Al-Cu-Mg series aluminum alloy plate as well as preparation method and application thereof
Through the preparation method of Al-Cu-Mg aluminum alloy sheet, the problem of degradation of casting performance of skin materials in large-scale aircraft is solved, the high strength and corrosion resistance of the ingots are achieved, and the high quality of skins for aerospace is met. Require.
Patent Information
- Application Number
- CN202411108506.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-26
Abstract
Description
Technical Field
[0001] The invention belongs to the field of aircraft materials, and in particular relates to an Al-Cu-Mg series aluminum alloy plate and a preparation method and application thereof. Background Art
[0002] Skin (or skin panel) refers to a dimensional component that covers the skeleton structure of an aerospace vehicle (also referred to as "aircraft") and is fixed to the skeleton with adhesives or rivets to form the aerodynamic shape of the aircraft. The skin is equivalent to the "skin" of the aircraft. Its main function is to protect the internal structure of the aircraft, maintain the shape of the aircraft, and give it good aerodynamic characteristics. When flying, aircraft will face strong aerodynamic forces, complex environments and stresses. Therefore, there are very high requirements for the surface, strength, plasticity, corrosion resistance and process level of the skin material.
[0003] The skin material of early low-speed aircraft was cloth, but the current skin material mainly uses metal materials, among which aluminum alloy skin is the most widely used. Some hypersonic aircraft also use titanium alloy or stainless steel skin.
[0004] At present, Al-Cu-Mg aluminum alloys have good mechanical properties, high strength and good processing performance after heat treatment. They are less sensitive to repeated static loads and vibration loads, and have little tendency to stress corrosion. They can be processed into products such as plates, rods, tubes, wires, profiles and forgings. At the same time, they have certain heat resistance and low cost advantages. They are widely used in industrial fields such as aerospace and rail transportation, especially becoming the best choice for skins in aerospace vehicles.
[0005] As we all know, the thickness of the skin varies depending on the aircraft model and usage requirements. For military aircraft, the thickness of the skin is usually 0.8 to 2.5 mm; for civil aircraft, the thickness is usually 2 to 4 mm. For modern passenger aircraft with a semi-monocoque fuselage design, the thickest part of the skin is generally no more than 2 mm. In some special areas, such as the emergency door opening area, the thickness of the skin can reach 5 to 6 mm. Due to the thin thickness of the skin, the tolerance for defects is almost zero, and the consistency and stability of the product are extremely high.
[0006] In recent years, with the rapid development of the aerospace industry, the demand for large-scale aircraft has also increased rapidly. In order to meet the requirements of high-speed flight and complex space environment, the size of skin panels has gradually increased. As the size of skin panels increases, the specifications of alloy ingots have also increased significantly (for example, the width has increased from 1650mm to 2300mm), resulting in a significant deterioration in the casting performance of the ingots.
[0007] Therefore, in order to ensure that the skin has excellent performance on the basis of large specifications and thin thickness, it is necessary to design the preparation process of the aluminum alloy skin panel. Summary of the invention
[0008] In view of this, the object of the present invention is to provide an Al-Cu-Mg series aluminum alloy plate and a preparation method and application thereof. The Al-Cu-Mg series aluminum alloy plate has good casting performance, high strength, and excellent corrosion resistance and heat resistance.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a method for preparing an Al-Cu-Mg series aluminum alloy plate, comprising:
[0011] The alloy raw materials are sequentially subjected to batching, smelting, composition adjustment, melt purification, grain refinement, casting, soaking treatment, rolling and annealing to obtain Al-Cu-Mg series aluminum alloy plates;
[0012] Wherein, 3≤Cu / Mg<5 in the ingredients;
[0013] The casting speed in the casting is 37-46 mm / min;
[0014] The cooling rate during the soaking treatment is 80 to 200° C. / h.
[0015] Preferably, the ingredients are:
[0016] Si≤0.10wt%;
[0017] Fe≤0.25wt%;
[0018] Cu 3.5~5.0wt%;
[0019] Mn 0.3~0.9wt%;
[0020] Mg 1.0~2.0wt%;
[0021] Cr≤0.05wt%;
[0022] Zn≤0.10wt%;
[0023] Ti≤0.05wt%;
[0024] Be 0.0005~0.0015wt%;
[0025] Na≤0.0005wt%;
[0026] Li≤0.0010wt%;
[0027] Pb≤0.002wt%;
[0028] Bi≤0.001wt%;
[0029] Sn≤0.001wt%;
[0030] The balance is Al.
[0031] Preferably, the water flow rate of the casting is 40 to 90 m 3 / h / root; the temperature of the aluminum liquid in the flow plate is 685~710℃, and the water temperature is 22~26℃.
[0032] Preferably, the soaking treatment is as follows: heating to 510-540°C at a rate of 50-90°C / h, keeping the temperature at 495-503°C for 15-30h, and then cooling.
[0033] Preferably, the ingot obtained by the soaking treatment is subjected to milling, aluminum cladding and heating treatment before rolling.
[0034] Preferably, the temperature of the heating treatment is 350-440° C., and the insulation time is 4-12 hours.
[0035] Preferably, after the heating treatment, the following operations are performed:
[0036] The obtained ingot is sequentially subjected to hot rough rolling, hot finish rolling and cold rolling;
[0037] The thickness of the blank obtained by the hot rough rolling is 20-30 mm; the thickness of the blank obtained by the hot finish rolling is 5-12 mm; the thickness of the blank obtained by the cold rolling is 0.8-4 mm.
[0038] Preferably, the annealing temperature is 350-440° C., and the annealing time is 60-180 min.
[0039] Preferably, the annealing further includes cooling, and the cooling rate ranges from 10 to 28° C. / h.
[0040] Preferably, the annealing is replaced by solution quenching.
[0041] Preferably, the melt purification includes in-furnace powder spraying, in-furnace rotary degassing, online degassing and online filtration.
[0042] Preferably, the hydrogen content of the melt after the melt purification is within 0.10ml / 100g Al; the slag content of the melt is within 0.02mm 2 / kg or N20 is within 20K / kg.
[0043] In a second aspect, the present invention provides an Al-Cu-Mg aluminum alloy plate prepared according to the above-mentioned preparation method, wherein the thickness of the ingot used for the Al-Cu-Mg aluminum alloy plate is 450-550 mm, the width is 2150-2750 mm, and the length is 2500-7000 mm.
[0044] In a third aspect, the present invention provides a use of the above-mentioned Al-Cu-Mg series aluminum alloy sheet in the preparation of aerospace skins.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] The present invention provides a method for preparing an Al-Cu-Mg series aluminum alloy plate, wherein the alloy raw material is sequentially subjected to batching, smelting, component adjustment, melt purification, grain refinement, casting, soaking treatment, rolling and annealing (or solution quenching) to obtain the Al-Cu-Mg series aluminum alloy plate. The present invention controls the batching components in the alloy raw material: 3≤Cu / Mg<5, so that the obtained ingot has a higher yield strength, which is beneficial to its subsequent processing; at the same time, by controlling the casting speed in the casting process to 37-46mm / min, the cracking tendency of the ingot, the looseness of the ingot core and the degree of chemical component segregation can be effectively reduced, and the averageness of the ingot is improved; the cooling rate in the soaking treatment is controlled to 80-200℃ / h, while ensuring that the ingot has excellent processing performance, the ingot cracking can be prevented.
