Manufacturing method of high-performance gear steel

Through alloy composition design and process control, the problem of insufficient performance of existing CrNiMo-based gear steel at low temperatures is solved, and the steel for CrNiMo-based gears with high hardenability and excellent low-temperature impact performance is achieved, meeting the high standard requirements of wind power output gears , and reduces production costs.

CN119020568APending Publication Date: 2024-11-26SHIGANG JINGCHENG EQUIP TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410997631.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing CrNiMo gear steels are difficult to meet the strict requirements of wind power output gears for high hardenability and excellent low-temperature impact performance at low temperatures, and have high production costs.

Method used

Through alloy composition design and production process control, chemical composition and process parameters are adjusted, such as carbon, silicon, manganese, chromium, nickel, etc., using converter smelting, LF refining, VD vacuum refining, continuous casting, heating, continuous rolling, and finishing, etc., such as carbon, silicon, manganese, chromium, and nickel. , molybdenum, aluminum and nitrogen content, control process parameters such as opening rolling temperature, finish rolling temperature, vacuum holding time and heating zone division to ensure high hardenability and low-temperature impact performance of steel.

Benefits of technology

The CrNiMo-based gear steel that achieves high hardenability and excellent low-temperature impact performance meets the high standard performance requirements of wind power output gears, reduces the amount of Cr and Ni, has cost advantages, and effectively prevents cracking in the quenching process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0004960686380000021
    Figure BDA0004960686380000021
  • Figure BDA0004960686380000051
    Figure BDA0004960686380000051
Patent Text Reader

Abstract

The invention provides a manufacturing method of high-performance gear steel, and belongs to the technical field of metallurgy. The manufacturing method comprises the working procedures of converter smelting, LF refining, VD vacuum refining, continuous casting, heating, continuous rolling, finishing and warehousing. The continuous rolling procedure comprises rough rolling and finish rolling; descaling, wherein the descaling pressure is larger than or equal to 300 bar; rough rolling: the initial rolling temperature is 1050-1150 DEG C; the large rolling reduction of a single pass is controlled to be 90-110 mm; finish rolling: the finish rolling temperature is 920-980 DEG C; through alloy component design and production process control, the CrNiMo series gear steel with high hardenability and excellent low-temperature impact performance is obtained, and the mechanical properties can reach that the yield strength is larger than or equal to 950 MPa, the tensile strength is larger than or equal to 1250 MPa, the ductility is larger than or equal to 13%, the percentage reduction of area is larger than or equal to 55%, the impact performance Akv at the normal temperature is larger than or equal to 60 J, and the impact performance Akv at the temperature of-40 DEG C is larger than or equal to 35 J.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a method for manufacturing high-performance gear steel. Background Art

[0002] Gear steel is a key material with large usage and high requirements in wind power materials; the performance requirements of gear steel not only affect the technical and economic indicators such as the life of wind power equipment, but also affect the requirements of safety in use. The working environment of wind power output gears is complex and harsh, and its materials are usually required to have good strength, toughness and wear resistance. In addition, it is also required to have good characteristics of bearing impact, bending and contact stress. Therefore, the material is required to have high hardenability, excellent impact and performance, especially low-temperature impact. The commonly used material is CrNiMo gear steel, but the conventional requirements for CrNiMo gear steel in the EN10084 standard are as follows: With the rapid development of the wind power industry, wind power output gears have more and more stringent requirements for their key material gear steel, and the production cost is also included in the gear steel development requirements. Therefore, it is necessary to provide a wind power output gear steel with high hardenability and excellent low-temperature impact performance to meet the material needs of the wind power gear industry.

