L245MH hydrogen delivery pipeline steel and production method thereof

By adopting a combination of specific chemical components and process flow in the hydrogen conveying pipeline, the problem of hydrogen embrittlement damage in high pressure and long distance transportation of the hydrogen conveying pipeline is solved, and excellent mechanical properties and low production in a 10MPa pure hydrogen environment are achieved. Cost, suitable for large-diameter pipeline steel at higher pressures and longer distances.

CN119020701AInactive Publication Date: 2024-11-26HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410997634.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing hydrogen transport pipelines are prone to hydrogen embrittlement damage during high pressure and long distance transportation, and the plasticity, toughness and fatigue properties of the materials are deteriorated. The existing technology has high cost and long production cycles, making it difficult to be suitable for higher pressures and more Research and development of long-distance large-diameter pipeline steel.

Method used

Using specific chemical components combinations and process flows, including pre-desulfurization of molten iron, converter smelting, LF refining, RH refining, continuous casting, heating, rolling and cooling processes, control chemical components such as C, Si, Mn, Cr, Nb, Ti The content and process parameters of equal elements form L245MH hydrogen conveying pipeline steel with excellent high-pressure hydrogen compatibility, ensuring excellent mechanical properties in a 10MPa pure hydrogen environment.

Benefits of technology

In a pure hydrogen environment of 10MPa, the ratio of tensile strength, elongation after break and cross-section shrinkage to the air environment is greater than 0.90 and 0.95, and the CTOD value of step-type compact tensile specimens is greater than 0.80, which significantly improves the material's resistance. Hydrogen embrittlement performance, while reducing production costs and lead times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020701A_ABST
    Figure CN119020701A_ABST
Patent Text Reader

Abstract

The invention discloses L245MH hydrogen delivery pipeline steel and a production method thereof. The pipeline steel comprises the following chemical components in percentage by mass: 0.020 to 0.035 percent of C, 0.30 to 0.40 percent of Si, 1.3 to 1.8 percent of Mn, less than or equal to 0.010 percent of P, less than or equal to 0.001 percent of S, 0.15 to 0.30 percent of Cr, 0.01 to 0.02 percent of Alt, 0.01 to 0.02 percent of Nb, 0.01 to 0.02 percent of Ti and the balance of Fe and inevitable impurities. The production method comprises the procedures of molten iron pre-desulfurization, converter smelting, LF refining, RH vacuum refining, continuous casting, heating, rolling, cooling and coiling. The pipeline steel provided by the invention not only has mechanical properties of conventional pipeline steel, but also has excellent high-pressure hydrogen compatibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of long-distance pipeline steel preparation, and specifically relates to L245MH hydrogen transmission pipeline steel and a production method thereof. Background Art

[0002] As a green, low-carbon energy, hydrogen energy has many ways to obtain and a wide range of applications, and has great development prospects. At present, my country's hydrogen energy industry has begun to take shape, but the distribution of domestic hydrogen resources is extremely uneven. Hydrogen resources are mainly distributed in the northwest, northeast, and central and western regions where refining enterprises, wind and solar power generation, and natural gas resources are rich. The consumer market is mainly concentrated in the eastern and southern regions. Long-distance hydrogen energy transportation has become a bottleneck restricting the large-scale development of the hydrogen energy industry.

[0003] Pipeline transportation of high-pressure hydrogen is efficient and economical, and is the best way to achieve large-scale, long-distance hydrogen transportation. However, hydrogen has a high diffusion rate and strong permeability in metal materials. Long-term service in a high-pressure hydrogen-containing environment will cause "hydrogen embrittlement" damage to the material. When micro-defects in the material expand to a critical size, fracture failure will occur. In a high-pressure gaseous hydrogen environment, the plasticity, toughness, and fatigue properties of existing pipeline steel materials will deteriorate significantly. Currently, existing hydrogen pipelines mainly use seamless pipes, with a transmission pressure of ≤4MPa and a pipe diameter between 50-300mm. In the future, with the large-scale use of hydrogen, large-diameter pipeline steels suitable for higher pressures and longer distances are urgently needed to be developed.