[0047] By using the preparation method provided by the present invention, aluminum alloy ingots with specifications of 450-550 mm × 2150-2750 mm can be prepared, which can meet the subsequent preparation of aerospace skins, and its excellent casting performance, high strength, excellent corrosion resistance and heat resistance can meet the high quality requirements of the skins. DETAILED DESCRIPTION
[0048] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] With the rapid development of the aerospace industry, the demand for large-scale aircraft has also increased rapidly. In order to meet the requirements of high-speed flight and complex space environment, the size of skin materials has also increased day by day to significantly reduce the number of rivets for fixing the skin. In order to meet the demand for super-large skin materials, while reducing costs and improving efficiency, the specifications of ingots have increased significantly. For hard aluminum alloy square ingots, the larger the ingot, the more severe the looseness of the ingot core, the worse the casting performance, and the crack tendency will increase sharply with the increase of the width-to-thickness ratio.
[0050] The aluminum alloy sheet for skin is converted from horizontal rolling to direct rolling, and the weight of a single coil can be greatly increased, thereby greatly improving the yield rate and shortening the production cycle. However, as the size of the ingot increases significantly, the width of the ingot needs to be increased from 1650mm to 2300mm. However, in general, the thickness of the square ingot of hard aluminum alloy does not exceed 500mm, the width does not exceed 2000mm, and the width-to-thickness ratio does not exceed 4. However, in order to meet the demand for super-large skin materials, the ingot specifications need to be greatly improved, and the width-to-thickness ratio can even be as high as 5, which greatly increases the difficulty of casting molding and organizational performance control. At present, there are problems such as poor casting molding of super-large specifications and unstable mechanical properties in production, which seriously restricts the rapid development of super-large skin materials, especially the application of super-large skin aluminum alloy materials.
[0051] Based on the above problems, the present invention provides a method for preparing an Al-Cu-Mg series aluminum alloy plate, which comprises:
[0052] The alloy raw materials are sequentially subjected to batching, smelting, component adjustment, melt purification, grain refinement, casting, heat treatment, rolling and annealing to obtain Al-Cu-Mg series aluminum alloy plates.
[0053] According to the present invention, firstly, the alloy raw materials need to be prepared. In the present invention, in order to meet the requirements of high purity, aluminum ingots with higher purity and other raw materials with better quality are used to ensure that other impurity elements such as Si, Fe, Zn, Pb, etc. are controlled at a lower level. The alloy raw materials preferably include: aluminum ingots, scraps, master alloys, pure metals, etc.
[0054] In the present invention, the aluminum ingot is preferably an original aluminum ingot with a grade of Al99.70 or above.
[0055] In the present invention, the waste material is preferably a primary waste material batch, which can be selected from 2A12 primary waste material batch and 2024 alloy primary waste material batch.
[0056] In the present invention, the master alloy may be selected from any one or more of AlCu master alloy, AlBe master alloy, AlMn master alloy or AlTi master alloy.
[0057] In the present invention, the pure metal may be selected from Cu plates and / or Mg ingots.
[0058] In the present invention, in order to ensure that the obtained Al-Cu-Mg series aluminum alloy sheet has excellent mechanical properties and processing properties, its chemical composition needs to be designed, as described in detail as follows:
[0059] (1) Reasonable matching of Cu, Mg, and Mn element contents
[0060] Cu and Mg are the main strengthening elements in Al-Cu-Mg alloys, and the main strengthening phases are Al2Cu(θ) phase and Al2CuMg(S) phase. The higher the Cu content, the more θ phase there is, and the higher the Mg content, the more S phase there is. It should be noted that the alloy containing 4-6wt% Cu and 1.0-2.0wt% Mg has the highest strength in the quenched and naturally aged state. When containing 0.6wt% Mn, the alloy with 3.5-6wt% Cu and 1.2-2.0wt% Mg has the best high temperature endurance strength. In Al-Cu alloys, the addition of Mg can reduce the solubility of Cu in aluminum. When Al-Cu alloys contain more than 4wt% Cu and 1.0wt% Mg at the same time, there are still undissolved θ and S phases in the quenched state, which leads to accelerated local corrosion; and when there is excess Cu and Mg in the alloy, the aging effect will be reduced because they fail to enter the solid solution during quenching.
[0061] In Al-Cu-Mg alloys, adding an appropriate amount of Mn can increase the recrystallization temperature of the alloy, which is beneficial to maintaining the unrecrystallized structure, refining the structure of the cold-deformed material, improving the mechanical properties of the alloy at room temperature, and significantly improving the thermal strength of the alloy.
[0062] Therefore, the present invention preferably controls Mg 1.0-2.0wt%, Cu 3.5-5.0wt%, 3≤Cu / Mg<5, and Mn 0.3-0.9wt%.
[0063] (2) Reasonable control of Si, Fe, Zn, and Be element contents
[0064] When Si exists in Al-Cu-Mg alloy, Mg preferentially forms Mg2Si phase with Si, and excess Mg will form S phase with higher strength; in addition, Si will also increase the tendency of casting cracks.
[0065] FeAl3 formed by Fe and Al and FeAl3 formed by other elements are insoluble coarse compounds, which not only reduce the plasticity of the ingot, but also increase the tendency of cracks during casting and deformation. However, an appropriate amount of Fe can improve the harmfulness of Si, so the Fe content should generally be controlled to be 1.1 to 1.5 times the mass of Si.
[0066] A small amount of Zn (0.1-0.3wt%) has no effect on the room temperature mechanical properties of the ingot, but it will significantly reduce the heat resistance of the alloy and increase the crack tendency during casting and welding. Therefore, Zn is a harmful element in hard alloys, so the Zn content should be controlled within a lower range as much as possible.
[0067] In addition, in order to reduce the oxidation of the ingot during the melting and heat treatment process, it is necessary to add an appropriate amount of Be element to improve the properties of the oxide film and improve the casting performance.
[0068] Therefore, the present invention controls Si≤0.20wt%, Fe≤0.30wt%, Zn≤0.10wt%, and Be0.0005-0.0015wt%.
[0069] (3) Strictly control the content of trace elements
[0070] In Al-Cu-Mg alloys, Na exists in a free state, which will severely damage the casting and hot deformation properties of the alloy, resulting in "sodium brittleness". At the same time, the presence of Li will significantly increase the oxidation rate of liquid aluminum, causing the purity of the melt to deteriorate.
[0071] In addition, Pb, Bi, and Sn are all low-melting-point elements, which will seriously affect the high-temperature performance of the ingot. Therefore, their content needs to be strictly controlled within a lower range.
[0072] Therefore, the present invention controls Na≤0.0005wt%, Li≤0.0010wt%, Pb≤0.002wt%, Bi≤0.001wt%, and Sn≤0.001wt%.
[0073] In summary, in the present invention, the ingredients preferably include:
[0074] Si≤0.10wt%;
[0075] Fe≤0.25wt%;
[0076] Cu 3.5~5.0wt%;
[0077] Mn 0.3~0.9wt%;
[0078] Mg 1.0~2.0wt%;
[0079] Cr≤0.05wt%;
[0080] Zn≤0.10wt%;
[0081] Ti≤0.05wt%;
[0082] Be 0.0005~0.0015wt%;
[0083] Na≤0.0005wt%;
[0084] Li≤0.0010wt%;
[0085] Pb≤0.002wt%;
[0086] Bi≤0.001wt%;
[0087] Sn≤0.001wt%;
[0088] The balance is Al.
