High formability 485MPa grade cold stamping steel for automobile bridge housing and production method thereof

By optimizing chemical composition and process flow, the forming performance of steel for cold stamping automobile axle shells is improved, and the problems of insufficient extension and molding performance in the prior art are solved, and the high forming performance of 485MPa-level cold stamping automobile axle shells are achieved. Steel production.

CN118639118BActive Publication Date: 2024-11-29ANGANG STEEL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411124976.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-29
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The extension and forming performance of existing steel for cold stamping automobile axle shells is low, which cannot meet the high forming needs of the load-loaded vehicle drive axle shells.

Method used

Chemical components are C0.085%~0.183%, Si 0.25%~0.85%, Mn 1.45%~2.22%, Al 0.35%~0.55%, Nb 0.010%~0.130%, Ti 0.003%~0.045%, Cr 0.02% High-forming 485MPa grade cold stamping automobile axle shell with ~0.54%, W 0.035% ~0.250%, Cu 0.21% ~0.51%, Rare Earth Elements 0.010% ~0.018%, Ca 0.0011% ~0.0030%, Mg 0.0015% ~0.1150% Using steel, the structural structure and cooling mode of the steel plate are controlled through smelting, heating, rolling and cooling processes, and the yield strength, tensile strength and impact work of the steel plate are improved.

Benefits of technology

The high forming performance of steel plates is achieved, with yield strength ≥485MPa, tensile strength ≥615MPa, transverse elongation A50 ≥38%, -40℃ lateral impact work ≥208J, -40℃ longitudinal impact work ≥240J, and transverse cold bending 180°D=a is qualified, which significantly improves molding performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a high-formability 485MPa grade cold stamping automobile bridge housing steel and a production method thereof. The chemical components of the steel are as follows by weight percentage: C 0.085%-0.183%, Si 0.25%-0.85%, Mn 1.45%-2.22%, Al 0.35%-0.55%, Nb 0.010%-0.130%, Ti 0.003%-0.045%, Cr 0.02%-0.54%, W 0.035%-0.250%, Cu 0.21%-0.51%, rare earth elements 0.010%-0.018%, Ca 0.0011%-0.0030%, Mg 0.0015%~0.1150%, and limited to P≤0.016%, S≤0.008%, N≤0.003%, the balance is Fe and unavoidable impurities. Steel plate yield strength ≥485MPa, tensile strength ≥615MPa, transverse elongation A 50 ≥38%, ‑40℃ transverse impact energy ≥208J, ‑40℃ longitudinal impact energy ≥240J, and transverse cold bending 180°D=a is qualified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal materials, and in particular relates to a high-formability 485MPa grade cold stamping automobile bridge housing steel and a production method thereof. The steel plate of the invention is mainly suitable for manufacturing cold stamping automobile bridge housing steel. Background Art

[0002] The automobile axle housing is one of the main components of the automobile driving system. It supports the weight of the frame and the assemblies at the rear of the frame, and protects the components of the transmission system. In the manufacturing field of the axle housing industry, there are two completely different product manufacturing methods: stamping and welding axle housings and casting axle housings. With the development of axle housing manufacturing technology and the need to reduce automobile weight and energy, especially for the axle housing driven by a truck, 12~16mm thick hot-rolled steel plates have been used to make stamping and welding axle housings, replacing the casting axle housings with complex manufacturing processes, low production efficiency, heavy weight and high cost.

[0003] Chinese patent application No. 202210449751.6 discloses a 500MPa grade automobile bridge housing steel for hot stamping and a production method thereof, wherein the chemical composition is, by weight percentage, C0.160%~0.235%, Si 0.07%~0.55%, Mn 1.50%~1.75%, Al0.010%~0.063%, Nb0.010%~0.045%, Ti0.010%~0.046%, V0.022%~0.075%, Mo0.10%~0.15%, B0.0012%~0.0032%, rare earth elements La+Ce 0.020%~0.030%, Ca 0.0010%~0.0015%, and Ca 0.0010%~0.0015%. .0 0 4 0%, P≤ 0.0 1 0%, S≤0 .005%, N≤0 .003%, the remainder is Fe and impurities. The yield strength of the steel plate is ≥500MPa, the tensile strength is ≥600MPa, and the transverse elongation A50 is ≥36%. The automobile axle housing steel can be used to produce hot stamping parts, but cannot be used for cold stamping parts.