[0003] 18CrNiMo7-6 is the grade of EN10084 surface hardened steel, which is the steel grade representation method of the European Committee for Standardization. Its digital number is 1.6587; 18CrNiMo7-6 hardened steel is widely used in wind power, mining reducer gears, locomotive gears, etc. due to its good processing performance, mechanical properties and high wear resistance. At present, the conventional performance requirements of the material circulating in the market are: tensile strength ≥1080MPa, yield strength ≥785MPa, elongation ≥10%, shrinkage ≥40%; room temperature impact Akv ≥40J; but with the rapid development of the gear industry, output gear steel with high hardenability and excellent low temperature impact performance is in urgent need of research and development. For example, an energy company has requirements for the performance of 18CrNiMo7-6 rolled materials: after low temperature quenching (830℃) + low temperature tempering (180℃), tensile strength ≥1200MPa, yield strength ≥905MPa, elongation ≥11%, shrinkage ≥35%; room temperature impact Akv ≥40J, -40℃ impact Akv ≥27J. This material can hardly meet this use requirement under low temperature quenching, and it is necessary to adjust the original composition and control temperature and rolling to achieve high hardenability and refined grains. Summary of the invention

[0004] The invention provides a method for manufacturing high-performance gear steel, and obtains CrNiMo series gear steel with high hardenability and excellent low-temperature impact performance through alloy composition design and production process control.

[0005] In order to solve the above technical problems, the technical scheme adopted by the present invention is as follows: a method for manufacturing high-performance gear steel, the manufacturing method comprising converter smelting, LF refining, VD vacuum refining, continuous casting, heating, continuous rolling, finishing, and warehousing processes; the continuous rolling process comprises rough rolling and finishing rolling; descaling: descaling pressure ≥300bar; rough rolling: starting rolling temperature 1050~1150℃, try to control it according to the lower limit; the maximum reduction of a single pass is controlled at 90~110mm; finishing rolling: the finishing rolling temperature is 920~980℃, try to control it according to the lower limit.

[0006] In the converter smelting process of the present invention, the steel tapping conditions are [C]≥0.06%, [P]≤0.012%, and the steel tapping temperature is 1600-1650°C.

[0007] In the LF refining process of the present invention, LF is in place and diffusion deoxidation is carried out with 2.0-5.0 kg / t of silicon carbide per ton of steel, the reducing atmosphere in the furnace is maintained, the white slag is maintained for ≥20 minutes, and the final slag basicity is ≥3.0; alloy is prohibited from being added 10 minutes before LF ladle hanging, aluminum is highly controlled before VD, aluminum is not added after VD as much as possible, and 1 / 2-2 / 3 of the slag is dumped before entering VD.

[0008] In the VD vacuum refining process of the present invention, the high vacuum holding time below VD 67Pa is ≥15 minutes; during the vacuum holding period, obvious leakage can be observed on the steel liquid surface to ensure the vacuum degassing effect; after the vacuum treatment is completed, the temperature is measured and sampled, and a covering agent is added at a rate of 1.0-1.5kg / t steel to evenly cover the entire slag surface; the soft blowing time is ≥15 minutes (to ensure that the molten steel is not exposed); the ladle temperature: 1597±5℃ for the open-casting furnace; 1567±5℃ for the continuous casting furnace.

[0009] The continuous casting process of the present invention has a continuous casting billet specification of 600mm≤Φ≤800mm, a pulling speed of 0.24±0.02m / min, a specific water content of 0.11±0.01L / kg, a crystallizer electric stirring current of 100±1A / frequency of 2.0±0.02HZ, and a final stirring current of 150±1.5A / frequency of 6.0±0.06HZ; a continuous casting billet specification of 450mm≤Φ<600mm, a pulling speed of 0.43±0.03m / min, and a specific water content of 0.18±0.01 L / kg, crystallizer electric stirring current 100±1A / frequency 2.0±0.02HZ, final stirring current 150±1.5A / frequency 8.0±0.08HZ; continuous casting billet specification 300mm≤Φ<450mm, pulling speed 0.85±0.05m / min, specific water content 0.22±0.01L / kg, crystallizer electric stirring current 100±1A / frequency 2.0±0.02HZ, final stirring current 150±1.5A / frequency 8.0±0.08HZ.

[0010] In the heating process of the present invention, the blank is heated: the preheating zone is ≤750°C, the heating temperature of zones 11-15 is 1200-1270°C, and the heating areas in the furnace are divided into a preheating zone, a heating zone (zones 1-9), and a uniform temperature zone (zones 11-15).