[0089] The ingredients of the batching more preferably include:
[0090] Si≤0.08wt%;
[0091] Fe≤0.20wt%;
[0092] Cu 3.6~4.8wt%;
[0093] Mn 0.4~0.8wt%;
[0094] Mg 1.2~1.8wt%;
[0095] Cr≤0.04wt%;
[0096] Zn≤0.08wt%;
[0097] Ti≤0.04wt%;
[0098] Be 0.0005~0.0012wt%;
[0099] Na≤0.0003wt%;
[0100] Li≤0.0008wt%;
[0101] Pb≤0.001wt%;
[0102] Bi≤0.0008wt%;
[0103] Sn≤0.0008wt%;
[0104] The balance is Al.
[0105] In the present invention, the melting temperature in the furnace during the smelting process is preferably 730-760°C, more preferably 735-750°C; during the smelting process, it is preferred that sampling and analysis be performed after the alloy raw materials are melted, and the composition of the melt is adjusted according to the requirements of the ingredient composition to ensure that each element is within the control range.
[0106] In the present invention, the composition adjustment preferably includes:
[0107] The actual analysis results of the chemical composition before the furnace are compared with the range values of each element in the ingredients of the pre-obtained alloy. If the element content is lower than the lower limit of the range value, a certain amount of pure metal of the element or an intermediate alloy containing the element is added until the element reaches the range. If the element content exceeds the upper limit of the range value, aluminum ingots are added to the furnace to reduce the excessive elements to within the range.
[0108] In practical applications, the thickness of aluminum sheets used for skinning is generally 0.8 to 4 mm, and the consistency of the aluminum sheets is extremely high, and the tolerance for defects is almost zero, so a high-purity and high-stability melt is required. Therefore, after the composition adjustment is completed, the present invention needs to purify the melt. In the present invention, the melt purification is preferably carried out in furnace powder spray refining, furnace rotary degassing refining, online degassing and online filtration in sequence.
[0109] In the present invention, the powder spray refining in the furnace preferably uses high-purity argon to blow the granular refining agent into the melt or an equivalent refining process. The purity of the high-purity argon should be no less than 99.999%; the granular refining agent includes 52-62wt% KCl, 37-47wt% MgCl2, NaCl≤1wt%, H2O≤1wt%, CaCl≤0.50wt%, MgO≤0.50wt%, and the remainder is impurities; the time of the powder spray refining in the furnace is 15-50min, preferably 20-30min.
[0110] In the present invention, the rotary degassing refining in the furnace is carried out in a heat preservation furnace, and the melt is refined by a high-purity argon-chlorine mixed gas through a high-speed rotating rotor in the furnace. The volume ratio of argon and chlorine is 95-99% and 1-5%; the purity of argon and chlorine should not be less than 99.999%, the temperature of the melt during refining is 720-750°C, preferably 730-740°C; the refining time is 10-60min, preferably 30-50min. In the present invention, after the rotary degassing refining in the furnace is completed, the liquid hydrogen content in the obtained melt is preferably ≤0.20mL / 100g Al.
[0111] In the present invention, the online degassing is preferably performed using high-purity argon or high-purity argon-chlorine mixed gas. Among them, in the high-purity argon-chlorine mixed gas, the volumes of argon and chlorine are 95-99% and 1-5%, respectively; the purity of argon and chlorine should not be less than 99.999%. In some embodiments of the present invention, the online degassing is preferably performed in series with a dual-rotor online degassing device. After the online degassing is completed, the liquid hydrogen content in the obtained melt is preferably within 0.10mL / 100g Al, preferably within 0.08mL / 100g Al; the slag content in the melt is controlled at 0.02mm 2 / kg or less, preferably 0.015mm 2 / kg; or N20 is within 20K / kg, preferably within 18K / kg.
[0112] In the present invention, the online filtration adopts plate filtration or deep bed filtration. In some embodiments of the present invention, a ceramic filter plate is used for melt filtration, and the filtration accuracy of the ceramic filter plate is preferably ≥50ppi.
[0113] According to the present invention, after the melt purification is completed, grain refinement is performed. In the present invention, aluminum titanium boron wire is preferably used to refine the as-cast structure, which can obtain a uniform and fine structure and improve the casting performance. In some embodiments of the present invention, Al-5Ti-1B wire is preferably used for grain refinement, and its amount is 1.2-2.0 kg / t, preferably 1.3-1.8 kg / t, and more preferably 1.4-1.6 kg / t.
[0114] Then, according to the present invention, casting is performed.
[0115] During the casting process, as the cooling rate increases, the density of the ingot increases, and the brittle compound phases distributed inside the grains and on the grain boundaries become finer, so the performance improves dramatically; but at the same time, as the cooling rate increases, the temperature gradient in the ingot becomes larger, and the stress caused by asynchronous solidification increases dramatically. At the same time, the crystallization range of Al-Cu-Mg alloys is 502-638°C, which makes the asynchronous shrinkage phenomenon more serious, and the alloy is very prone to side cracks and subcutaneous cracks.
[0116] In addition, with the increase of casting speed, the tendency of side cracks in the ingot decreases, the average crystallization rate increases, the intracrystalline structure becomes refined, and the average performance of the material is improved; however, as the casting speed increases, the porosity of the core of the ingot and the degree of chemical composition segregation also increase.
[0117] Furthermore, increasing the casting temperature during the casting process can reduce the size of the suspended crystal zone in the liquid cavity of the ingot, improve the exhaust and shrinkage compensation conditions, reduce the tendency to form primary crystal compounds, and increase the density of the ingot, thereby improving the cast mechanical properties; however, if the casting temperature is too high, it will cause grain coarsening and increase the hot brittleness of the alloy.
[0118] In summary, considering that the width and width-to-thickness ratio of the ingot for the super-large skin plate are both in an extraordinary situation, the present invention has screened and preferably controls the casting speed to be 37-46 mm / min, preferably 40-43 mm / min; the water flow rate is 40-90 m 3 / h. root, preferably 55-80m 3 / h. root; the temperature of the aluminum liquid in the flow plate is 685-710°C, preferably 695-700°C; the water temperature is 22-26°C, preferably 23-25°C.
[0119] In the present invention, the uneven cooling and solidification during the casting process results in a large stress in the obtained ingot. During the storage process before being loaded into the soaking furnace, the ingot may crack due to the difference in stress and the uneven release. In severe cases, the ingot may explode, and this tendency increases with the increase in the size of the ingot. Therefore, in order to eliminate the ingot stress and reduce the segregation of the ingot, it is necessary to perform a high-temperature homogenization annealing treatment (i.e., soaking treatment) on the ingot, so that the strengthening phase can be evenly filled and dissolved.
