Reagent MJ563 for extracting indium from copper smoke dust leachate as well as preparation method and application of reagent MJ563
The indium reagent MJ563 was extracted through copper smoke leaching liquid, and anionic composite extractant prepared by pressurized reaction of N-methyldiethanolamine, urea, pine oil and EDTA under an oxygen atmosphere was solved. The safety of indium separation in the prior art was solved. Risk and high cost issues achieve efficient indium extraction and recycling, reducing production costs.
Patent Information
- Application Number
- CN202411084662.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art has safety risks and high production costs in the efficient separation and enrichment of indium from low-concentration solutions, especially in the discharge of hydrogen arsenide gas and high-concentration chloride ion wastewater during zinc powder replacement.
The indium reagent MJ563 is extracted with copper smoke leaching liquid. This reagent is prepared by pressurized reaction of N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) under an oxygen atmosphere to form an anionic composite extractant, which can Indium is stably extracted under high acidity conditions and mixed with sulfonated kerosene for the recovery of indium.
The efficient extraction and recovery of indium is achieved, and the indium extraction rate reaches 80-90%, while reducing zinc powder consumption and production costs, and reducing wastewater discharge of high concentrations of chloride ions.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and chemical industry, and particularly relates to a copper fume leaching liquid indium extraction reagent MJ563 and a preparation method and application thereof. Background Art
[0002] Indium is an important strategic resource and one of the supporting materials for the development of high technology. China's indium reserves rank first in the world. Although the reserves are not scarce, since indium has no independent deposits and mainly coexists with minerals such as lead, zinc, copper, and tin, according to the current technical level, the comprehensive recovery rate of indium is only 40% to 60%, and the recyclable indium is only a very small part of the reserves. Therefore, developing a method for efficiently separating and enriching indium from a solution containing low concentrations of indium is a difficult problem to be studied and solved.
[0003] The traditional method for treating indium is zinc powder replacement indium precipitation-indium-rich slag secondary leaching-extraction stripping process, which is to add zinc powder to a solution containing low-concentration indium sulfate to replace indium precipitation, obtain indium-rich slag with an indium mass fraction greater than 1%, and then use secondary leaching of the indium-rich slag, the indium concentration in the leaching solution is 2~5g / L, and then extract, strip, replace, and electrolyze to obtain metallic indium. This process is simpler than the first method, and the indium recovery rate is improved, but the zinc powder replacement process is prone to produce highly toxic arsenic gas, which poses a safety risk, and due to the high concentration of residual sulfuric acid in the solution, the zinc powder consumption is 100~150 times the theoretical consumption of indium replacement, the zinc powder consumption is large, and the production cost is high. And the zinc powder consumption is large, and the production cost is high. Similarly, in the indium extraction process, indium is stripped with high-concentration hydrochloric acid, resulting in a large amount of wastewater containing high-concentration chloride ions.
[0004] Therefore, it is very necessary to develop an indium extraction reagent and a recovery method that can solve the above-mentioned technical problems. Summary of the invention
[0005] The first purpose of the present invention is to provide a copper fume leaching solution extraction indium reagent MJ563; the second purpose is to provide a preparation method of the copper fume leaching solution extraction indium reagent MJ563; the third purpose is to provide an application of the copper fume leaching solution extraction indium reagent MJ563.
[0006] The first object of the present invention is achieved in that the copper fume leaching solution indium extraction reagent MJ563 is prepared using N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) as raw materials.
[0007] The second object of the present invention is achieved by subjecting N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) in a prescribed ratio to a pressure reaction under an oxygen atmosphere to prepare the product.
[0008] The specific operation is as follows: N-methyldiethanolamine (tertiary amine), urea, pine oil, ethylenediaminetetraacetic acid (EDTA) reacts for 1-4 hours at an oxygen pressure of 0.5-1.0 kPa and a temperature of 300-400°C, and the reaction is stopped to obtain a composite agent MJ563 for extracting indium; wherein the molar ratio of tertiary amine, urea, pine oil, and EDTA is 1-5:2-9:1-10:10-100. The extractant has stable extraction performance for indium under high acid and high temperature conditions.
[0009] The third object of the present invention is achieved by using the copper fume leaching solution indium extraction reagent MJ563 in the process of recovering indium from highly acidic wastewater.
[0010] The technical principle of the copper fume leaching solution extraction indium reagent MJ563 described in the present invention is: under the dispersing effect of pine oil, N-methyldiethanolamine, urea and ethylenediaminetetraacetic acid (EDTA) react and combine to form anionic valence bonds, that is, MJ563 anionic composite extractant, and In ions in the solution combine with the anions of MJ563 to form indium-methyl chelates, thereby realizing the separation of indium from copper, zinc, iron, arsenic and silicon in the solution. DETAILED DESCRIPTION
[0011] The present invention is further described below in conjunction with the embodiments, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.
[0012] The copper fume leaching solution indium extraction reagent MJ563 of the present invention is prepared by using N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) as raw materials.
[0013] The molar ratio of N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) is (1-5): (2-9): (1-10): (10-100).
