on the garment for a long time. Compared with the original technical solution of spraying transparent paint to meet the requirements of multiple machine washing and dry cleaning of the garment without whitening, dirtiness and dullness. The ox-horn products processed by the present invention do not need to be sprayed with paint at all, and there will be no influence of spraying paint on the naturalness and corresponding environmental protection problems, and the natural nature of the ox-horn buttons is maintained.
[0032] The processing method provided by the present invention can achieve the effect that the surface of the ox-horn button is not white, dirty, or matte as a whole, and can not only achieve clean color and improved texture, meet the customer's demand for the use of ox-horn products, but also improve the added value of the product, achieve rapid product delivery, and win more customers' orders for ox-horn buttons. The present invention solves the problem that with the current further demand of downstream customers for the quality of ox-horn buttons, the existing spray painting process can no longer meet the customer's expectations, and the naturalness of the product cannot reflect the essential characteristics of the natural material, and improves the environmental protection of the processing process. The present invention further improves the competitiveness of ox-horn products in the market, meets the customer's demand for product performance, better broadens the depth and breadth of application of ox-horn products, and produces greater economic effects.
[0033] The processing technology and chemical treatment method of natural horn buttons provided by the present invention give horn buttons a new texture quality, realize a new texture and high performance of natural horn buttons in the auxiliary materials industry, broaden the application of high-end horn button products in clothing accessories, and better match them with current high-end casual clothing to enhance the added value of products, thereby achieving the value enhancement of high-end men's and women's clothing using horn products and a substantial increase in the order volume, meeting the high-end needs of current market customers of business casual men's and women's clothing, and achieving more excellent new quality in the industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a photograph of the appearance of the bright black horn button after machine washing or dry cleaning after being treated in Example 1 of the present invention;
[0035] Figure 2 This is a photo of the appearance of a bright black horn button after machine washing or dry cleaning without the treatment of the present invention;
[0036] Figure 3 This is the appearance of the bright horn button treated with spray paint in the existing process, after machine washing 3 times and dry cleaning 3 times;
[0037] Figure 4 This is a photograph of the appearance of the semi-gloss black horn button after machine washing or dry cleaning after being treated in Example 2 of the present invention;
[0038] Figure 5 This is the appearance of a semi-gloss horn button treated with spray paint in the existing process, after machine washing 3 times and dry cleaning 3 times;
[0039] Figure 6 This is a photograph of the appearance of the semi-gloss coffee-colored horn buttons treated in Example 3 of the present invention after machine washing or dry cleaning. DETAILED DESCRIPTION
[0040] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention rather than limiting the patent claims of the present invention.
[0041] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.
[0042] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably uses analytically pure materials or materials with conventional purity requirements in the field of ox horn button preparation.
[0043] The brands and abbreviations of all raw materials of the present invention are conventional brands and abbreviations in the art. Each brand and abbreviation is clear and definite in the field of its related use. Those skilled in the art can purchase them from the market or prepare them by conventional methods according to the brands, abbreviations and corresponding uses.
[0044] The present invention provides application of a treatment liquid in preparing horn buttons;
[0045] The treatment liquid, measured by weight, comprises:
[0046]
[0047]
[0048] In the present invention, the content of citric acid is 3 to 6 parts by weight, can be 3.5 to 5.5 parts by weight, can be 4 to 5 parts by weight.
[0049] In the present invention, the content of the sodium dodecylbenzene sulfonate is 2 to 5 parts by weight, can be 2.5 to 4.5 parts by weight, can be 3 to 4 parts by weight. Specifically, the sodium dodecylbenzene sulfonate (CAS: 25155-30-0) can be a corresponding product sold by Shandong Shouhua Chemical Co., Ltd.
[0050] In the present invention, the content of the acid is 1 to 2 parts by weight, can be 1.2 to 1.8 parts by weight, can be 1.4 to 1.6 parts by weight.
[0051] In the present invention, the content of water is 90 to 92 parts by weight, can be 90.4 to 91.6 parts by weight, can be 90.8 to 91.2 parts by weight.
[0052] In the present invention, the acid preferably includes acetic acid.