[0120] The conventional cooling method for hard aluminum alloy after soaking treatment is natural cooling, with an average cooling rate of less than 20℃ / h. However, the cooling rate is slow, which can easily cause more second phases (i.e., Al2Cu(θ) phase and Al2CuMg(S) phase) to precipitate during the cooling process. At the same time, the second phases will have the risk of aggregation, which will prevent them from being fully crushed and dissolved in the subsequent processing, resulting in reduced mechanical properties and corrosion properties of the plate. In addition, due to the large size of the ingot, cracking may occur if the cooling rate is too fast. Therefore, in order to obtain finely dispersed compounds, higher performance and uniform structure, the cooling rate after soaking treatment should be reasonably controlled.
[0121] In the present invention, the ingot should be kept for no more than 6 hours before soaking treatment. The soaking treatment is first heated to 510-540°C at a rate of 50-90°C / h for 8-12 hours, preferably at a rate of 60-80°C / h to 515-530°C for 9-10 hours. Then, keep warm at 495-503°C for 15-30 hours, preferably at 498-500°C for 20-25 hours. After the soaking is completed, it is preferably cooled at a cooling rate of 80-200°C / h for 2-6 hours, and more preferably cooled at a cooling rate of 100-150°C / h for 3-5 hours.
[0122] Since the corrosion resistance of Al-Cu-Mg alloys is low, and the Cu content in the alloy is higher than 4wt% and the Mg content is higher than 1wt%, there are still undissolved θ and S phases in the quenched state. In order to improve the corrosion resistance of the skin, the ingot is generally clad with aluminum after milling. Since the thickness of the skin plate is generally 0.8 to 4mm, most of which are within 2mm, any contamination during the production process will cause quality problems in the skin. Therefore, the entire process of ingot milling, aluminum cladding and ingot heating needs to maintain a very high degree of cleanliness.
[0123] In summary, the present invention provides comprehensive protection during the ingot milling and aluminum cladding processes, and the ingot heating furnace is kept cleaned regularly. In the present invention, the heating temperature of the ingot is 350-440°C, preferably 380-400°C; the holding time is 4-12h, preferably 8-10h. In the present invention, the ingot is heated and then rolled, and the rolling preferably includes hot rough rolling, hot finish rolling and cold rolling in sequence. The thickness of the billet obtained by the hot rough rolling is 20-30mm, preferably 22-25mm; the thickness of the billet obtained by the hot finish rolling is 5-12mm billet, preferably 6-10mm; the thickness of the billet obtained by the cold rolling is 0.8-4mm, preferably 1-2mm. After the rolling is completed, the plate is preferably cleaned to ensure that the emulsion on the plate is cleaned.
[0124] Since hard aluminum alloy will be strongly strengthened in the natural aging state, the plate state is generally O state or T3 / T4 state. In the present invention, the plate state is O state, so the plate needs to be annealed after rolling.
[0125] O-state products generally use coil annealing. After the metal is deformed by cold working, it is in an unstable state due to the increase in free energy. Annealing is used in production to eliminate the work hardening caused by the deformation and improve the plasticity of the product, thereby improving the processing performance of the plate. At the same time, in order to prevent the quenching effect after annealing and to maximize the precipitation of Cu and Mg from the solid solution, the cooling rate cannot be too fast. Therefore, in order to meet the requirements of the plate with higher mechanical properties and combined with production practice, the annealing temperature is 350-440°C, preferably 380-400°C; the annealing time is 60-180min, preferably 80-150min. After the annealing is completed, the cooling method preferably adopts a cooling rate of no more than 28°C / h, preferably 10-28°C / h, and air-cools with the furnace to below 260°C before air-cooling. It is more preferred to adopt a cooling rate of 15-25°C / h and air-cools with the furnace to below 260°C before air-cooling.
[0126] It should be noted that when the plate is in T3 / T4 state, it is necessary to carry out solution quenching after rolling. Generally, the strengthening effect mainly depends on the solution temperature, holding time, transfer time and quenching temperature. Among them, the higher the solution temperature, the longer the holding time, the higher the degree of solid solution, and the temperature has a much greater influence on the solid solution effect than time. The closer to the lowest eutectic temperature, the better the effect. At the same time, in order to consider industrial production and cost control, the quenching temperature is generally 3 to 5 ° C lower than the eutectic temperature; the lower the transfer time and quenching water temperature, the better the solid solution effect. The general methods of thin plate quenching are salt bath furnaces and air furnaces. Although salt bath furnaces have the advantages of fast heating speed, small temperature difference and accurate temperature, they are difficult to control manually due to the difficulty of manual control of transfer time and have greater safety and environmental risks. They have been gradually eliminated; although air furnaces are highly efficient and have no safety and environmental risks, they have the disadvantages of poor uniformity and accurate temperature control compared to salt bath furnaces. Therefore, the present invention adopts an air cushion furnace to carry out solution quenching, which not only prevents the surfaces of the thin plates from contacting each other, heats up quickly, and controls the deformation of the plate shape well, but also has the advantages of small temperature difference and accurate temperature, and no safety and environmental risks. The eutectic temperature of Al-Cu-Mg alloy sheets for skin is generally 507-510°C. In order to meet higher mechanical properties and combine with production practice, the solution process of the present invention is: heating temperature 495-505°C, preferably 498-500°C; keeping warm at this temperature for 5-15 minutes, preferably 8-10 minutes; then quenching in water at 10-30°C, preferably 15-20°C; quenching transfer time is generally 5-20s, preferably 10-15s.
[0127] The present invention also provides an Al-Cu-Mg aluminum alloy plate prepared according to the above preparation method, wherein the thickness of the ingot for the Al-Cu-Mg aluminum alloy plate is 450-550 mm, preferably 480-500 mm; the width is 2150-2750 mm, preferably 2250-2550 mm; the length is 2500-7000 mm, preferably 3000-5000 mm.
[0128] The aluminum alloy sheet obtained by the present invention has excellent mechanical properties, good casting properties, and excellent corrosion resistance and heat resistance. Based on this, the present invention also provides an application of the above-mentioned Al-Cu-Mg series aluminum alloy sheet in the preparation of aerospace skins.
[0129] In order to further illustrate the present invention, the following examples are provided for detailed description. The experimental raw materials used in the following examples of the present invention are all common commercially available products.
[0130] Example 1
[0131] The aluminum alloy is prepared according to the following method: ingot selection, raw material selection, smelting, composition adjustment, melt purification, grain refinement, casting, soaking, rolling and annealing are performed in sequence;
[0132] Ingot selection: Plate thickness 2.0mm; Ingot specification 450×2250mm;
[0133] Raw material selection: Al99.70 grade original aluminum ingot, Al99.95 grade or above copper plate, Al99.9 grade or above magnesium ingot, AlCu, AlBe, AlMn, AlTi master alloy, grain refiner (aluminum titanium boron wire), 2A12 first-level scrap ingredients;
[0134] Melting process: After the alloy raw materials are melted, samples are taken for analysis; the melting temperature in the furnace is 740°C, and the melt composition is adjusted to meet the requirements of element matching;
[0135] The composition is adjusted to meet the following requirements:
[0136] Si≤0.10wt%;Fe≤0.25wt%;Cu3.5~5.0wt%;Mn 0.3~0.9wt%;Mg1.0~2.0wt%;Cr≤0.05wt%;Zn≤0.10wt%;Ti≤0.05wt%;Be 0.0005~0.0015wt%;Na≤0.0005wt%;Li≤0.0010wt%;Pb≤0.002wt%;Bi≤0.001wt%;Sn≤0.001wt%;The balance is Al;
[0137] Powder spraying in the furnace: After the composition is adjusted, high-purity argon is used in the furnace to blow granular refining agent (57wt% KCl, 42wt% MgCl2, 0.18wt% NaCl, 0.12wt% CaCl, 0.23wt% MgO, 0.30wt% H2O, the remainder is impurities) into the melt. The purity of argon should not be less than 99.999%, and the refining time is 20min;
[0138] Rotary degassing in the furnace: After the powder spraying refining in the furnace, the qualified melt is transferred to the holding furnace. The melt is refined by high-purity argon-chlorine mixed gas through the high-speed rotating rotor in the furnace. The purity of argon and chlorine should be not less than 99.999%. The melt temperature during refining is 745℃ and the refining time is 30min. The hydrogen content of the melt after refining is 0.25mL / 100g Al.