[0004] Chinese patent CN 114645215 A discloses an L245S hydrogen pipeline and its production method, which can produce pipeline steel with a yield strength of 350-420MPa and a tensile strength of 440-500MPa in a 6MPa hydrogen environment. However, the invention adopts an online quenching + offline tempering process, which has high process costs and a long production cycle, and the product can only be used in a 6MPa hydrogen environment. Summary of the invention

[0005] The purpose of the present invention is to provide an L245MH hydrogen transmission pipeline steel and a production method thereof, so as to solve the key technology of steel plates for high-pressure and long-distance hydrogen storage pipeline transportation. In addition to the mechanical properties that conventional pipeline steels should have, the steel plate also has excellent high-pressure hydrogen compatibility. In a pure hydrogen environment of 10MPa, the ratios of the tensile strength, elongation after fracture, and cross-sectional shrinkage of the notched specimen to those in the air environment are greater than 0.90 and 0.95, and the ratio of the CTOD value of the step-type compact tensile specimen to that of the air environment is greater than 0.8.

[0006] To achieve the above object, the present invention adopts the following technical solutions: The invention discloses an L245MH hydrogen transmission pipeline steel, wherein the chemical composition and the mass percentage thereof are as follows: C: 0.020-0.035%, Si: 0.30-0.40%, Mn: 1.2-1.5%, P≤0.010%, S≤0.001%, Cr: 0.15-0.30%, Alt: 0.01-0.02%, Nb: 0.01-0.02%, Ti: 0.01-0.02%, and the balance is Fe and unavoidable impurities.

[0007] The components and contents of the L245MH hydrogen pipeline steel of the present invention are set based on the following: C: Carbon is one of the most effective elements in strengthening effect. It plays a role of solid solution strengthening and significantly improves the strength of steel. It is the basic element for forming ferrite. However, too high carbon content will seriously affect the steel's resistance to hydrogen embrittlement. Therefore, the design range of carbon content is 0.020~0.035%.

[0008] Si: Silicon also plays a role in solid solution strengthening. Silicon is dissolved in ferrite and can improve the strength and toughness of steel. However, too high silicon content will cause the carbon in the material to graphitize during heat treatment. Therefore, the design range of silicon content is 0.30~0.40%.

[0009] Mn: Manganese can be dissolved in ferrite to improve the strength of steel and expand the austenite phase; but too high a manganese content will cause banded segregation in the steel; this patent is to obtain a certain amount of residual austenite to improve the resistance to hydrogen embrittlement, so the manganese content is designed to range from 1.2 to 1.5%.

[0010] Cr: Chromium can improve the hardenability of steel, form chromium alloy carbides, disperse finely, refine the structure, and improve the strength and plasticity of steel; but too much chromium will cause seasonal sensitivity of steel and make the mechanical properties unstable, so the design range of chromium content is 0.15~0.30%.

[0011] Alt: Aluminum is the main deoxidizing element, which reduces the oxygen content of steel and plays a role in nitrogen fixation. However, excessive addition can easily lead to an increase in the size and content of inclusions, reducing the steel's resistance to hydrogen embrittlement. Therefore, the design range of aluminum is an appropriate addition amount of 0.01-0.02%.

[0012] Nb, Ti: Niobium and titanium are precipitation strengthening and fine grain strengthening elements for steel. The carbonitride precipitation at different stages of slab heating and hot rolling plays a role in grain refinement and precipitation strengthening, while improving the strength and toughness of steel. Niobium carbides are strong hydrogen traps, further improving the hydrogen embrittlement resistance of steel; titanium TiC particles can provide effective hydrogen capture sites, and evenly dispersed TiC can effectively inhibit the growth of the original austenite grains of the material. Considering the addition effect and alloy cost, the niobium content is designed to be 0.01-0.02%, and the titanium content is designed to be 0.01-0.02%.

[0013] P, S: Phosphorus and sulfur are harmful elements that damage the plasticity of steel. The lower the content, the better. Taking the production cost into comprehensive consideration, the phosphorus content is designed to be ≤0.001%, and the sulfur content is designed to be ≤0.001%.