[0053] In the present invention, the horn buttons preferably include natural horn buttons.
[0054] In the present invention, the application specifically preferably includes the application of improving the surface texture of horn buttons and horns and / or purification, and more preferably the application of improving the surface texture of horn buttons and horns or purification.
[0055] In the present invention, the preparation of horn buttons is preferably performed chemically on the horn buttons using a treatment liquid after the horn buttons have been dry-polished and / or dry-rolled, and more preferably performed chemically on the horn buttons using a treatment liquid after the horn buttons have been dry-polished or dry-rolled.
[0056] In the present invention, the application preferably includes application in forming a stratum corneum on the horn surface of horn buttons.
[0057] In the present invention, the application preferably includes cleaning impurities and oil on horn buttons.
[0058] In the present invention, the horn buttons are preferably ordinary horn buttons or laser-treated horn buttons.
[0059] The present invention provides a method for processing horn buttons, comprising the following steps:
[0060] The semi-finished ox-horn button product after dry polishing and / or dry rolling is placed in a chemical treatment liquid for soaking to obtain an ox-horn button;
[0061] The chemical treatment liquid comprises the treatment liquid in the application according to any one of the above claims.
[0062] In the present invention, before the dry rolling step, it is preferred that the ox horn button blanks are subjected to one or more steps of sorting, button making, water roller polishing, cleaning and drying, and more preferably, the ox horn button blanks are subjected to multiple steps of sorting, button making, water roller polishing, cleaning and drying.
[0063] In the present invention, the pH value of the chemical treatment solution is preferably 3 to 5, more preferably 3.4 to 4.6, and more preferably 3.8 to 4.2.
[0064] In the present invention, before the dry rolling step, the steps of sorting, button making, water rolling polishing, cleaning and drying the horn button blanks are preferably included in sequence.
[0065] In the present invention, the chemical treatment liquid is preferably obtained by mixing treatment liquid components.
[0066] In the present invention, the mixing time is preferably 2 to 3 minutes, more preferably 2.2 to 2.8 minutes, and more preferably 2.4 to 2.6 minutes.
[0067] In the present invention, the soaking time is preferably 2 to 8 minutes, more preferably 3 to 7 minutes, and more preferably 4 to 6 minutes.
[0068] In the present invention, the soaking step preferably further includes a cleaning step.
[0069] In the present invention, the processing method can preferably be used to process finished horn buttons.
[0070] In the present invention, the horn buttons preferably include horn buttons whose surface is natural horn and horn buttons whose surface is natural horn and laser-treated.
[0071] In the present invention, the laser traces on the surface of the horn button after laser treatment are preferably yellow laser traces. Specifically, the laser traces in the present invention include laser patterns and / or laser fonts.
[0072] In the present invention, the yellow laser trace is treated again with a chemical treatment liquid, preferably to obtain a laser trace of the same color as the horn surface matrix.
[0073] The process provided by the invention comprises: blank→sorting→button making→water roller polishing→ultrasonic cleaning→drying→dry polishing→chemical treatment→drying→inspection and packaging.
[0074] The present invention processes the horn buttons after dry polishing, mainly to remove the auxiliary materials added during the button shaping and punching, water roller polishing and dry polishing, as well as the dirt and oil attached to the button surface, and at the same time participate in the comprehensive reaction of the main components such as protein contained in the horn material itself, so that the color of the button surface is clearer and the color is more obvious, and no adhesion remains. At the same time, a layer of cuticle is formed, so that the buttons will never turn dull and dirty after being used on the garment for a long time. In order to meet the customer's garment needs of multiple machine washing and dry cleaning without whitening, dirtiness and dullness, the original product is treated by spraying transparent paint to meet the use requirements. The present invention processes horn products, and there is no need for spraying paint, so the natural nature of the horn buttons is maintained.