[0139] Online degassing: After rotary degassing and refining in the furnace, high-purity argon-chlorine mixed gas of not less than 99.999% is used for online degassing. The hydrogen content after melt purification treatment by double-rotor online degassing device in series is 0.08mL / 100g Al.
[0140] Online filtration: After online degassing, 30+50ppi ceramic filter plates are used for melt filtration;
[0141] Grain refinement: Add aluminum titanium boron wire online to refine the as-cast structure, with a dosage of 1.4kg / t;
[0142] Casting parameters: casting speed 40mm / min, water flow 55m 3 / h. root, the temperature of aluminum liquid in the flow plate is 695℃, and the water temperature is 25℃; the ingot forming effect is better;
[0143] Heat treatment process: The cast aluminum alloy is subjected to heat treatment, and the heating rate of the ingot homogenization annealing is 50℃ / h, the heating time is 10h, the holding temperature is 495℃, the holding time is 15h, the cooling rate is 80℃ / h, and the cooling time is 5.5h;
[0144] Ingot rolling: After the ingot is milled and coated with aluminum, it is heated to 400℃ and kept at this temperature for 8 hours. After the ingot is heated, it is roughly hot rolled into a 30mm thick billet, and then hot finished rolled to a 10mm billet, which is first pre-annealed and then cold rolled to 2.0mm. After rolling, the plate is cleaned to ensure that the emulsion on the plate is cleaned;
[0145] Annealing treatment: the plate is pre-annealed before cold rolling, the annealing temperature is 380℃, the annealing time is 80min, the cooling method is 20℃ / h cooling rate, and the furnace is air-cooled to below 260℃ before being air-cooled out of the furnace.
[0146] After the above processes, the cold-rolled plates are sheared and tested for performance before being packaged and delivered.
[0147] Quality Inspection:
[0148] (1) Macroscopic examination of ingot: Grain size grade 1; the test method is GB / T3246.2 "Test methods for microstructure of deformed aluminum and aluminum alloy products - Part 2 Macroscopic examination methods";
[0149] (2) Chemical composition: Si 0.08wt%, Fe 0.18wt%, Cu 4.56wt%, Mg 1.45wt%, Cu / Mg=3.14, Mn 0.62wt%, Cr 0.01wt%, Zn 0.07wt%, Ti 0.02wt%, Be 0.0008wt%, Na 0.0003wt%, Li 0.0004wt%, Pb 0.0015wt%, Bi 0.0005wt%, Sn 0.0005wt%; the detection method is GB / T 20975 "Analysis method of aluminum alloy" and GB / T 7999 "Photoelectric direct reading emission spectrometry analysis method of aluminum and aluminum alloy";
[0150] (3) Hydrogen content: 0.08 mL / 100 g Al; the detection method is YS / T600 "Closed-circuit method for measuring hydrogen in liquid state of aluminum and aluminum alloys";
[0151] (4) Mechanical properties: O state performance, tensile strength 163MPa, elongation 23%; T42 state performance, tensile strength 431MPa, yield strength 266MPa, elongation 22%. The test method is GB / T16865 "Test specimens and methods for tensile test of deformed aluminum, magnesium and their alloy products".
[0152] Example 2
[0153] The aluminum alloy is prepared according to the following method: ingot selection, raw material selection, smelting, composition adjustment, melt purification, grain refinement, casting, soaking, rolling and annealing are performed in sequence;
[0154] Ingot selection: Plate thickness 0.8mm; Ingot specification 450×2250mm;
[0155] Raw material selection: Al99.70 grade aluminum ingot, Al99.95 grade copper plate, Al99.9 grade magnesium ingot, AlCu, AlBe, AlMn, AlTi master alloy, grain refiner (aluminum titanium boron wire), 2024 alloy first-level scrap ingredients;
[0156] Melting process: After the alloy raw materials are melted, samples are taken for analysis; the melting temperature in the furnace is 750°C, and the melt composition is adjusted to the control range according to the element matching requirements (refer to Example 1);
[0157] Powder spraying in the furnace: After the composition is adjusted, high-purity argon is used in the furnace to blow granular refining agent (57wt% KCl, 42wt% MgCl2, 0.18wt% NaCl, 0.12wt% CaCl, 0.23wt% MgO, 0.30wt% H2O, the remainder is impurities) into the melt. The purity of argon should not be less than 99.995%, and the refining time is 20min;
[0158] Rotary degassing in the furnace: After the powder spraying refining in the furnace, the qualified melt is transferred to the holding furnace. The melt is refined by high-purity argon-chlorine mixed gas through the high-speed rotating rotor in the furnace. The purity of argon and chlorine should be not less than 99.999%. The melt temperature during refining is 740℃ and the refining time is 30min. The hydrogen content of the melt after refining is 0.24mL / 100g Al.
[0159] Online degassing: After rotary degassing and refining in the furnace, high-purity argon-chlorine mixed gas of not less than 99.999% is used for online degassing. The hydrogen content after melt purification treatment using a double-rotor online degassing device in series is 0.07mL / 100g Al;
[0160] Online filtration: After online degassing, melt filtration is performed using a deep bed;
[0161] Grain refinement: Add aluminum titanium boron wire online to refine the as-cast structure, with a dosage of 1.6 kg / t;
[0162] Casting parameters: casting speed 41mm / min, water flow 55m 3 / h. root, the flow plate aluminum liquid temperature is 698℃, the water temperature is 27℃; the ingot molding effect is good;
[0163] Heat treatment process: The cast aluminum alloy is subjected to heat treatment, the heating rate of the ingot homogenization annealing is 50℃ / h, the heating time is 10h, the holding temperature is 497℃, the holding time is 15h, the cooling rate is 80℃ / h, and the cooling time is 6h.
[0164] Ingot rolling: After the ingot is milled and coated with aluminum, it is heated to 400℃ and kept at this temperature for 8 hours. After the ingot is heated, it is roughly hot rolled into a 30mm thick billet, and then hot finished rolled to a 6mm billet, which is first pre-annealed and then cold rolled to 0.8mm. After rolling, the plate is cleaned to ensure that the emulsion on the plate is cleaned;
[0165] Annealing treatment: the plate is pre-annealed before cold rolling, the annealing temperature is 380℃, the annealing time is 80min, and the cooling method is 25℃ / h cooling rate with the furnace to below 260℃ and then air-cooled out of the furnace;
[0166] After the above processes, the cold-rolled plates are sheared and tested for performance before being packaged and delivered.