[0014] The thickness of the L245MH hydrogen transmission pipeline steel of the present invention is 10 to 15 mm.

[0015] The hot-rolled structure of the L245MH hydrogen pipeline steel of the present invention is ferrite and a small amount of residual austenite, the grain size grade is ≥10.0, the yield strength is 245-400MPa, the tensile strength is 415-485MPa, the elongation is ≥30%, and the -20°C Charpy V-notch impact energy is ≥300J.

[0016] The L245MH hydrogen transmission pipeline steel of the present invention has a tensile strength and a cross-sectional shrinkage rate of a notched specimen greater than 90% and 95% in an air environment in a pure hydrogen environment at 10 MPa, and a CTOD value of a step-type compact tensile specimen greater than 80% in an air environment.

[0017] The production method of L245MH hydrogen transmission pipeline steel of the present invention comprises the steps of molten iron pre-desulfurization, converter smelting, LF refining, RH refining, continuous casting, heating, rolling, cooling and coiling.

[0018] Preferably, in the converter smelting process of the present invention, the P content in the molten steel is ≤0.010wt% and the S content is ≤0.003wt% when the converter is tapped; in the LF refining process, white slag desulfurization is adopted, and the S content control target is ≤0.001wt%. In the RH refining process, the vacuum cycle time is ≥25min; the molten steel after RH vacuum refining is fed into the calcium wire for ≥150m for calcium treatment, and the soft argon blowing time after calcium treatment is ≥8min, and secondary heating after calcium treatment is strictly prohibited.

[0019] Preferably, the continuous casting process of the present invention: adopts full-process protective casting, uses dynamic light reduction, the reduction amount is ≥7mm, the secondary cooling water adopts weak cooling mode, the casting superheat is 15-30°C, and the slab pulling speed is 0.8-1.0m / min for constant speed casting.

[0020] Preferably, the heating process of the present invention has a heating temperature of 1180-1220° C. and a heating time of 180-200 min.

[0021] Preferably, in the rolling process of the present invention, the rough rolling end temperature is 1100-1200° C., the finishing temperature of the finishing rolling is 820-870° C.; the finishing rolling is performed for 5-7 passes, and the cumulative reduction is ≥70%.

[0022] Preferably, the cooling process of the present invention is as follows: the slab after finish rolling is sent to a laminar cooling section for accelerated cooling at a cooling rate of 15-20°C / s, and then air-cooled to 600-650°C for coiling; after coiling, the steel coils are stacked and slowly cooled.

[0023] The beneficial effects of adopting the above technical solution are: (1) In terms of composition design, the present invention adopts low carbon equivalent and ultra-low phosphorus and sulfur to ensure controllable center segregation; increases the Mn element content to expand the austenite phase region; adds niobium, chromium and other microalloys to obtain a low hydrogen embrittlement sensitive structure and improve the compatibility of the material in a high-pressure hydrogen environment.

[0024] (2) The present invention adopts a dual process for steelmaking to ensure ultra-low inclusions and phosphorus and sulfur control; adopts the TMCP process, which has low production costs and short delivery cycles, and has market competitive advantages; by reducing the cooling rate, high temperature curling, and adopting slow cooling, a certain amount of residual austenite structure is obtained, thereby improving the hydrogen embrittlement resistance.

[0025] (3) The L245MH steel plate provided by the present invention has a grain size of more than 10 grades, a banded structure of 0.5 grades and below, a total amount of inclusions not exceeding 2.0 grades, and uniform and stable steel plate performance. In addition to meeting the mechanical properties of conventional pipelines, it also has excellent resistance to high-pressure gas-phase hydrogen embrittlement. In a pure hydrogen environment of 10MPa, the tensile strength and cross-sectional shrinkage of the notched specimen are greater than 90% and 95% of those in the air environment, and the CTOD value of the step-type compact tensile specimen is greater than 80% of that in the air environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a transmission image of the structure of the steel plate in Example 1. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is further described in detail below in conjunction with embodiments. Example 1