[0004] The Chinese patent application with application number 202010623646.0 discloses a 620MPa grade cold stamped steel plate for automobile axle housing and a preparation method thereof, wherein the chemical composition of the steel plate is prepared according to the following mass fractions: C≤0.10%, Si≤0.45%, Mn≤1.60%, P≤0.010%, S≤0.005%, V≤0.060%, Nb≤0.060%, Als≤0.035%, and the balance is Fe. The present invention improves the strength and comprehensive performance indicators of the axle housing manufacturing material, with a yield strength of ≥520MPa, a tensile strength of ≥620MPa, and an elongation of ≥23%. The steel plate has a high strength, but an elongation of only 23%. Its elongation and forming properties are both low, and the cold stamping effect is not ideal. Summary of the invention

[0005] The purpose of the present invention is to provide a high-formability 485MPa grade cold stamping automobile bridge housing steel and a production method thereof. In view of the development needs of the automotive steel field, the high-formability 485MPa grade cold stamping automobile bridge housing steel of the present invention has a yield strength of ≥485MPa, a tensile strength of ≥615MPa, and a transverse elongation A 50 ≥38%, -40℃ transverse impact energy ≥208J, -40℃ longitudinal impact energy ≥240J, and transverse cold bending 180°D=a is qualified.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] High formability 485MPa grade cold stamping steel for automobile bridge housing, the chemical composition of the steel is as follows by weight: C0.085%~0.183%, Si 0.25%~0.85%, Mn 1.45%~2.22%, Al 0.35%~0.55%, Nb 0.010%~0.130%, Ti 0.003%~0.045%, Cr 0.02%~0.54%, W 0.035%~0.250%, Cu 0.21%~0.51%, rare earth elements 0.010%~0.018%, Ca 0.0011%~0.0030%, Mg 0.0015%~0.1150%, and P is limited to ≤0.016%, S≤0.008%, N≤0.003%, and the balance is Fe and unavoidable impurities.

[0008] The structure of the steel is as follows: ferrite accounts for 30% to 70% by volume, martensite accounts for 15% to 55% by volume, retained austenite accounts for 4% to 13% by volume, and bainite accounts for 4% to 12% by volume.

[0009] Steel plate yield strength ≥485MPa, tensile strength ≥615MPa, transverse elongation A 50≥38%, -40℃ transverse impact energy ≥208J, -40℃ longitudinal impact energy ≥240J, and transverse cold bending 180°D=a qualified hot-rolled plate.

[0010] The thickness of the finished steel plate is 5 to 18 mm.

[0011] The main functions of the components of the high-formability 485MPa grade cold stamping steel for automobile axle housing in the present invention are:

[0012] C: Carbon ensures the strength of the steel plate through solid solution strengthening and is also used to expand the austenite zone. Free carbon can have a good stabilizing effect on austenite, thereby improving the formability of the steel plate. It is also the most economical element to improve the strength of the material. If the carbon content is too low, the mechanical properties of the steel plate in the present invention cannot be obtained. If the content is too high, the steel plate will become brittle, there is a risk of delayed fracture, and it is also unfavorable to the welding performance, plasticity and toughness of the steel plate. Therefore, the optimal range of carbon in the present invention is 0.085% to 0.183%.

[0013] Si: Silicon is a solid solution strengthening element, which can improve the strength of the steel plate by solid solution strengthening in ferrite. At the same time, it can also inhibit the decomposition of residual austenite and the precipitation of carbides, reduce inclusions in steel, and also improve the hardenability of the steel plate. However, if the silicon content is too low, it will not have a strengthening effect, and if the content is too high, it will affect the hot rolling surface quality, resulting in a large amount of iron oxide scale and welding performance. Therefore, the silicon content in the present invention is 0.25% to 0.85%.

[0014] Mn: Manganese can form substitutional solid solution in steel, play a strong solid solution strengthening role, and is also an austenite stabilizing element in steel, expanding the austenite zone, reducing the critical quenching speed of steel, and can also refine the grains, so that the yield strength and tensile strength increase linearly. The content of this element increases the strength of steel within a certain range while hardly reducing the plasticity and toughness of steel, and can also improve the hardenability of steel. However, if the manganese content is too low, the supercooled austenite is unstable, and the processing properties such as plasticity and toughness of the steel plate are reduced. If the manganese content is too high, the welding performance of the steel plate will deteriorate, and the production cost will increase. At the same time, the carbon equivalent of the steel will also increase, and the uniformity of the steel plate organization will deteriorate during the smelting and hot rolling process, which is easy to cause serious banded structure defects in the organization. Therefore, the manganese content is selected to be 1.45% to 2.22%.