[0167] Quality Inspection:
[0168] (1) Macroscopic examination of ingot: Grain size grade 1; the test method is GB / T3246.2 "Test methods for microstructure of deformed aluminum and aluminum alloy products - Part 2 Macroscopic examination methods";
[0169] (2) Chemical composition: Si 0.05wt%, Fe 0.16wt%, Cu 4.61wt%, Mg 1.38wt%, Cu / Mg=3.34, Mn 0.59wt%, Cr 0.01wt%, Zn 0.03wt%, Ti 0.02wt%, Be 0.0007wt%, Na 0.0003wt%, Li 0.0004wt%, Pb 0.0012wt%, Bi 0.0005wt%, Sn 0.0006wt%; the detection method is GB / T 20975 "Analysis method of aluminum alloy" and GB / T 7999 "Photoelectric direct reading emission spectrometry analysis method of aluminum and aluminum alloy";
[0170] (3) Hydrogen content: 0.07 mL / 100 g Al; the detection method is YS / T600 "Closed-circuit method for measuring hydrogen in liquid state of aluminum and aluminum alloys";
[0171] (4) Mechanical properties: O state performance, tensile strength 171MPa, elongation 21%; T42 state performance, tensile strength 429MPa, yield strength 260MPa, elongation 22%. The test method is GB / T16865 "Test specimens and methods for tensile test of deformed aluminum, magnesium and their alloy products".
[0172] Example 3
[0173] The aluminum alloy is prepared according to the following method: ingot selection, raw material selection, smelting, composition adjustment, melt purification, grain refinement, casting, soaking, rolling and annealing are performed in sequence;
[0174] Ingot selection: Plate thickness 0.8mm; Ingot specification 450×2250mm;
[0175] Raw material selection: Al99.70 grade original aluminum ingot, Al99.95 grade or above copper plate, Al99.9 grade or above magnesium ingot, AlCu, AlBe, AlMn, AlTi master alloy, grain refiner (aluminum titanium boron wire), 2A12 alloy first-level scrap ingredients;
[0176] Melting process: After the alloy raw materials are melted, samples are taken for analysis; the melting temperature in the furnace is 750°C, and the melt composition is adjusted to the control range according to the element matching requirements (refer to Example 1);
[0177] Powder spraying in the furnace: After the composition is adjusted, high-purity argon is used in the furnace to blow granular refining agent (57wt% KCl, 42wt% MgCl2, 0.18wt% NaCl, 0.12wt% CaCl, 0.23wt% MgO, 0.30wt% H2O, the remainder is impurities) into the melt. The purity of argon should not be less than 99.995%, and the refining time is 20min;
[0178] Rotary degassing in the furnace: After the powder spray refining in the furnace is qualified, it is transferred to the holding furnace. The melt is refined with high-purity argon gas. The purity of argon gas should not be less than 99.999%. The melt temperature during refining is 740℃ and the refining time is 30min. The hydrogen content of the melt after refining is 0.19mL / 100g Al.
[0179] Online degassing: After rotary degassing and refining in the furnace, high-purity argon-chlorine mixed gas of not less than 99.999% is used for online degassing. The hydrogen content after melt purification treatment using a double-rotor online degassing device in series is 0.06mL / 100g Al;
[0180] Online filtration: After online degassing, 30+50ppi ceramic filter plates are used for melt filtration;
[0181] Grain refinement: Add aluminum titanium boron wire online to refine the as-cast structure, with a dosage of 1.0 kg / t;
[0182] Casting parameters: casting speed 41mm / min, water flow 55m 3 / h. root, the temperature of aluminum liquid in the flow plate is 690℃, and the water temperature is 27℃; the ingot forming effect is good;
[0183] Soaking process: The cast aluminum alloy is subjected to a soaking treatment, and the heating rate of the ingot homogenization annealing is 50°C / h, the heating time is 10h, the holding temperature is 495°C, the holding time is 15h, the cooling rate is 80°C / h, and the cooling time is 5h;
[0184] Ingot rolling: After the ingot is milled and coated with aluminum, it is heated to 400℃ and kept at this temperature for 8 hours. After the ingot is heated, it is roughly hot rolled into a 30mm thick billet, and then hot finished rolled to a 6mm billet, which is first pre-annealed and then cold rolled to 0.8mm. After rolling, the plate is cleaned to ensure that the emulsion on the plate is cleaned;
[0185] Annealing treatment: the plate is pre-annealed before cold rolling, the annealing temperature is 380℃, the annealing time is 80min, and the cooling method is 22℃ / h cooling rate with the furnace to below 260℃ and then air-cooled out of the furnace;
[0186] After the above processes, the cold-rolled plates are sheared and tested for performance before being packaged and delivered.
[0187] Quality Inspection:
[0188] (1) Macroscopic examination of ingot: Grain size grade 1; the test method is GB / T3246.2 "Test methods for microstructure of deformed aluminum and aluminum alloy products - Part 2 Macroscopic examination methods";
[0189] (2) Chemical composition: Si 0.05wt%, Fe 0.14wt%, Cu 4.57wt%, Mg 1.42wt%, Cu / Mg=3.22, Mn 0.57wt%, Cr 0.01wt%, Zn 0.05wt%, Ti 0.02wt%, Be 0.0007wt%, Na 0.0002wt%, Li 0.0005wt%, Pb 0.0010wt%, Bi 0.0005wt%, Sn 0.0006wt%; the detection method is GB / T 20975 "Analysis method of aluminum alloy" and GB / T 7999 "Photoelectric direct reading emission spectrometry analysis method of aluminum and aluminum alloy";
[0190] (3) Hydrogen content: 0.06 mL / 100 g Al; the detection method is YS / T600 "Closed-circuit method for measuring hydrogen in liquid state of aluminum and aluminum alloys";
[0191] (4) Mechanical properties: O state performance, tensile strength 174MPa, elongation 20%; T42 state performance, tensile strength 425MPa, yield strength 264MPa, elongation 21%. The test method is GB / T16865 "Test specimens and methods for tensile test of deformed aluminum, magnesium and their alloy products".
[0192] Comparative Example 1
[0193] The aluminum alloy is prepared according to the following method: ingot selection, raw material selection, smelting, composition adjustment, melt purification, grain refinement, casting, soaking, rolling and annealing are performed in sequence;
[0194] Ingot selection: Plate thickness 2.0mm; Ingot specification 450×2250mm;
[0195] Raw material selection: Al99.70 grade original aluminum ingot, Al99.95 grade or above copper plate, Al99.9 grade or above magnesium ingot, AlCu, AlBe, AlMn, AlTi master alloy, grain refiner (aluminum titanium boron wire), 2A12 alloy first-level scrap ingredients;
[0196] Melting process: After the alloy raw materials are melted, samples are taken for analysis; the melting temperature in the furnace is 740°C, and the melt composition is adjusted to the control range according to the element matching requirements (refer to Example 1);
[0197] Powder spraying in the furnace: After the composition is adjusted, high-purity argon is used in the furnace to blow granular refining agent (57wt% KCl, 42wt% MgCl2, 0.18wt% NaCl, 0.12wt% CaCl, 0.23wt% MgO, 0.30wt% H2O, the remainder is impurities) into the melt. The purity of argon should not be less than 99.999%, and the refining time is 20min;
[0198] Rotary degassing in the furnace: After the powder spraying refining in the furnace, the melt is transferred to the holding furnace. The melt is refined by high-purity argon-chlorine mixed gas through the high-speed rotating rotor in the furnace. The purity of argon and chlorine should be not less than 99.999%. The melt temperature during refining is 745℃ and the refining time is 30min. The hydrogen content of the melt after refining is 0.27mL / 100g Al.