[0011] The specific control parameters of the heating process of the present invention are shown in the table below.

[0012]

[0013] The finishing process of the present invention is straightening, the curvature is ≤4mm / m, and the total curvature is ≤0.4% of the total length.

[0014] The chemical composition and mass percentage of the high-performance gear steel described in the present invention are: C: 0.16-0.19%, Si: 0.24-0.28%, Mn: 0.65-0.70%, P≤0.012%, S≤0.005%, Ni: 1.60-1.65%, Cr: 1.65-1.69%, Mo: 0.29-0.31%, Nb: 0.020-0.030%, Al: 0.030-0.035%, N: 0.0090-0.0120%, and the rest are Fe and unavoidable impurities.

[0015] The high-performance gear steel of the present invention has the specifications of round steel of φ80-300mm; the mechanical properties of the high-performance gear steel are as follows: yield strength ≥950MPa, tensile strength ≥1250MPa, elongation ≥13%, cross-sectional shrinkage ≥55%, impact performance Akv ≥60J at room temperature, and impact Akv ≥35J at -40℃.

[0016] The composition design principle of the present invention:

[0017] Part of the carbon enters the steel matrix to play a role in solid solution strengthening, and the other part of the carbon will combine with the carbide-forming elements in the alloy elements to form alloy carbides. Carbides, as hard and brittle phases, further play a strengthening role. Increasing the carbon content in the steel can increase the strength and hardness of the steel, but too much carbon will reduce its plasticity and toughness. Therefore, the present invention chooses to add a carbon content of 0.16-0.19%.

[0018] Silicon can improve the hardness of steel, but adding too much will reduce the plasticity and toughness of the steel. Silicon is also an element added to steel as a deoxidizer during steelmaking. Therefore, the present invention chooses to add 0.24-0.28% silicon.

[0019] Manganese can improve the strength and wear resistance of steel, weaken and eliminate the "hot brittleness" phenomenon of sulfur, and improve the hardenability of steel. Manganese also has a deoxidation effect in the steelmaking process. Too much manganese will increase the overheating sensitivity of steel, cause coarse grains, increase white spot sensitivity and temper brittleness. Therefore, the present invention chooses to add a manganese content of 0.65-0.70%.

[0020] Although phosphorus can increase the strength and hardness of steel, it significantly reduces the plasticity and toughness of steel, especially at low temperatures. It makes the steel significantly brittle and produces cold brittleness. Excessive phosphorus can also lead to structural segregation. Therefore, the present invention strictly controls the phosphorus content to ≤0.012%.

[0021] On one hand, sulfur forms a low melting point compound with iron, causing "hot brittleness" during hot working; on the other hand, it also reduces the cleanliness of steel, causing the risk of exceeding the inclusion standard. Therefore, the present invention strictly controls the sulfur content to ≤ 0.005%.

[0022] Part of chromium in steel dissolves in iron to form a solid solution, and part of chromium forms carbides and alloy carbides with carbon and other alloy elements. Chromium is a medium carbide-forming element. Chromium carbides can be finely and evenly distributed in the volume of steel to improve the strength, hardness, yield point and wear resistance of the steel. Since it can refine the structure and evenly distribute it, the plasticity and toughness are also good. Chromium can also improve the hardenability of steel and improve the corrosion resistance and antioxidant effect of steel. Therefore, the present invention chooses to add a chromium content of 1.65-1.69%.

[0023] Nickel can reduce the critical point and increase the stability of austenite in steel, so its quenching temperature can be reduced, hardenability is good, and the fatigue limit of steel is improved. It can prevent the growth of grains at high temperatures, maintain the fine grain structure of steel, improve the strength of steel, and reduce the ductile-brittle transition temperature. Therefore, the present invention chooses to add a nickel content of 1.60-1.65%.

[0024] Molybdenum plays a major role in solid solution strengthening and precipitation strengthening in steel, which can significantly improve the hardenability and thermal strength of steel, inhibit the segregation of impurity elements such as P and S at grain boundaries, reduce temper brittleness, and refine the grains of steel. Therefore, the present invention selects to add a molybdenum content of 0.29-0.31%.