[0015] P: Phosphorus can increase the formation temperature of the α phase and expand the temperature range of the α phase. However, excessive phosphorus content will deteriorate the workability of the steel plate and have an adverse effect on plasticity, toughness and fatigue properties. In order to obtain a higher elongation, the upper limit is set at 0.010%.

[0016] S: Sulfur forms sulfide inclusions such as MnS, which become the starting point of cracks and deteriorate the processing performance, seriously affecting the formability of the steel sheet. Therefore, the lower the content, the better, and its upper limit is set to 0.005%.

[0017] Al: Al is a commonly used deoxidizer in steel. It plays a role in deoxidation and nitrogen determination during the smelting process, and can effectively improve the anti-oxidation performance of the steel plate. It can also inhibit the decomposition of residual austenite and the precipitation of carbides. However, too much aluminum will lead to a large number of aluminum inclusions, increase production costs, and cause difficulties in continuous casting production. Adding a certain amount of Al to steel can form AlN precipitation, which plays a certain role in refining grains, thereby improving the toughness and plasticity of the steel plate. Therefore, in the present invention, the Al content is limited to 0.35% to 0.55%.

[0018] Nb: Niobium plays a major role in steel fine grain strengthening and precipitation strengthening. It can also expand the rolling process window, improve the uniformity of steel coil performance, and refine the structure to improve the cold forming performance of steel plates. At high temperatures, niobium exists in austenite in a solid solution state, which can inhibit the growth of austenite grains and static and dynamic recrystallization during thermal deformation, and increase the recrystallization termination temperature, which can increase the final rolling temperature; at the same time, the precipitation of niobium carbonitride can also delay recrystallization and prevent the growth of austenite grains. It has obvious fine grain strengthening and precipitation strengthening effects, can effectively reduce the grade of banded structure of steel plates, and improve impact performance. Therefore, the optimal range of Nb content in the present invention is between 0.010% and 0.130%.

[0019] Ti: Titanium can effectively delay the recrystallization of deformed austenite, prevent the growth of austenite grains, increase the recrystallization temperature of austenite, refine the grains, and improve the strength and toughness of steel. Moreover, Ti is a strong carbon and nitride forming element, which can combine with carbon and nitrogen to form stable and fine carbon and nitride, playing a significant role in grain refinement and precipitation strengthening. Therefore, the optimal range of Ti content in the present invention is between 0.003% and 0.045%.

[0020] Cr: It is a carbide-forming element that can delay pearlite transformation and improve the hardenability of steel, thus facilitating the formation of martensite structure, and refining the structure to achieve a strengthening effect. It can also stabilize the residual austenite. Too low chromium content will affect the hardenability of steel, while too high chromium content will increase production costs and also make the processing and formability of the material worse. The principle of selecting the chromium content is to promote the formation of martensite, so the chromium content of the present invention is selected between 0.02% and 0.54%.

[0021] W: Tungsten is the metal with the highest melting point. The WC formed has high hardness. Its role in steel is similar to that of molybdenum. It is better than molybdenum in enhancing wear resistance. Tungsten can also improve the hardenability of steel and effectively inhibit grain growth. When its content is less than 0.035%, the effect is slight. When it exceeds 0.25%, the brittleness increases. Therefore, the optimal range of W content in the present invention is between 0.035% and 0.250%.

[0022] Cu: Copper can also expand the austenite phase, improve the weather resistance of steel, improve the weldability of steel, and effectively improve the corrosion resistance of steel. However, when the Cu content is high, it causes hot brittleness and deteriorates the surface performance of the steel plate. In addition, at a certain Cu content, it is beneficial to the strength and hot workability of the steel plate, effectively reduces the hot rolling edge crack tendency of the steel plate, and significantly improves the surface quality of the steel plate. Cu also has the effect of reducing work hardening and improving the plasticity of the steel plate. Therefore, the copper content of the present invention is selected to be 0.21% to 0.51%.