[0075] The present invention is a complete and detailed overall technical solution, which better guarantees the quality grade of natural horn buttons, further improves the appearance of natural horn buttons, and eliminates the phenomenon of matting, whitening and becoming dirty after machine washing and dry cleaning. The application of the above-mentioned treatment liquid in the preparation of horn buttons and a treatment method for purifying the texture of natural horn buttons can specifically include the following contents:
[0076] The process flow is: blank → sorting → button making → water roller polishing → ultrasonic cleaning → drying → dry roller → chemical treatment → drying → inspection and packaging. Among them, the treatment liquid is used in the chemical treatment step.
[0077] A (natural horn button) texture purification treatment process and the application of the corresponding chemical treatment liquid, including:
[0078] Chemical treatment fluid:
[0079] Citric acid: (industrial grade): 3-6%
[0080] Sodium dodecylbenzenesulfonate: 2-5%
[0081] Acetic acid: 1-2%
[0082] Water: 90-92%
[0083] Chemical treatment process:
[0084] Weigh equal amounts of citric acid, sodium sulfonate, acetic acid and tap water according to the ratio, put them into a plastic bucket and mix them together. Stir evenly with a wooden stick (2 to 3 minutes), control the pH value to 3 to 5, and prepare it for use.
[0085] Place 3 to 6 kg of buttons in a mesh plastic basket, immerse the buttons in the basket into the treatment solution for 2 to 8 minutes, take them out, and rinse them with clean water to remove the chemical additives residue on the product surface.
[0086] The present invention uses semi-finished products that are air-dried for processing horn buttons, which can react with amino acids, proteins and other substances in the material, and can dissolve abrasives and oil substances attached to the button surface during the surface water rolling and dry rolling processes, and at the same time fully react with components such as protein, amino acids, taurine, phosphorus substances and other components contained in the horn material to form oxidized cutin on its surface, so that the overall color is purified and clear, and the characteristics of the natural horn material are more evident, and no attachments are left. The finished horn buttons after the chemical treatment are used will never become dull, white or dirty when machine washed or dry cleaned on garments.
[0087] When the semi-finished natural horn buttons are processed by the present invention, the processing liquid of the special formula of the present invention must be used for processing, so that the processed horn buttons after being used on finished clothes can withstand multiple machine washing, dry cleaning and ironing without whitening, and the glossiness does not dull and other texture functions.
[0088] The surface of the ox-horn button treated with the treatment liquid of the present invention can also be laser treated, and the font will become yellow font. If the yellow font is not needed, the yellow font can be removed by secondary treatment with chemical liquid to make the font color consistent with the color of the substrate. The yellow font after laser treatment can also be retained. At the same time, the yellow font can be protected by spraying protective paint so that it will not disappear due to machine washing, dry cleaning, ironing and other tests. At the same time, the ox-horn button treated with the chemical treatment liquid will enhance the bonding force with the protective paint, and will improve the color fastness of the ox-horn spray-painted button to machine washing and dry cleaning.
[0089] The chemically treated horn button has a clean surface texture and a black color, has no whitish or dull performance, and can withstand continuous machine washing and dry cleaning for 10 times without whitish discoloration or dullness.
[0090] The above content of the present invention provides the application of the treatment liquid in the preparation of ox-horn buttons and a treatment method for purifying the texture of natural ox-horn buttons. The chemical treatment liquid specially designed by the present invention with a specific composition and formula is used in the preparation of ox-horn buttons, and a corresponding treatment method is also provided. The present invention treats the ox-horn buttons after dry polishing, not only removing the auxiliary materials added during the button shaping punching, water roller polishing and dry polishing, as well as the dirt and oil attached to the button surface, but also participating in the comprehensive reaction of the main components such as protein contained in the ox-horn material itself, so that the color of the button surface is clearer and the color is more obvious, and no adhesion remains. At the same time, a layer of cuticle is formed, so that the buttons will never turn dull and dirty after being used on the garment for a long time. Compared with the original technical solution of spraying transparent paint to meet the requirements of multiple machine washing and dry cleaning of the garment without whitening, dirtiness and dullness. The ox-horn products treated by the present invention do not need to be sprayed with paint at all, and there will be no influence of spraying paint on the naturalness and corresponding environmental protection problems, and the natural nature of the ox-horn buttons is maintained.