[0025] Aluminum / nitrogen: Aluminum combines with nitrogen to form aluminum nitride, and low-temperature precipitation can refine the grains and inhibit the aging of low-carbon steel. It can also improve the toughness of steel at low temperatures, improve the oxidation resistance of steel, and improve the wear resistance and fatigue strength of steel. Therefore, the present invention selects to add an aluminum content of 0.030-0.035% and a nitrogen content of 0.009-0.012%, and the Al / N ratio needs to be controlled between 2-4.

[0026] Niobium as a microalloying element added to steel does not change the structure of iron, but combines with carbon, nitrogen and sulfur in the steel to change the microstructure of the steel, and can achieve dispersed distribution of precipitates by inducing precipitation and controlling the cooling rate, and adjust the toughness level of the steel in a wide range. Therefore, adding niobium can not only improve the strength of the steel, but also improve the toughness, high temperature oxidation resistance and corrosion resistance of the steel, and reduce the brittle transition temperature of the steel. Therefore, the present invention selects the addition of niobium content of 0.020-0.030%.

[0027] The beneficial effects of the above technical solution are as follows: 1. The present invention obtains CrNiMo gear steel with high hardenability and excellent low-temperature impact performance through alloy composition design and reasonable production process control. The tensile impact performance test according to gb / t228 and gb / t229 can meet the gear performance requirements in most harsh environments; at the same time, the present invention adds Nb to adjust the strength and toughness on the basis of the original material standard, reduces the addition of Cr and Ni, and has a greater cost advantage in the field of wind power output gear steel. 2. The present invention ensures that the hardenability of steel meets the low-temperature quenching performance requirements through reasonable composition design, and effectively prevents cracking during the quenching process; smelting adopts electric furnace smelting, LF and VD refining process, and solidification adopts continuous casting. By setting the optimal process parameters, each process is optimally matched to improve the inclusion content and low-multiple quality of the steel. Through the continuous rolling process, the uniformity and low-multiple quality of the steel are further improved, and the overall performance stability of the steel is improved. 3. The high-performance gear steel 18crnimo7-6 of the present invention has a specification range of φ80 to 300mm, and its performance is tested according to GB / T228 and GB / T229 standards. φ10mm tensile strength: tensile strength reaches more than 1250MPa, yield strength reaches more than 950MPa, elongation reaches more than 13%, and cross-sectional shrinkage reaches more than 55%; room temperature impact reaches more than 60J, -40℃ impact reaches more than 35J; it meets the standard requirements of most high-standard gear steels. DETAILED DESCRIPTION

[0028] The present invention will be further described in detail below with reference to specific embodiments.

[0029] Examples 1-6

[0030] A method for manufacturing high-performance gear steel, comprising converter smelting, LF refining, VD vacuum refining, continuous casting, heating, continuous rolling, finishing, and warehousing processes;

[0031] 1) Converter smelting process, tapping conditions [C] ≥ 0.06%, [P] ≤ 0.012%, tapping temperature 1600-1650° C. The converter process control parameters of Examples 1-6 are shown in Table 1.

[0032] Table 1 Control parameters of converter process in Examples 1-6

[0033] Example Steel tapping C% Steel tapping P% Steel tapping temperature ℃ Whether to slag 1 0.074 0.0113 1620 no 2 0.060 0.0120 1650 no 3 0.078 0.0105 1600 no 4 0.089 0.0117 1612 no 5 0.062 0.0112 1634 no 6 0.084 0.0115 1625 no

[0034] 2) LF refining process: When LF is in place, use 2.0-5.0kg / t of silicon carbide for diffusion deoxidation, maintain the reducing atmosphere in the furnace, keep the white slag for ≥20 minutes, and the final slag basicity ≥3.0; no alloy is allowed to be added 10 minutes before LF lifting, high aluminum is controlled before VD, and aluminum is not added after VD as much as possible, and 1 / 2-2 / 3 of the slag is dumped before entering VD.