[0023] Rare earth elements (La+Ce): Rare earth has strong deoxidation and desulfurization capabilities. The spherical sulfides or sulfur oxides formed replace the long strip manganese sulfide inclusions, which can improve the plasticity and anisotropy of the steel plate. Rare earth can improve the fatigue performance of the steel plate and improve the welding performance of the steel plate. Rare earth has a strong affinity with other impurity elements in steel, which can reduce the content of sulfur, oxygen, phosphorus, hydrogen and other elements in the steel and eliminate their harmful effects. Therefore, the present invention limits the rare earth (La+Ce) content to 0.010% to 0.018%.

[0024] Ca: Calcium can change the morphology of steel sulfide (MnS), prevent the formation of long strips of MnS inclusions, and improve the plasticity, toughness and fatigue properties of the steel plate. Therefore, the present invention controls the Ca content to 0.0011% to 0.0030%.

[0025] Mg: Magnesium is a good deoxidizer, desulfurizer and spheroidizer in steel. Magnesium can reduce the number of inclusions in steel, reduce their size, make their distribution uniform and improve their morphology. A trace amount of magnesium can improve the size and distribution of carbides in steel and promote the fine and uniform carbide particles. Therefore, the present invention controls the Mg content to 0.0015% to 0.1150%.

[0026] N: As for the N content in steel, the lower the N content, the better. However, too low a content will lead to production difficulties and increase costs. Therefore, in the present invention, the N content is ≤0.003%.

[0027] A method for preparing high-formability 485MPa grade cold stamping automobile bridge housing steel, comprising smelting, heating, rolling and cooling, specifically comprising:

[0028] 1) Smelting: RH+LF process is adopted, H and O contents are strictly controlled, H≤0.0002%, O≤0.0015%, calcium treatment is carried out in the refining process, electromagnetic stirring and light pressure reduction technology are used in the continuous casting process, and the billet pulling speed is ≤1.1m / min.

[0029] 2) Heating: Directly heat the continuous casting slab with a thickness of (160-240) mm and a width of (1450-2030) mm and heat it in a walking beam heating furnace. The heating temperature is 1300-1330°C and the holding time is 182-210 minutes. The furnace pressure is always controlled in a slightly positive pressure state in the dynamic state, and the positive pressure value is controlled at 3-15 Pa. Reduce oxidation and burning. Appropriate heating temperature and appropriate holding time can make the alloy elements in the slab completely dissolved, the slab composition is uniform, and play a role in controlling the original austenite grain size.

[0030] 3) Rolling and cooling: The rough rolling adopts the rolling process of 3+3 mode (R1 adopts 3 rolling passes, R2 adopts 3 rolling passes), a total of 6 rolling passes, the rough rolling outlet temperature is 1125~1180℃, the intermediate billet thickness is 44~65mm, and the width is 1450~2030mm. The intermediate billet is insulated with a heat preservation cover before entering the hot rolling and finishing mill to reduce the temperature drop of the intermediate billet on the delayed roller and the temperature difference between the head, tail and plate width directions. The finishing rolling is 7-stand continuous rolling, high-pressure water descaling before finishing rolling, the finishing rolling inlet temperature is not higher than 1125℃, the final rolling temperature is 740~855℃, and the laminar cooling + ultra-fast cooling cooling mode is adopted after final rolling. The laminar cooling rate is 10~15℃ / s. After cooling to 650~735℃, ultra-fast cooling is carried out, and the cooling rate is ≥153℃ / s. The steel plate is cooled to 305~425℃ and then coiled. The laminar cooling to 650-735℃ aims to make ferrite precipitate quickly, while suppressing grain growth, the ferrite content is guaranteed, so that the ferrite grains are refined. The ultra-fast cooling to 305-425℃ aims to make martensite precipitate quickly and in large quantities, while suppressing grain growth, the martensite content is guaranteed, so that the martensite grains are refined. The convexity control accuracy of the steel plate is ±40μm, the flatness is controlled within 18I, the thickness control accuracy is ±40μm, the finished product thickness is 5-18mm, and the thickness tolerance is controlled within ±0.1mm.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1) The addition of Cr can improve the strength and toughness of the steel plate, delay the pearlite transformation, and improve the hardenability of the steel, which is beneficial to the formation of martensite structure, refine the structure, strengthen it, and stabilize the retained austenite.