[0199] Online degassing: After rotary degassing and refining in the furnace, high-purity argon-chlorine mixed gas of not less than 99.999% is used for online degassing. The hydrogen content after melt purification treatment by double-rotor online degassing device in series is 0.09mL / 100g Al;
[0200] Online filtration: After online degassing, 30+50ppi ceramic filter plates are used for melt filtration;
[0201] Grain refinement: Add aluminum titanium boron wire online to refine the as-cast structure, with a dosage of 1.4kg / t;
[0202] Casting parameters: casting speed 50mm / min, water flow 55m 3 / h. root, aluminum liquid temperature of flow plate is 695℃, water temperature is 25℃;
[0203] Since the comparative example adopts a faster casting speed, the ingot cracked when casting to 2000mm and was scrapped.
[0204] Comparative Example 2
[0205] The aluminum alloy is prepared according to the following method: ingot selection, raw material selection, smelting, composition adjustment, melt purification, grain refinement, casting, soaking, rolling and annealing are performed in sequence;
[0206] Ingot selection: Plate thickness 0.8mm; Ingot specification 450×2250mm;
[0207] Raw material selection: Al99.70 grade aluminum ingot, Al99.95 grade copper plate, Al99.9 grade magnesium ingot, AlCu, AlBe, AlMn, AlTi master alloy, grain refiner (aluminum titanium boron wire), 2024 alloy first-level scrap ingredients;
[0208] Melting process: After the alloy raw materials are melted, samples are taken for analysis; the melting temperature in the furnace is 750°C, and the melt composition is adjusted to the control range according to the element matching requirements (refer to Example 1);
[0209] Powder spraying in the furnace: After the composition is adjusted, high-purity argon is used in the furnace to blow granular refining agent (57wt% KCl, 42wt% MgCl2, 0.18wt% NaCl, 0.12wt% CaCl, 0.23wt% MgO, 0.30wt% H2O, the remainder is impurities) into the melt. The purity of argon should not be less than 99.995%, and the refining time is 20min;
[0210] Rotary degassing in the furnace: After the powder spray refining in the furnace is qualified, it is transferred to the holding furnace. The melt is refined with high-purity argon gas. The purity of argon gas should not be less than 99.999%. The melt temperature during refining is 740℃ and the refining time is 30min. The hydrogen content of the melt after refining is 0.20mL / 100g Al.
[0211] Online degassing: After rotary degassing and refining in the furnace, high-purity argon-chlorine mixed gas of not less than 99.999% is used for online degassing. The hydrogen content after melt purification treatment using a double-rotor online degassing device in series is 0.06mL / 100g Al;
[0212] Online filtration: After online degassing, 30+50ppi ceramic filter plates are used for melt filtration;
[0213] Grain refinement: Add aluminum titanium boron wire online to refine the as-cast structure, with a dosage of 1.0 kg / t;
[0214] Casting parameters: casting speed 41mm / min, water flow 55m 3 / h. root, the temperature of aluminum liquid in the flow plate is 690℃, and the water temperature is 27℃; the ingot forming effect is good;
[0215] Soaking process: The cast aluminum alloy is subjected to a soaking treatment, the heating rate of the ingot homogenization annealing is 50℃ / h, the heating time is 10h, the holding temperature is 495℃, the holding time is 15h, and air cooling is adopted after the holding, the average cooling rate is less than 30℃ / h, and the cooling time is 6h;
[0216] Ingot rolling: After the ingot is milled and coated with aluminum, it is heated to 400℃ and kept at this temperature for 8 hours. After the ingot is heated, it is roughly hot rolled into a 30mm thick billet, and then hot finished rolled to a 6mm billet, which is first pre-annealed and then cold rolled to 0.8mm. After rolling, the plate is cleaned to ensure that the emulsion on the plate is cleaned;
[0217] Annealing treatment: the plate is pre-annealed before cold rolling, the annealing temperature is 380℃, the annealing time is 80min, and the cooling method is 25℃ / h cooling rate with the furnace to below 260℃ and then air-cooled out of the furnace;
[0218] After the above processes, the cold-rolled plates are sheared and tested for performance before being packaged and delivered.
[0219] Quality Inspection:
[0220] (1) Macroscopic examination of ingot: Grain size grade 1; the test method is GB / T3246.2 "Test methods for microstructure of deformed aluminum and aluminum alloy products - Part 2 Macroscopic examination methods";
[0221] (2) Chemical composition: Si 0.05wt%, Fe 0.14wt%, Cu 4.57wt%, Mg 1.42wt%, Cu / Mg 3.22, Mn 0.57wt%, Cr 0.01wt%, Zn 0.05wt%, Ti 0.02wt%, Be 0.0007wt%, Na 0.0002wt%, Li 0.0005wt%, Pb 0.0010wt%, Bi 0.0005wt%, Sn 0.0006wt%; the detection method is GB / T 20975 "Analysis method of aluminum alloy" and GB / T 7999 "Photoelectric direct reading emission spectrometry analysis method of aluminum and aluminum alloy";
[0222] (3) Hydrogen content: 0.06 mL / 100 g Al; the detection method is YS / T600 "Closed-circuit method for measuring hydrogen in liquid state of aluminum and aluminum alloys";
[0223] (4) Mechanical properties: O state performance, tensile strength 160MPa, elongation 22%; T42 state performance, tensile strength 415MPa, yield strength 248MPa, elongation 24%. The test method is GB / T16865 "Test specimens and methods for tensile test of deformed aluminum, magnesium and their alloy products".
[0224] Since the comparative example adopts a slower cooling rate, the yield strength of the plate does not meet the product requirements and is scrapped.
[0225] Comparative Example 3
[0226] The aluminum alloy is prepared according to the following method: ingot selection, raw material selection, smelting, composition adjustment, melt purification, grain refinement, casting, soaking, rolling and annealing are performed in sequence;
[0227] Ingot selection: Plate thickness 0.8mm; Ingot specification 450×2250mm;
[0228] Raw material selection: Al99.70 grade original aluminum ingot, Al99.95 grade or above copper plate, Al99.9 grade or above magnesium ingot, AlCu, AlBe, AlMn, AlTi master alloy, grain refiner (aluminum titanium boron wire), 2A12 alloy first-level scrap ingredients;
[0229] Melting process: After the alloy raw materials are melted, samples are taken for analysis; the melting temperature in the furnace is 750°C, and the melt composition is adjusted to the control range according to the element matching requirements (refer to Example 1);
[0230] Powder spraying in the furnace: After the composition is adjusted, high-purity argon is used in the furnace to blow granular refining agent (57wt% KCl, 42wt% MgCl2, 0.18wt% NaCl, 0.12wt% CaCl, 0.23wt% MgO, 0.30wt% H2O, the remainder is impurities) into the melt. The purity of argon should not be less than 99.995%, and the refining time is 20min;
[0231] Rotary degassing in the furnace: After the powder spraying refining in the furnace, the qualified melt is transferred to the holding furnace. The melt is refined by high-purity argon-chlorine mixed gas through the high-speed rotating rotor in the furnace. The purity of argon and chlorine should be not less than 99.999%. The melt temperature during refining is 745℃ and the refining time is 30min. The hydrogen content of the melt after refining is 0.25mL / 100g Al.