[0028] The thickness of L245MH hydrogen pipeline steel in this embodiment is 14.3 mm, and the chemical composition is C=0.023%, Si=0.39%, Mn=1.45%, P=0.008%, S=0.0008%, Cr=0.15%, Alt=0.016%, Nb=0.015%, Ti=0.015%, and the balance is Fe and unavoidable impurities; its production method includes molten iron pre-desulfurization, converter smelting, LF refining, RH refining, continuous casting, heating, rolling, cooling and coiling processes; key process parameters are controlled as follows: (1) Steelmaking: The P content in the molten steel is 0.0071% and the S content is 0.0029% when the converter is tapped; in the LF refining process, white slag desulfurization is used, and the S content out of the station is 0.0008%. The RH vacuum cycle time is 25.4 minutes. The molten steel after RH vacuum refining is fed into the calcium line for 155 meters for calcium treatment. After calcium treatment, the soft argon blowing time is 9 minutes.

[0029] (2) Continuous casting: full-process protection pouring is adopted, dynamic light pressure is used, the pressure reduction is 7mm, the secondary cooling water adopts weak cooling mode, the casting overheat is 18℃, and the slab pulling speed is 0.85m / min for constant speed casting.

[0030] (3) Heating: heating temperature 1190°C, heating time 180 min.

[0031] (4) Rolling: The end temperature of rough rolling is 1100℃, and the end temperature of finishing rolling is 852℃; finishing rolling is performed in 7 passes with a cumulative reduction of 76%.

[0032] (5) Cooling: The slab after finish rolling is sent to the laminar cooling section for accelerated cooling at a cooling rate of 15°C / s, and then air-cooled to 640°C for coiling; after coiling, the steel coils are stacked and slowly cooled.

[0033] The mechanical properties of the L245MH hydrogen pipeline steel of this embodiment are shown in Table 1; the performance ratio in a 10 MPa pure hydrogen environment to that in an air environment is shown in Table 2.

[0034] The microstructure transmission diagram of the pipeline steel in this embodiment is shown in Figure 1 ,Depend on Figure 1 It can be seen that the structure is a ferrite structure with a residual austenite structure. The structures of the pipeline steels in the other embodiments are the same as those in embodiment 1 and are not shown one by one. Example 2

[0035] The thickness of L245MH hydrogen pipeline steel in this embodiment is 12.7 mm, and the chemical composition is C=0.030%, Si=0.31%, Mn=1.25%, P=0.007%, S=0.0006%, Cr=0.17%, Alt=0.016%, Nb=0.016%, Ti=0.015%, and the balance is Fe and unavoidable impurities; its production method includes molten iron pre-desulfurization, converter smelting, LF refining, RH refining, continuous casting, heating, rolling, cooling and coiling processes; key process parameters are controlled as follows: (1) Steelmaking: The P content in the molten steel is 0.007% and the S content is 0.0027% when the converter is tapped; in the LF refining process, white slag desulfurization is used, and the S content out of the station is 0.0006%. The RH vacuum cycle time is 25 minutes. The molten steel after RH vacuum refining is fed into the calcium line for 150 meters for calcium treatment. After calcium treatment, the soft argon blowing time is 8.5 minutes.

[0036] (2) Continuous casting: full-process protection pouring is adopted, dynamic light pressure is used, the pressure reduction is 7mm, the secondary cooling water adopts weak cooling mode, the casting overheat is 20℃, and the slab pulling speed is 0.90m / min for constant speed casting.

[0037] (3) Heating: heating temperature 1190°C, heating time 180 min.

[0038] (4) Rolling: The end temperature of rough rolling is 1130℃, and the end temperature of finishing rolling is 842℃; finishing rolling is performed in 7 passes with a cumulative reduction of 76%.

[0039] (5) Cooling: The slab after finish rolling is sent to the laminar cooling section for accelerated cooling at a cooling rate of 20°C / s, and then air-cooled to 610°C for coiling; after coiling, the steel coil is stacked and slowly cooled.