[0033] 2) The WC formed by W has high hardness, enhances wear resistance, improves the hardenability of steel, and effectively inhibits grain growth.

[0034] 3) Cu can improve the weather resistance and weldability of steel, and can also effectively improve the corrosion resistance of steel. At a certain Cu content, it is beneficial to the strength and hot workability of the steel plate, effectively reducing the tendency of hot rolling edge cracking of the steel plate, and significantly improving the surface quality of the steel plate. Cu also has the effect of reducing work hardening and improving the plasticity of the steel plate.

[0035] 4) Rare earth elements (La+Ce) have strong deoxidation and desulfurization capabilities. The spherical sulfides or sulfur oxides formed replace the long strip manganese sulfide inclusions, which can improve the plasticity and anisotropy of the steel plate. Rare earth can improve the fatigue performance of the steel plate and improve the welding performance of the steel plate.

[0036] 5) The addition of Ca can change the morphology of steel sulfides and improve the plasticity, toughness and fatigue properties of the steel plate.

[0037] 6) The addition of Mg can reduce the number of inclusions in steel, reduce their size, make their distribution uniform, and improve their morphology. A trace amount of magnesium can improve the size and distribution of carbides in steel and promote the fine and uniform carbide particles.

[0038] 7) After rolling, the cooling mode of laminar cooling + ultra-fast cooling is adopted to obtain the various phase structures at different cooling stages.

[0039] 8) The microstructure of the steel of the present invention is ferrite, martensite, retained austenite and bainite. Under the coupling effect of transformation induced plasticity (TRIP) effect and coordinated deformation of the mixed microstructure of martensite and bainite, the formability of the steel plate is significantly improved during the forming process.

[0040] 9) The present invention has excellent mechanical properties, yield strength ≥485MPa, tensile strength ≥615MPa, transverse elongation A 50 ≥38%, -40℃ transverse impact energy ≥208J, -40℃ longitudinal impact energy ≥240J, and transverse cold bending 180°D=a is qualified. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the specific implementation methods of the present invention are further described below in conjunction with embodiments. The following embodiments are used to specifically illustrate the contents of the present invention. These embodiments are only general descriptions of the contents of the present invention and do not limit the contents of the present invention.

[0042] The main process of the present invention is as follows:

[0043] The continuous casting slab with a thickness of (160-240) mm and a width of (1450-2030) mm is directly hot-transferred and hot-charged into a step-beam heating furnace for heating at a temperature of 1300-1330°C and a holding time of 182-210 min. The furnace pressure is always controlled in a slightly positive pressure state in the dynamic state, and the positive pressure value is controlled at 3-15 Pa to reduce oxidation and burning. The rough rolling adopts a 3+3 mode rolling process (R1 adopts 3 passes and R2 adopts 3 passes), with a total of 6 passes. The rough rolling outlet temperature is 1125-1180°C, the intermediate billet thickness is 44-65 mm, and the width is 1450-2030 mm. The intermediate billet is kept warm by a heat preservation cover before entering the hot rolling and finishing mill to reduce the temperature drop of the intermediate billet on the delayed roller and the temperature difference between the head and tail and the plate width direction. The finishing rolling is a 7-stand continuous rolling, and high-pressure water is used for descaling before finishing rolling. The finishing rolling inlet temperature is not higher than 1125°C The final rolling temperature is 740-855°C. After the final rolling, the cooling mode of laminar cooling + ultra-fast cooling is adopted. The laminar cooling rate is about 10-15°C / s. After cooling to 650-735°C, ultra-fast cooling is carried out. The cooling rate is ≥153°C / s. The steel plate is cooled to 305-425°C and then coiled. The convexity control accuracy of the steel plate is ±40μm, the flatness is controlled within 18I, the thickness control accuracy is ±40μm, the finished product thickness is 5-18mm, and the thickness tolerance is controlled within ±0.1mm.

[0044] The specific composition, hot rolling process system, steel plate properties and tissue volume percentage of the six embodiments of the present invention are shown in Tables 1-4.