[0091] The processing method provided by the present invention can achieve the effect that the surface of the ox-horn button is not white, dirty, or matte as a whole, and can not only achieve clean color and improved texture, meet the customer's demand for the use of ox-horn products, but also improve the added value of the product, achieve rapid product delivery, and win more customers' orders for ox-horn buttons. The present invention solves the problem that with the current further demand of downstream customers for the quality of ox-horn buttons, the existing spray painting process can no longer meet the customer's expectations, and the naturalness of the product cannot reflect the essential characteristics of the natural material, and improves the environmental protection of the processing process. The present invention further improves the competitiveness of ox-horn products in the market, meets the customer's demand for product performance, better broadens the depth and breadth of application of ox-horn products, and produces greater economic effects.
[0092] The processing technology and chemical treatment method of natural horn buttons provided by the present invention give horn buttons a new texture quality, realize a new texture and high performance of natural horn buttons in the auxiliary materials industry, broaden the application of high-end horn button products in clothing accessories, and better match them with current high-end casual clothing to enhance the added value of products, thereby achieving the value enhancement of high-end men's and women's clothing using horn products and a substantial increase in the order volume, meeting the high-end needs of current market customers of business casual men's and women's clothing, and achieving more excellent new quality in the industry.
[0093] Experimental results show that the natural horn buttons prepared by the present invention have a clean color texture and soft brightness on the surface, and can withstand continuous machine washing and dry cleaning for 10 times without the surface becoming dull, white or dirty.
[0094] In order to further illustrate the present invention, the application of the treatment liquid provided by the present invention in the preparation of ox-horn buttons and a treatment method of ox-horn buttons are described in detail below in combination with the examples. However, it should be understood that these examples are implemented on the premise of the technical scheme of the present invention, and detailed implementation methods and specific operating procedures are given only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention, and the protection scope of the present invention is not limited to the following examples.
[0095] Example 1
[0096] Horn button texture purification formula composition (%)
[0097] Citric acid: (industrial grade): 3%
[0098] Sodium dodecylbenzenesulfonate: 4%
[0099] Acetic acid: 2%
[0100] Water: 91%.
[0101] The glossy black horn button blanks are shaped and polished with water. After drying, the above-mentioned treatment solution is prepared with the pH value controlled at 4. The buttons are then placed in the treatment solution for 6 minutes. The protein and other substances on the surface of the horn material are reacted to remove the residual dirt on the surface and the holes. After trial production, the overall color, brightness and texture are purer.
[0102] 1. Machine washable: Machine washable ISO 6330-2012 4N; GB / T 8629-2017 4N Textile Household Washing and Drying Test Procedure Test Color Fastness 4.5, Appearance Evaluation Gloss without matte and surface whitening and discoloration;
[0103] 2. Dry cleaning resistance: ISO 3175-2:2010 Professional care of textiles and clothing, color fastness test after dry cleaning and wet cleaning, level 4.5, appearance evaluation gloss without matte and surface whitening and discoloration;
[0104] 3. Color fastness to hot pressing: GB / T 6152-1997 "Textiles - Tests for color fastness - Color fastness to hot pressing" The product surface has no matte, no discoloration, and no staining;
[0105] According to the above standard test, the product as a whole has no appearance wear and tear, light matting, whitening and discoloration on the surface, etc. The overall quality meets the appearance and surface discoloration, rough edges, and no whitening of the auxiliary material product industry standard. In terms of performance, it is resistant to water washing, dry cleaning, and ironing without matting and discoloration. In particular, when it is machine washed 10 times in a row at home, there is no light matting or color change. (The original untreated product will become matte and white after one machine wash and dry cleaning, and the whitening level is 3 to 3.5. After this technology is treated, the product surface will not change in color and light.)
[0106] See also Figure 1 , Figure 1 This is a photograph of the appearance of the bright black horn button after machine washing or dry cleaning after being treated in Example 1 of the present invention.
[0107] See also Figure 2 , Figure 2 This is a photograph of the appearance of a bright black horn button after machine washing or dry cleaning without the treatment of the present invention.