[0035] 3) VD vacuum refining process, high vacuum holding time below VD 67Pa is ≥15 minutes; during the vacuum holding period, obvious leakage can be observed on the steel liquid surface to ensure the vacuum degassing effect; after the vacuum treatment is completed, temperature measurement and sampling are carried out, and a covering agent is added at 1.0-1.5kg / t steel to evenly cover the entire slag surface; soft blowing time is ≥15 minutes (to ensure that the molten steel is not exposed); ladle temperature: open pouring furnace 1597±5℃; continuous pouring furnace 1567±5℃; Example 1-6 LF refining, VD vacuum refining process control parameters are shown in Table 3.

[0036] Table 2 Control parameters of LF refining and VD vacuum refining process in Example 1-6

[0037]

[0038]

[0039] 4) Continuous casting process, continuous casting billet specifications 600mm≤Φ≤800mm, pulling speed 0.24±0.02m / min, specific water content 0.11±0.01L / kg, crystallizer electric stirring current 100±1A / frequency 2.0±0.02HZ, final stirring current 150±1.5A / frequency 6.0±0.06HZ; continuous casting billet specifications 450mm≤Φ<600mm, pulling speed 0.43±0.03m / min, specific water content 0.18±0.01L / kg, crystallizer electric stirring Current 100±1A / frequency 2.0±0.02HZ, final stirring current 150±1.5A / frequency 8.0±0.08HZ; continuous casting billet specification 300mm≤Φ<450mm, pulling speed 0.85±0.05m / min, specific water content 0.22±0.01L / kg, crystallizer electric stirring current 100±1A / frequency 2.0±0.02HZ, final stirring current 150±1.5A / frequency 8.0±0.08HZ; The continuous casting process control parameters of Examples 1-6 are shown in Table 3.

[0040] Table 3 Control parameters of continuous casting process of Examples 1-6

[0041]

[0042] 5) Heating process, billet heating: preheating zone ≤750°C, heating temperature of zones 11-15 1200-1270°C, specific control parameters are shown in the table below; heating process control parameters of Examples 1-6 are shown in Table 4.

[0043] Table 4 Control parameters of heating process in Examples 1-6

[0044]

[0045] 6) Continuous rolling process, including rough rolling and finishing rolling; descaling: descaling pressure ≥ 300bar; rough rolling: starting rolling temperature 1050-1150℃, try to control it under the lower limit; single pass maximum reduction is controlled at 90-110mm; finishing rolling: entering finishing rolling temperature 920-980℃, try to control it under the lower limit.

[0046] 7) Finishing process, straightening, curvature ≤ 4 mm / m, total curvature ≤ 0.4% of the total length; the control parameters of the continuous rolling process of Examples 1-6 are shown in Table 5, the chemical composition of the high-performance gear steel finished product is shown in Table 6, and the properties are shown in Table 7.

[0047] Table 5 Control parameters of continuous rolling finishing and finishing process of Examples 1-6

[0048]

[0049]

[0050] Table 6 Chemical composition and properties of finished product of high performance gear steel of Example 1-6 See Table 7

[0051] Example C Si Mn P S Ni Cr Mo Nb Al N 1 0.172 0.264 0.692 0.0094 0.0026 1.600 1.664 0.290 0.023 0.0300 0.0111 2 0.171 0.259 0.650 0.0096 0.0024 1.627 1.661 0.297 0.020 0.0281 0.0105 3 0.190 0.253 0.682 0.0098 0.0034 1.620 1.690 0.299 0.024 0.0298 0.0098 4 0.161 0.249 0.684 0.0096 0.0017 1.621 1.656 0.305 0.030 0.0321 0.0115 5 0.160 0.240 0.700 0.0099 0.0016 1.618 1.671 0.310 0.025 0.0322 0.0120 6 0.165 0.280 0.678 0.0084 0.0015 1.650 1.650 0.295 0.026 0.0350 0.0090

[0052] Table 7 Performance of finished high performance gear steel products of Examples 1-6

[0053]

[0054] The above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A method for manufacturing high-performance gear steel, characterized in that: The manufacturing method includes converter smelting, LF refining, VD vacuum refining, continuous casting, heating, continuous rolling, finishing, and warehousing processes; the continuous rolling process includes rough rolling and finishing rolling; descaling: the descaling pressure is ≥300 bar; Rough rolling: starting rolling temperature 1050~1150℃; single pass maximum reduction controlled 90~110mm; Finishing rolling: The finishing rolling temperature is 920~980℃.