[0045] Table 1 Chemical composition of the examples of the present invention (wt, %)

[0046] serial number C Si Mn P S Al Nb Ti Cr W Cu Rare earth (La+Ce) Ca Mg N Example 1 0.085 0.85 1.45 0.010 0.007 0.35 0.012 0.003 0.54 0.035 0.21 0.010 0.0011 0.0015 0.001 Example 2 0.098 0.78 1.65 0.015 0.008 0.38 0.035 0.018 0.43 0.053 0.33 0.013 0.0014 0.0562 0.003 Example 3 0.112 0.72 1.78 0.009 0.002 0.43 0.052 0.022 0.48 0.088 0.41 0.017 0.0016 0.0869 0.002 Example 4 0.156 0.66 1.97 0.003 0.002 0.48 0.078 0.034 0.33 0.153 0.45 0.015 0.0020 0.0923 0.001 Example 5 0.171 0.45 2.08 0.004 0.002 0.52 0.095 0.041 0.15 0.186 0.48 0.016 0.0026 0.109 0.003 Example 6 0.183 0.25 2.22 0.008 0.005 0.55 0.130 0.045 0.02 0.250 0.51 0.018 0.0030 0.115 0.001

[0047] Table 2 Hot rolling process system of the embodiment of the present invention

[0048] serial number Thickness and width specifications / mm Billet drawing speed / m / min Heating temperature / ℃ Insulation time / min Heating furnace pressure / Pa Rough rolling outlet temperature / ℃ Intermediate billet specifications / mm Finishing rolling inlet temperature / ℃ Final rolling temperature / ℃ Laminar cooling temperature / ℃ Laminar cooling rate ℃ / s Coiling temperature / ℃ Ultra-fast cooling rate ℃ / s Example 1 160×1451 1.1 1305 182 4 1126 44×1451 1123 855 735 10 425 153 Example 2 195×1523 1.0 1312 186 8 1138 50×1523 1085 846 716 11 406 156 Example 3 200×1545 1.1 1328 190 5 1147 52×1545 1105 823 682 12 388 162 Example 4 215×1668 1.1 1318 201 3 1156 54×1668 1118 808 673 13 369 165 Example 5 240×1989 1.0 1320 205 1 1170 46×1989 1098 792 665 14 328 171 Example 6 220×2030 1.0 1330 210 2 1179 60×2030 1119 740 650 15 305 174

[0049] Table 3 Mechanical properties parameters of the embodiments of the present invention

[0050] serial number Steel plate thickness / mm Thickness control accuracy / μm Convexity control accuracy / μm Straightness Yield strength / MPa Tensile strength / MPa <![CDATA[Elongation at break in the transverse direction (A 50 ) / %]]> Transverse impact value (-40℃) / J Longitudinal impact value (-40℃) / J Cold bending test 180° (horizontal) Example 1 5 +15 -5 17I 535 665 38.5 221 255 D=a qualified Example 2 8 -20 -8 15I 522 659 39.3 220 254 D=a qualified Example 3 10 -4 -4 18I 513 652 41.5 219 251 D=a qualified Example 4 15 -5 +3 18I 505 648 41.8 216 248 D=a qualified Example 5 14 +9 +6 18I 492 632 42.1 212 244 D=a qualified Example 6 18 +30 +7 17I 485 615 43.5 208 240 D=a qualified

[0051] Table 4 Tissue volume percentage in the embodiments of the present invention

[0052] serial number Ferrite Martensite Retained austenite bainite Example 1 69.1% 18.8% 7.5% 4.6% Example 2 59.8% 26.7% 6.8% 6.7% Example 3 70.0% 15.6% 7.5% 6.9% Example 4 34.8% 55.0% 4.9% 5.3% Example 5 36.0% 42.8% 10.1% 11.1% Example 6 47.7% 41.2% 7.0% 4.1%

[0053] In order to describe the present invention, the present invention is appropriately and fully illustrated by the examples in the above. The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made should be included in the protection scope of the present invention. The patent protection scope of the present invention should be defined by the claims.