[0108] Depend on Figure 1 and Figure 2 By comparison, it can be seen that the horn buttons that are not treated by the present invention have obvious dullness and whitening in appearance.
[0109] See also Figure 3 , Figure 3 The appearance of the glossy horn button treated with spray paint in the existing process, after machine washing 3 times, and after dry cleaning 3 times. From left to right, they are the appearance of the glossy horn button treated with spray paint, after machine washing 3 times, and after dry cleaning 3 times.
[0110] Depend on Figure 1 and Figure 3 By comparison, it can be seen that the bright horn buttons treated with spray paint are much less natural in appearance than the horn buttons treated by the present invention, and cannot reflect the essential characteristics of natural materials.
[0111] Example 2
[0112] Horn button texture purification formula composition (%)
[0113] Citric acid: (industrial grade): 6%
[0114] Sodium dodecylbenzenesulfonate: 3%
[0115] Acetic acid: 1%
[0116] Water: 90%.
[0117] The semi-gloss black horn button blank is shaped and then water-rolled for semi-gloss. After drying, it is subjected to secondary dry-rolling treatment for gloss. Prepare the treatment solution with a pH value of 3, and then place the button in the treatment solution for 4 minutes to dissolve the protein and other substances in the horn material to remove the white dirt and oil on the overall surface and holes. After trial production, the overall semi-gloss is treated, and the overall color and gloss texture are purer.
[0118] 1. Machine washable: Machine washable ISO 6330-2012 4N; GB / T 8629-2017 4N Textile Household Washing and Drying Test Procedure Test Color Fastness 4.5, Appearance Evaluation Gloss without matte and surface whitening and discoloration;
[0119] 2. Dry cleaning resistance: ISO 3175-2:2010 Professional care of textiles and clothing, color fastness test after dry cleaning and wet cleaning, level 4.5, appearance evaluation gloss without matte and surface whitening and discoloration;
[0120] 3. Color fastness to hot pressing: GB / T 6152-1997 "Textiles - Tests for color fastness - Color fastness to hot pressing" The product surface has no matte, no discoloration, and no staining;
[0121] According to the above standard test, the product as a whole has no appearance wear and tear, light matting, whitening and discoloration on the surface, etc. The overall quality meets the appearance and surface discoloration, rough edges, and no whitening of the auxiliary material product industry standard. In terms of performance, it is resistant to water washing, dry cleaning, and ironing without matting and discoloration. In particular, when it is machine washed 10 times in a row at home, there is no light matting or color change. (The original untreated product will become matte and white after one machine wash and dry cleaning, and the whitening level is 3 to 3.5. After this technology is treated, the product surface will not change in color and light.)
[0122] See also Figure 4 , Figure 4 This is a photograph of the appearance of the semi-gloss black horn button treated in Example 2 of the present invention after machine washing or dry cleaning.
[0123] See also Figure 5 , Figure 5 The following are the appearance pictures of the semi-gloss horn button treated with spray paint in the existing process, after machine washing 3 times, and after dry cleaning 3 times. From left to right, they are the appearance pictures of the semi-gloss horn button treated with spray paint, after machine washing 3 times, and after dry cleaning 3 times.
[0124] Depend on Figure 4 and Figure 5 By comparison, it can be seen that the semi-gloss horn buttons treated with spray paint are much less natural in appearance than the horn buttons treated by the present invention, and cannot reflect the essential characteristics of natural materials.
[0125] Example 3
[0126] Horn button texture purification formula composition (%)
[0127] Citric acid: (industrial grade): 3%
[0128] Sodium dodecylbenzenesulfonate: 3%
[0129] Acetic acid: 2%
[0130] Water: 92%.
[0131] The semi-gloss coffee-colored horn button blank is shaped and then water-rolled and polished to a semi-gloss finish, and then faded to coffee color. After drying, it is treated again. The treatment liquid is prepared, and the pH value is controlled at 5. Then the button is placed in the treatment liquid for 3 minutes. After the protein and other substances on the surface of the horn material are reacted, the white dirt and oil on the overall surface, holes, and knife feet are removed. After the trial production, the overall color and gloss texture are purer.