[0014] The preparation method of the copper fume leaching solution indium extraction reagent MJ563 of the present invention is to prepare the reagent by subjecting N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) in a prescribed ratio to a pressure reaction under an oxygen atmosphere.
[0015] The oxygen pressure of the pressurized reaction is 0.5~1.0KPa.
[0016] The temperature of the pressurized reaction is 300-400°C.
[0017] The time of the pressurized reaction is 1 to 4 hours.
[0018] The application of the copper fume leaching solution indium extraction reagent MJ563 of the present invention is the application of the copper fume leaching solution indium extraction reagent MJ563 in the process of recovering indium from highly acidic wastewater.
[0019] The application of the copper fume leaching solution indium extraction reagent MJ563 in the process of recovering indium from highly acidic wastewater is to add sulfonated kerosene to the copper fume leaching solution indium extraction reagent MJ563, mix them evenly, and then extract the indium-containing fume leaching solution.
[0020] The volume ratio of the copper fume leaching solution to extract indium reagent MJ563 and sulfonated kerosene is (10-40): (60-90).
[0021] The present invention is further described below with specific implementation cases: Example 1 N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) in a molar ratio of 1:2:1:10 were pressurized and reacted at an oxygen pressure of 0.5-1.0 KPa and a temperature of 350-400°C for 1 h to obtain the copper fume leaching solution indium extraction reagent MJ563.
[0022] Example 2 N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) in a molar ratio of 5:9:10:100 were pressurized and reacted at an oxygen pressure of 0.5-1.0 KPa and a temperature of 300-330°C for 4 hours to obtain the copper fume leaching solution indium extraction reagent MJ563.
[0023] Example 3 N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) in a molar ratio of 3:6:5:60 were pressurized and reacted at an oxygen pressure of 0.5-1.0 KPa and a temperature of 320-350°C for 3 hours to obtain the copper fume leaching solution indium extraction reagent MJ563.
[0024] Example 4 N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) in a molar ratio of 2:7:5:80 were pressurized and reacted at an oxygen pressure of 0.5-1.0 KPa and a temperature of 360-380°C for 2 hours to obtain the copper fume leaching solution indium extraction reagent MJ563.
[0025] Example 5 N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) in a molar ratio of 4:6:8:40 were pressurized and reacted at an oxygen pressure of 0.5-1.0 KPa and a temperature of 350-370°C for 2.5 hours to obtain copper fume leaching solution indium extraction reagent MJ563.
[0026] Example 6 The copper fume leaching solution prepared in Example 3 was used to extract the indium reagent for testing, as follows: Accurately measure 10-40% volume fraction of MJ563 composite extractant + 60-90% sulfonated kerosene, mix them evenly, and extract the indium-containing smoke leaching solution containing 50-1000 mg / L of indium. The ratio of O / A is 1:3-10, the stirring speed is 50-200r / min, the reaction temperature is 20-40℃, and the reaction is stopped. The organic phase and the aqueous phase are separated, and the indium extraction rate reaches 80-90%.
[0027] Example 7 The copper fume leaching solution indium extraction reagent MJ563 prepared in Example 1, Example 2, Example 4, and Example 5 were tested respectively, and the method was the same as that in Example 6. The results all showed that the copper fume leaching solution indium extraction reagent MJ563 of the present invention had an extraction rate of 80-90% for molybdenum.
Claims
1. A copper dust leaching solution extraction indium reagent MJ563, characterized in that: The copper fume leaching solution indium extraction reagent MJ563 is prepared using N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) as raw materials.
2. The copper fume leaching solution extraction indium reagent MJ563 according to claim 1, characterized in that: The molar ratio of N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) is (1-5): (2-9): (1-10): (10-100).
3. A method for preparing the copper fume leaching solution indium extraction reagent MJ563 described in 1 or 2, characterized in that: The product is prepared by subjecting N-methyldiethanolamine, urea, pine oil and ethylenediaminetetraacetic acid (EDTA) in a formulated ratio to a pressure reaction under an oxygen atmosphere.
4. The preparation method according to claim 3, characterized in that: The oxygen pressure of the pressurized reaction is 0.5~1.0KPa.
5. The preparation method according to claim 3, characterized in that: The temperature of the pressurized reaction is 300-400°C.
6. The preparation method according to claim 3, characterized in that: The time of the pressurized reaction is 1 to 4 hours.
7. An application of the copper fume leaching solution extracting indium reagent MJ563 according to claim 1 or 2, characterized in that: The copper fume leaching solution is used to extract indium reagent MJ563 in a process for recovering indium from highly acidic wastewater.
8. The use according to claim 7, characterized in that: The application of the copper fume leaching solution indium extraction reagent MJ563 in the process of recovering indium from highly acidic wastewater is to add sulfonated kerosene to the copper fume leaching solution indium extraction reagent MJ563, mix them evenly, and then extract the indium-containing fume leaching solution.
9. The use according to claim 8, characterized in that: The volume ratio of the copper fume leaching solution to extract indium reagent MJ563 and sulfonated kerosene is (10-40): (60-90).