2. The method for manufacturing high-performance gear steel according to claim 1, characterized in that: In the converter smelting process, the steel tapping conditions are [C] ≥ 0.06%, [P] ≤ 0.012%, and the steel tapping temperature is 1600-1650°C.

3. The method for manufacturing high-performance gear steel according to claim 1, characterized in that: In the LF refining process, LF is in place and diffusion deoxidation is carried out with 2.0-5.0 kg / t of silicon carbide per ton of steel, a reducing atmosphere is maintained in the furnace, the white slag retention time is ≥20 minutes, and the final slag basicity is ≥3.

0.

4. The method for manufacturing high-performance gear steel according to claim 1, characterized in that: In the VD vacuum refining process, the high vacuum holding time below VD 67Pa is ≥15 minutes; during the vacuum holding period, obvious leakage can be observed on the steel liquid surface to ensure the vacuum degassing effect; after the vacuum treatment is completed, the temperature is measured and sampled, and a covering agent is added at 1.0-1.5kg / t steel to evenly cover the entire slag surface; the soft blowing time is ≥15 minutes, and the ladle temperature: the continuous casting furnace is 1567±5℃.

5. A method for manufacturing high-performance gear steel according to any one of claims 1 to 4, characterized in that: The continuous casting process has a continuous casting billet specification of 600mm≤Φ≤800mm, a pulling speed of 0.24±0.02m / min, a specific water content of 0.11±0.01L / kg, a crystallizer electric stirring current of 100±1A / frequency of 2.0±0.02HZ, and a final stirring current of 150±1.5A / frequency of 6.0±0.06HZ; a continuous casting billet specification of 450mm≤Φ<600mm, a pulling speed of 0.43±0.03m / min, and a specific water content of 0.18±0.01L / kg, crystallizer electric stirring current 100±1A / frequency 2.0±0.02HZ, final stirring current 150±1.5A / frequency 8.0±0.08HZ; continuous casting billet specification 300mm≤Φ<450mm, pulling speed 0.85±0.05m / min, specific water content 0.22±0.01L / kg, crystallizer electric stirring current 100±1A / frequency 2.0±0.02HZ, final stirring current 150±1.5A / frequency 8.0±0.08HZ.

6. A method for manufacturing high-performance gear steel according to any one of claims 1 to 4, characterized in that: In the heating process, the blank is heated at: the preheating zone is ≤750°C, and the heating temperature of zones 11-15 is 1200-1270°C.

7. A method for manufacturing high-performance gear steel according to any one of claims 1 to 4, characterized in that: For the heating process, the specific control parameters are shown in the following table; 。 8. A method for manufacturing high-performance gear steel according to any one of claims 1 to 4, characterized in that: The finishing process is straightening, the curvature is ≤4mm / m, and the total curvature is ≤0.4% of the total length.

9. A method for manufacturing high-performance gear steel according to any one of claims 1 to 4, characterized in that: The chemical composition and mass percentage of the high-performance gear steel are: C: 0.16-0.19%, Si: 0.24-0.28%, Mn: 0.65-0.70%, P≤0.012%, S≤0.005%, Ni: 1.60-1.65%, Cr: 1.65-1.69%, Mo: 0.29-0.31%, Nb: 0.020-0.030%, Al: 0.030-0.035%, N: 0.0090-0.0120%, and the rest are Fe and unavoidable impurities.

10. A method for manufacturing high-performance gear steel according to any one of claims 1 to 4, characterized in that: The specification of the high-performance gear steel is round steel with a diameter of φ80 to 300 mm; the mechanical properties of the high-performance gear steel are as follows: yield strength ≥950 MPa, tensile strength ≥1250 MPa, elongation ≥13%, cross-sectional shrinkage ≥55%, impact performance Akv ≥60J at room temperature, and impact Akv ≥35J at -40°C.