[0132] 1. Machine washable: Machine washable ISO 6330-2012 4N; GB / T 8629-2017 4N Textile Household Washing and Drying Test Procedure Test Color Fastness 4.5, Appearance Evaluation Gloss without matte and surface whitening and discoloration;
[0133] 2. Dry cleaning resistance: ISO 3175-2:2010 Professional care of textiles and clothing, color fastness test after dry cleaning and wet cleaning, level 4.5, appearance evaluation gloss without matte and surface whitening and discoloration;
[0134] 3. Color fastness to hot pressing: GB / T 6152-1997 "Textiles - Tests for color fastness - Color fastness to hot pressing" The product surface has no matte, no discoloration, and no staining;
[0135] According to the above standard test, the product as a whole has no appearance wear and tear, light matting, whitening and discoloration on the surface, etc. The overall quality meets the appearance and surface discoloration, rough edges, and no whitening of the auxiliary material product industry standard. In terms of performance, it is resistant to water washing, dry cleaning, and ironing without matting and discoloration. In particular, when it is machine washed 10 times in a row at home, there is no light matting or color change. (The original untreated product will become matte and white after one machine wash and dry cleaning, and the whitening level is 3 to 3.5. After this technology is treated, the product surface will not change in color and light.)
[0136] See also Figure 6 , Figure 6 This is a photograph of the appearance of the semi-gloss coffee-colored horn buttons treated in Example 3 of the present invention after machine washing or dry cleaning.
[0137] The above is a detailed introduction to the application of the treatment liquid provided by the present invention in the preparation of horn buttons and a treatment method for purifying the texture of natural horn buttons. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enables any technician in the field to practice the present invention, including the manufacture and use of any device or system, and the implementation of any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements that are not different from the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.
Claims
1. Application of treatment liquid in the preparation of horn buttons; The treatment liquid, measured by weight, comprises: 3-6 parts by weight of citric acid; 2-5 parts by weight of sodium dodecylbenzenesulfonate; 1 to 2 parts by weight of acid; Water 90-92 parts by weight.
2. The use according to claim 1, characterized in that: The acid includes acetic acid; The horn buttons include natural horn buttons.
3. The use according to claim 1, characterized in that: The application specifically includes improving the surface texture of horn buttons and horns and / or purification.
4. The use according to claim 1, characterized in that: The method of preparing the horn buttons specifically comprises: after the horn buttons are dry-polished and / or dry-rolled, chemically treating the horn buttons with a treatment liquid; The application includes application in forming a stratum corneum on the horn surface of horn buttons.
5. The use according to claim 1, characterized in that: The applications include cleaning impurities and oil from horn buttons; The horn buttons are specifically ordinary horn buttons or laser-processed horn buttons.
6. A method for processing horn buttons, characterized in that: The following steps are involved: The semi-finished ox-horn button product after dry polishing and / or dry rolling is placed in a chemical treatment liquid for soaking to obtain an ox-horn button; The chemical treatment liquid comprises the treatment liquid in the application according to any one of claims 1 to 4.
7. The processing method according to claim 6, characterized in that: Before the dry rolling step, the ox horn button blanks are subjected to one or more steps of sorting, button making, water rolling polishing, cleaning and drying; The pH value of the chemical treatment solution is 3-5.
8. The processing method according to claim 6, characterized in that: Before the dry rolling step, the ox horn button blanks are sequentially subjected to the steps of sorting, button making, water rolling polishing, cleaning and drying; The chemical treatment liquid is specifically obtained by mixing treatment liquid components; The mixing time is 2 to 3 minutes.
9. The processing method according to claim 6, characterized in that: The soaking time is 2 to 8 minutes; The soaking step also includes a cleaning step; The processing method can be used to process finished horn buttons.
10. The processing method according to claim 6, characterized in that: The horn buttons include horn buttons with natural horn surfaces and horn buttons with natural horn surfaces and laser-treated surfaces; The laser marks on the surface of the horn button after laser treatment are yellow laser marks; After the yellow laser mark is treated again with a chemical treatment liquid, a laser mark with the same color as the surface matrix of the horn is obtained.