Claims

1. High formability 485MPa grade cold stamping steel for automobile axle housing, characterized by: The chemical composition of the steel is calculated by weight percentage: C 0.085%~0.183%, Si 0.25%~0.85%, Mn 1.45%~2.22%, Al 0.35%~0.55%, Nb0.052%~0.130%, Ti 0.003%~0.045%, Cr 0.02%~0.54%, W 0.035%~0.250%, Cu 0.21%~0.51%, rare earth elements 0.010%~0.018%, Ca 0.0011%~0.0030%, Mg 0.0015%~0.1150%, and P is limited to ≤0.016%, S ≤0.008%, N ≤0.003%, and the balance is Fe and unavoidable impurities; A method for preparing high-formability 485MPa grade cold stamping automobile bridge housing steel includes smelting, heating, rolling and cooling, specifically including: 1) Heating: The continuous casting slab is hot-transferred and hot-charged into the heating furnace for heating at a temperature of 1300-1330°C and a holding time of 182-210 minutes; 2) Rolling and cooling: The rough rolling outlet temperature is 1125-1179°C, the finishing rolling inlet temperature is not higher than 1125°C, the final rolling temperature is 740-855°C, and the laminar cooling + ultra-fast cooling cooling mode is adopted after the final rolling. The laminar cooling rate is 10-15°C / s. After cooling to 650-735°C, ultra-fast cooling is carried out, and the cooling rate is ≥153°C / s. The steel plate is cooled to 305-425°C before coiling; The steel plate yield strength ≥485MPa, tensile strength ≥615MPa, transverse elongation A50 ≥38%, -40℃ transverse impact energy ≥208J, -40℃ longitudinal impact energy ≥240J, and transverse cold bending 180°D=a qualified hot-rolled plate; The thickness of the finished steel plate is 5 to 18 mm.

2. The high formability 485MPa grade cold stamped automobile axle housing steel according to claim 1, characterized in that: The structure of the steel is as follows: ferrite accounts for 30% to 70% by volume, martensite accounts for 15% to 55% by volume, retained austenite accounts for 4% to 13% by volume, and bainite accounts for 4% to 12% by volume.

3. A method for preparing a high-formability 485MPa grade cold stamped automobile bridge housing steel as claimed in claim 1 or 2, comprising smelting, heating, rolling and cooling, characterized in that: Specifically include: 1) Heating: The continuous casting slab is hot-transferred and hot-charged into the heating furnace for heating at a temperature of 1300-1330°C and a holding time of 182-210 minutes; 2) Rolling and cooling: The outlet temperature of rough rolling is 1125-1180°C, the inlet temperature of finishing rolling is not higher than 1125°C, the final rolling temperature is 740-855°C, and the cooling mode of laminar cooling + ultra-fast cooling is adopted after final rolling. The laminar cooling rate is 10-15°C / s. After cooling to 650-735°C, ultra-fast cooling is carried out, and the cooling rate is ≥153°C / s. The steel plate is cooled to 305-425°C and then coiled.

4. The method for preparing the high-formability 485MPa grade cold-stamped automobile axle housing steel according to claim 3, characterized in that: The continuous casting slab has a size of (160-240) mm thick×(1450-2030) mm wide.

5. The method for preparing high-formability 485MPa grade cold stamping automobile axle housing steel according to claim 3, characterized in that: The furnace pressure of the heating furnace is always controlled in a slightly positive pressure state in the dynamic state, and the positive pressure value is controlled in a range of 3 to 15 Pa.

6. The method for preparing high-formability 485MPa grade cold stamped automobile axle housing steel according to claim 3, characterized in that: The intermediate billet before finish rolling and after rough rolling has a thickness of 44-65 mm and a width of 1450-2030 mm.

7. The method for preparing high-formability 485MPa grade cold stamped automobile axle housing steel according to claim 3 or 6, characterized in that: The intermediate billet after rough rolling is kept warm by a heat preservation cover before entering the hot rolling and finishing mill, and is descaled by high-pressure water before finishing rolling.

8. The method for preparing high-formability 485MPa grade cold stamped automobile axle housing steel according to claim 3, characterized in that: The convexity control accuracy of the steel plate is ±40μm, the flatness is controlled within 18I, and the thickness control accuracy is ±40μm.

Citation Information

Patent Citations

  • Process for the production of thin trip-steel strips and thin strips obtained using such a process

    CA2314830A1

  • High-strength steel sheet and method for manufacturing same

    CN107075644A

  • One-steel multi-stage hot-rolled sheet steel based on carbon distribution technology and manufacturing method thereof

    CN109355573A

  • 590MPa reinforced plastic dual-phase steel and preparation method thereof

    CN115491596A

  • High tensile strength steel sheet excellent in processibility and process for manufacturing the same

    EP1512760A2