[0232] Online degassing: After rotary degassing and refining in the furnace, high-purity argon-chlorine mixed gas of not less than 99.999% is used for online degassing. The hydrogen content after melt purification treatment using a double-rotor online degassing device in series is 0.09mL / 100g Al;
[0233] Online filtration: After online degassing, melt filtration is performed using a deep bed;
[0234] Grain refinement: Add aluminum titanium boron wire online to refine the as-cast structure, with a dosage of 1.6 kg / t;
[0235] Casting parameters: casting speed 41mm / min, water flow 60m 3 / h. root, the flow plate aluminum liquid temperature is 698℃, the water temperature is 27℃; the ingot molding effect is good;
[0236] Heat treatment process: The cast aluminum alloy is subjected to heat treatment, and the heating rate of the ingot homogenization annealing is 50℃ / h, the heating time is 10h, the holding temperature is 497℃, the holding time is 15h, the cooling rate is 80℃ / h, and the cooling time is 6h;
[0237] Ingot rolling: After the ingot is milled and coated with aluminum, it is heated to 400℃ and kept at this temperature for 8 hours. After the ingot is heated, it is roughly hot rolled into a 30mm thick billet, and then hot finished rolled to a 6mm billet, which is first pre-annealed and then cold rolled to 0.8mm. After rolling, the plate is cleaned to ensure that the emulsion on the plate is cleaned;
[0238] Annealing treatment: the plate is pre-annealed before cold rolling, the annealing temperature is 380℃, the annealing time is 80min, the cooling method is to adopt a cooling rate of no more than 25℃ / h and air-cool with the furnace to below 260℃ before being air-cooled out of the furnace;
[0239] After the above processes, the cold-rolled plates are sheared and tested for performance before being packaged and delivered.
[0240] Quality Inspection:
[0241] (1) Macroscopic examination of ingot: Grain size grade 1; the test method is GB / T3246.2 "Test methods for microstructure of deformed aluminum and aluminum alloy products - Part 2 Macroscopic examination methods";
[0242] (2) Chemical composition: Si 0.05wt%, Fe 0.16wt%, Cu 4.31wt%, Mg 1.61wt%, Cu / Mg=2.68, Mn 0.60wt%, Cr 0.01wt%, Zn 0.03wt%, Ti 0.02wt%, Be 0.0008wt%, Na 0.0003wt%, Li 0.0004wt%, Pb 0.0013wt%, Bi 0.0005wt%, Sn 0.0005wt%; the detection method is GB / T 20975 "Analysis method of aluminum alloy" and GB / T 7999 "Photoelectric direct reading emission spectrometry analysis method of aluminum and aluminum alloy";
[0243] (3) Hydrogen content: 0.09 mL / 100 g Al; the detection method is YS / T600 "Closed-circuit method for measuring hydrogen in liquid state of aluminum and aluminum alloys";
[0244] (4) Mechanical properties: O state performance, tensile strength 161MPa, elongation 23%; T42 state performance, tensile strength 409MPa, yield strength 245MPa, elongation 24%. The test method is GB / T16865 "Specimens and methods for tensile testing of deformed aluminum, magnesium and their alloy products";
[0245] Since the comparative example adopts a lower Cu / Mg ratio, the yield strength of the plate does not meet the product requirements and is scrapped.
[0246] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing an Al-Cu-Mg series aluminum alloy sheet, characterized in that: include: The alloy raw materials are sequentially subjected to batching, smelting, composition adjustment, melt purification, grain refinement, casting, soaking treatment, rolling and annealing to obtain Al-Cu-Mg series aluminum alloy plates; Wherein, 3≤Cu / Mg<5 in the ingredients; The casting speed in the casting is 37-46 mm / min; The cooling rate during the soaking treatment is 80 to 200° C. / h.
2. The preparation method according to claim 1, characterized in that: The ingredients of the batching are: Si≤0.10wt%; Fe≤0.25wt%; Cu 3.5~5.0wt%; Mn 0.3~0.9wt%; Mg 1.0~2.0wt%; Cr≤0.05wt%; Zn≤0.10wt%; Ti≤0.05wt%; Be 0.0005~0.0015wt%; Na≤0.0005wt%; Li≤0.0010wt%; Pb≤0.002wt%; Bi≤0.001wt%; Sn≤0.001wt%; The balance is Al.
3. The preparation method according to claim 1 or 2, characterized in that: The water flow rate of the casting is 40-90m 3 / h / root; the temperature of the aluminum liquid in the flow plate is 685~710℃, and the water temperature is 22~26℃.
4. The preparation method according to any one of claims 1 to 3, characterized in that The soaking treatment is as follows: heating to 510-540° C. at a rate of 50-90° C. / h, keeping the temperature at 495-503° C. for 15-30 hours, and then cooling.
5. The preparation method according to any one of claims 1 to 4, characterized in that: Before rolling, the ingot obtained by the soaking treatment is subjected to milling, aluminum cladding and heating treatment; The temperature of the heating treatment is 350-440° C., and the insulation time is 4-12 hours.
6. The preparation method according to claim 5, characterized in that: After the heating treatment, the following operations are performed: The obtained ingot is sequentially subjected to hot rough rolling, hot finish rolling and cold rolling; The thickness of the blank obtained by the hot rough rolling is 20-30 mm; the thickness of the blank obtained by the hot finish rolling is 5-12 mm; the thickness of the blank obtained by the cold rolling is 0.8-4 mm.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The annealing temperature is 350-440°C and the time is 60-180min; The annealing step further includes cooling, wherein the cooling rate is in the range of 10 to 28° C. / h; The annealing is replaced by solution quenching.
8. The preparation method according to any one of claims 1 to 7, characterized in that The melt purification includes powder spraying in the furnace, rotary degassing in the furnace, online degassing and online filtration; The hydrogen content of the melt after the melt purification is within 0.10ml / 100g Al; the slag content of the melt is within 0.02mm 2 / kg or N20 is within 20K / kg.
9. An Al-Cu-Mg aluminum alloy sheet prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The Al-Cu-Mg series aluminum alloy plate ingot has a thickness of 450-550 mm, a width of 2150-2750 mm, and a length of 2500-7000 mm.
10. Use of the Al-Cu-Mg aluminum alloy sheet prepared by the preparation method according to any one of claims 1 to 8 or the Al-Cu-Mg aluminum alloy sheet according to claim 9 in the preparation of aerospace skins.
Citation Information
Patent Citations
Heat treatment method for improving fatigue crack growth rate of 2xxx-T3 plate
CN105441838A
Processing technology for improving fatigue damage resistance of 2xxx series aluminium alloy plate
CN105441839A
Machining technology for improving fatigue damage resisting performance of 2xxx aluminum alloy plate
CN105483579A
Processing method of T4-state 2024 aluminum alloy sheet
CN110218921A
Method for preparing Al-Cu-Mg alloy oversized ingots
CN111270116A