[0040] The mechanical properties of the L245MH hydrogen pipeline steel of this embodiment are shown in Table 1; the performance ratio in a 10 MPa pure hydrogen environment to that in an air environment is shown in Table 2. Example 3

[0041] The thickness of L245MH hydrogen pipeline steel in this embodiment is 14.8 mm, and the chemical composition is C=0.027%, Si=0.33%, Mn=1.20%, P=0.007%, S=0.007%, Cr=0.20%, Alt=0.02%, Nb=0.013%, Ti=0.016%, and the balance is Fe and unavoidable impurities; its production method includes molten iron pre-desulfurization, converter smelting, LF refining, RH refining, continuous casting, heating, rolling, cooling and coiling processes; key process parameters are controlled as follows: (1) Steelmaking: The P content in the molten steel is 0.0083% and the S content is 0.0028% when the converter is tapped; in the LF refining process, white slag desulfurization is used, and the S content out of the station is 0.0007%. The RH vacuum cycle time is 25.5 minutes. The molten steel after RH vacuum refining is fed into the calcium line 152m for calcium treatment. After calcium treatment, the soft argon blowing time is 8 minutes.

[0042] (2) Continuous casting: full-process protection pouring is adopted, dynamic light pressure is used, the pressure reduction is 8mm, the secondary cooling water adopts weak cooling mode, the casting overheat is 25℃, and the slab pulling speed is 1.0m / min for constant speed casting.

[0043] (3) Heating: heating temperature 1210℃, heating time 200min.

[0044] (4) Rolling: The end temperature of rough rolling is 1180℃, and the end temperature of finishing rolling is 865℃; finishing rolling is performed in 6 passes with a cumulative reduction of 73%.

[0045] (5) Cooling: The slab after finish rolling is sent to the laminar cooling section for accelerated cooling at a cooling rate of 20°C / s, and then air-cooled to 630°C for coiling; after coiling, the steel coil is stacked and slowly cooled.

[0046] The mechanical properties of the L245MH hydrogen pipeline steel of this embodiment are shown in Table 1; the performance ratio in a 10 MPa pure hydrogen environment to that in an air environment is shown in Table 2. Example 4

[0047] The thickness of L245MH hydrogen pipeline steel in this embodiment is 15.9 mm, and the chemical composition is C=0.035%, Si=0.30%, Mn=1.30%, P=0.008%, S=0.006%, Cr=0.27%, Alt=0.01%, Nb=0.018%, Ti=0.02%, and the balance is Fe and unavoidable impurities; its production method includes molten iron pre-desulfurization, converter smelting, LF refining, RH refining, continuous casting, heating, rolling, cooling and coiling processes; key process parameters are controlled as follows: (1) Steelmaking: The P content in the molten steel is 0.0079% and the S content is 0.0027% when the converter is tapped; in the LF refining process, white slag desulfurization is used, and the S content out of the station is 0.0006%. The RH vacuum cycle time is 26 minutes. The molten steel after RH vacuum refining is fed into the calcium line 153m for calcium treatment. After calcium treatment, the soft argon blowing time is 8.5 minutes.

[0048] (2) Continuous casting: full-process protection pouring is adopted, dynamic light pressure is used, the pressure reduction is 8mm, the secondary cooling water adopts weak cooling mode, the casting overheat is 30℃, and the slab pulling speed is 0.95m / min for constant speed casting.

[0049] (3) Heating: heating temperature 1220℃, heating time 200min.

[0050] (4) Rolling: The end temperature of rough rolling is 1160℃, and the end temperature of finishing rolling is 858℃; finishing rolling is performed in 6 passes with a cumulative reduction of 74%.

[0051] (5) Cooling: The slab after finish rolling is sent to the laminar cooling section for accelerated cooling at a cooling rate of 18°C / s, and then air-cooled to 600°C for coiling; after coiling, the steel coil is stacked and slowly cooled.

[0052] The mechanical properties of the L245MH hydrogen pipeline steel of this embodiment are shown in Table 1; the performance ratio in a 10 MPa pure hydrogen environment to that in an air environment is shown in Table 2. Example 5

[0053] The thickness of L245MH hydrogen pipeline steel in this embodiment is 11.7 mm, and the chemical composition is C=0.032%, Si=0.38%, Mn=1.50%, P=0.009%, S=0.005%, Cr=0.30%, Alt=0.013%, Nb=0.02%, Ti=0.01%, and the balance is Fe and unavoidable impurities; its production method includes molten iron pre-desulfurization, converter smelting, LF refining, RH refining, continuous casting, heating, rolling, cooling and coiling processes; key process parameters are controlled as follows: (1) Steelmaking: The P content in the molten steel is 0.0072% and the S content is 0.0025% when the converter is tapped; in the LF refining process, white slag desulfurization is used, and the S content out of the station is 0.0009%. The RH vacuum cycle time is 25.3 minutes. The molten steel after RH vacuum refining is fed into the calcium line for 150 meters for calcium treatment. After calcium treatment, the soft argon blowing time is 9 minutes.

[0054] (2) Continuous casting: full-process protection pouring is adopted, dynamic light pressure is used, the pressure reduction is 8.5 mm, the secondary cooling water adopts weak cooling mode, the casting overheat is 15°C, and the slab pulling speed is 0.80 m / min for constant speed casting.

[0055] (3) Heating: heating temperature 1200°C, heating time 185 min.

[0056] (4) Rolling: The end temperature of rough rolling is 1200℃, and the end temperature of finishing rolling is 870℃; finishing rolling is performed in 5 passes with a cumulative reduction of 72%.

[0057] (5) Cooling: The slab after finish rolling is sent to the laminar cooling section for accelerated cooling at a cooling rate of 18°C / s, and then air-cooled to 620°C for coiling; after coiling, the steel coils are stacked and slowly cooled.

[0058] The mechanical properties of the L245MH hydrogen pipeline steel of this embodiment are shown in Table 1; the performance ratio in a 10 MPa pure hydrogen environment to that in an air environment is shown in Table 2. Example 6

[0059] The thickness of L245MH hydrogen pipeline steel in this embodiment is 10.8 mm, and the chemical composition is C=0.020%, Si=0.40%, Mn=1.35%, P=0.006%, S=0.008%, Cr=0.30%, Alt=0.015%, Nb=0.01%, Ti=0.012%, and the balance is Fe and unavoidable impurities; its production method includes molten iron pre-desulfurization, converter smelting, LF refining, RH refining, continuous casting, heating, rolling, cooling and coiling processes; key process parameters are controlled as follows: (1) Steelmaking: The P content in the molten steel is 0.0075% and the S content is 0.0029% when the converter is tapped; in the LF refining process, white slag desulfurization is used, and the S content out of the station is 0.0007%. The RH vacuum cycle time is 25.5 minutes. The molten steel after RH vacuum refining is fed into the calcium line 155m for calcium treatment. After calcium treatment, the soft argon blowing time is 8.5 minutes.

[0060] (2) Continuous casting: full-process protection pouring is adopted, dynamic light pressure is used, the pressure reduction is 7.5 mm, the secondary cooling water adopts weak cooling mode, the casting overheat is 20°C, and the slab pulling speed is 0.90 m / min for constant speed casting.

[0061] (3) Heating: heating temperature 1180°C, heating time 180 min.

[0062] (4) Rolling: The end temperature of rough rolling is 1150℃, and the end temperature of finishing rolling is 822℃; finishing rolling is performed in 7 passes with a cumulative reduction of 78%.

[0063] (5) Cooling: The slab after finish rolling is sent to the laminar cooling section for accelerated cooling at a cooling rate of 15°C / s, and then air-cooled to 650°C for coiling; after coiling, the steel coil is stacked and slowly cooled.

[0064] The mechanical properties of the L245MH hydrogen pipeline steel of this embodiment are shown in Table 1; the performance ratio in a 10 MPa pure hydrogen environment to that in an air environment is shown in Table 2.

[0065] Table 1 Mechanical properties test results of pipeline steel in various examples

[0066] Table 2 Hydrogen compatibility test results of pipeline steel in various examples

[0067] It can be seen from Tables 1 and 2 that the L245MH hydrogen transmission pipeline steel provided by the present invention not only meets the mechanical properties of conventional pipelines, but also has excellent resistance to high-pressure gas-phase hydrogen embrittlement. In a pure hydrogen environment of 10 MPa, the tensile strength and cross-sectional shrinkage of the notched specimen are greater than 90% and 95% of those in the air environment, and the CTOD value of the step-type compact tensile specimen is greater than 80% of that in the air environment.

Claims

1. A L245MH hydrogen transmission pipeline steel, characterized by: The chemical composition and mass percentage of the pipeline steel are: C: 0.020-0.035%, Si: 0.30-0.40%, Mn: 1.2-1.5%, P≤0.010%, S≤0.001%, Cr: 0.15-0.30%, Alt: 0.01-0.02%, Nb: 0.01-0.02%, Ti: 0.01-0.02%, and the balance is Fe and unavoidable impurities.

2. The L245MH hydrogen pipeline steel according to claim 1, characterized in that: The hot-rolled microstructure of the pipeline steel is ferrite and a small amount of residual austenite, with a grain size grade ≥10.0; a yield strength of 300-400 MPa, a tensile strength of 415-485 MPa, an elongation of ≥30%, and a -20°C Charpy V-notch impact energy of ≥300 J.

3. A L245MH hydrogen pipeline steel according to claim 1 or 2, characterized in that: In a pure hydrogen environment of 10 MPa, the tensile strength and cross-sectional shrinkage rate of the notched specimen of the pipeline steel are greater than 90% and 95% of those in an air environment, and the CTOD value of the step-type compact tensile specimen is greater than 80% of that in an air environment.

4. A method for producing L245MH hydrogen pipeline steel according to any one of claims 1 to 3, characterized in that: It includes molten iron pre-desulfurization, converter smelting, LF refining, RH refining, continuous casting, heating, rolling, cooling and coiling processes.

5. The method for producing L245MH hydrogen pipeline steel according to claim 4, characterized in that: The converter smelting process: when the converter taps steel, the P content in the molten steel is ≤0.010wt%, and the S content is ≤0.003wt%; in the LF refining process, white slag desulfurization is adopted, and the S content control target is ≤0.001wt%; in the RH refining process, the vacuum cycle time is ≥25min; the molten steel after RH vacuum refining is fed into the calcium wire for ≥150m for calcium treatment, and the soft argon blowing time after calcium treatment is ≥8min, and secondary heating after calcium treatment is strictly prohibited.

6. The method for producing L245MH hydrogen pipeline steel according to claim 4, characterized in that: The continuous casting process adopts full-process protection pouring, uses dynamic light pressure reduction, the pressure reduction amount is ≥7mm, the secondary cooling water adopts weak cooling mode, the casting overheat is 15-30°C, and the slab pulling speed is 0.8-1.0m / min for constant speed casting.

7. The method for producing L245MH hydrogen pipeline steel according to claim 4, characterized in that: The heating process comprises a heating temperature of 1180 to 1220° C. and a heating time of 180 to 200 minutes.

8. The method for producing L245MH hydrogen pipeline steel according to claim 4, characterized in that: The rolling process comprises: a rough rolling end temperature of 1100-1200° C., a finishing rolling end temperature of 820-870° C., and finishing rolling of 5-7 passes with a cumulative reduction of ≥70%.

9. The method for producing L245MH hydrogen pipeline steel according to claim 4, characterized in that: The cooling process comprises sending the finish-rolled slab into a laminar cooling section for accelerated cooling at a cooling rate of 15-20°C / s, and then air-cooling to 600-650°C for coiling; after coiling, the steel coil is stacked and slowly cooled.

Citation Information

Patent Citations

  • High intensity and high-toughness hot-rolled steel sheet and method for producing the same

    CN101397626A

  • Hot-rolled steel sheet for thick high strength line pipes, welded steel pipe for thick high strength line pipes, and manfuacturing method therefor

    CN109312437A

  • X52 pipeline steel hot-rolling coiled plate with super-thick specification and production method for same

    CN110777296A

  • High-cleanliness pipeline steel and smelting method thereof

    CN113278877A

  • Pipeline steel and manufacturing method thereof

    CN113637897A