TiAl alloy surface high-temperature anti-oxidation coating and preparation method thereof

The preparation of TiAlCrM/TiAlCrNb double-layer coating through magnetron sputtering and multi-arc ion plating technology solves the problem of insufficient oxidation resistance of TiAl alloy in high temperature environments, and achieves higher coating density and lower defect rate. Significantly improves the thermal cycle life and anti-oxidation properties of the coating.

CN119020739AInactive Publication Date: 2024-11-26NANJING UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310615413.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

TiAl alloy has insufficient oxidation resistance at above 850℃, which restricts its application in high temperature environments. The coating prepared by existing vacuum plasma spraying technology has defects such as internal holes and microcracks, which affects its life and reliability.

Method used

Magneto-controlled sputtering and multi-arc ion plating technology are used to prepare the TiAlCrM/TiAlCrNb double-layer coating, including first preparing the transition layer TiAlCrNb on the surface of the TiAl alloy matrix, and then forming an oxidation-resistant layer TiAlCrM on its surface, and improving it by sandblasting and coarse treatment. The bonding properties of the coating and the substrate.

Benefits of technology

A dense oxide film is generated, which relieves stress concentration in the coating, reduces cracking and peeling, improves the thermal cycle life and oxidation resistance of the coating, reduces manufacturing costs, and reduces holes and defects, and improves coating. The bonding properties of the layer and the substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020739A_ABST
    Figure CN119020739A_ABST
Patent Text Reader

Abstract

The invention discloses a TiAl alloy surface high-temperature anti-oxidation coating and a preparation method thereof.A TiAlCrNb layer and a TiAlCrM layer are sequentially and evenly deposited on the surface of a TiAl alloy subjected to surface treatment through at least one physical vapor deposition technology of magnetron sputtering and multi-arc ion plating; the TiAlCrM component comprises 22 to 47 at% of Ti, 45 to 55 at% of Al and 10 to 27 at% of Cr, M is a trace element, the content of M is less than 1 at%, and the TiAlCrNb component comprises 20 to 40 at% of Ti, 40 to 60 at% of Al, 1 to 30 at% of Cr and 1 to 8 at% of Nb. The thermal physical performance and the element composition of the prepared coating system are close to those of a TiAl matrix, the coating system has good thermal cycle resistance, interface stability and high-temperature oxidation resistance, and the high-temperature oxidation resistance of the TiAl alloy at the temperature of 900 DEG C or above is expected to be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anti-oxidation coatings, and in particular to a high-temperature anti-oxidation coating that can be used on the surface of a TiAl alloy and a preparation method thereof. Background Art

[0002] Thrust-to-weight ratio is an important parameter of aircraft engines, which is defined as the ratio of engine thrust to gravity. To improve the thrust-to-weight ratio of an engine, one method is to increase the temperature before the turbine, and another method is to use new materials, new processes and new structures to reduce the weight of the engine. The density of TiAl alloy (3.9g / cm 3 ) is about nickel-based high-temperature alloy (7.9~8.9g / cm 3 ), and has high high-temperature strength and creep resistance. Replacing some high-temperature parts of Ni-based alloys with it can effectively reduce the weight of the engine. In 2016, the PST TiAl single crystal invented by the team of Nanjing University of Science and Technology achieved an excellent combination and leapfrog improvement in strength, plasticity and creep resistance, and overcame the two long-standing world problems of TiAl alloy's high room temperature brittleness and low service temperature. Compared with the US 4822 alloy that has been officially commercialized, the room temperature tensile plasticity has increased from less than 2% to more than 6%, the yield strength is as high as more than 700MPa, the temperature bearing capacity has increased from less than 700℃ to more than 950℃, and the creep resistance at 900℃ has increased by 1 to 2 orders of magnitude. It is expected that the use temperature of TiAl alloy will be increased to more than 900℃, replacing the last two stages of low-pressure turbine blades, achieving engine weight reduction, and improving the engine thrust-to-weight ratio. However, the insufficient oxidation resistance of TiAl alloy above 850℃ restricts its further application.

[0003] The preparation of high-temperature anti-oxidation coating on the surface of TiAl alloy can effectively protect the alloy at high temperature. It has been reported that a single-layer TiAlCrY coating was prepared on the surface of TiAl alloy by vacuum plasma spraying technology, which has certain high-temperature anti-oxidation performance. However, the TiAlCrY coating prepared by this technology has many defects such as internal holes and microcracks, which affect the life of the coating. In particular, the coating shows great brittleness. During the hot and cold cycle process, the coating is subject to thermal stress and is prone to cracking and peeling. After the coating peels off, the alloy substrate is in direct contact with the air, which will lead to the rapid failure of the entire system. The TiAlCrY / TiAlCrNb double-layer coating prepared by vacuum plasma spraying technology can generate a continuous and dense oxide film on the surface of the TiAlCrY coating at high temperature, which plays an anti-oxidation role. The internal TiAlCrNb transition layer can relieve the stress concentration of the coating, thereby increasing the thermal cycle life of the coating. However, it was found that the coating prepared by this technology contained many defects such as pores, interfaces, and microcracks that could not be eliminated. In addition, affected by the spraying environment, the coating contained a large amount of oxygen impurities, which existed at the interface, affecting the reliability and service life of the coating. Summary of the invention

[0004] In order to solve the above problems, the purpose of the present invention is to provide a high temperature anti-oxidation coating on the surface of TiAl alloy and a preparation method thereof.

[0005] On the one hand, the present invention provides a high-temperature anti-oxidation coating on the surface of a TiAl alloy, wherein the coating comprises, from the inside to the outside, a transition layer TiAlCrNb and an anti-oxidation layer TiAlCrM.

[0006] On the other hand, the present invention provides a method for preparing a high-temperature anti-oxidation coating on the surface of a TiAl alloy, using at least one physical vapor deposition technology of magnetron sputtering and multi-arc ion plating to first prepare a transition layer TiAlCrNb on the surface of a TiAl alloy substrate, and then prepare an anti-oxidation layer TiAlCrM on the surface of the transition layer TiAlCrNb.

[0007] Preferably, the main chemical composition of the anti-oxidation layer TiAlCrM is: Ti 22-47at%, Al 45-55at%, Cr 10-27at%, M is a trace element, the content of which is less than 1at%, and the trace element includes at least one of Gd, Y and Hf.

[0008] Preferably, the thickness of the anti-oxidation layer TiAlCrM is 10-50 μm.

[0009] Preferably, the main chemical components of the transition layer TiAlCrNb are: Ti 20-40at%, Al 40-60at%, Cr 1-30at%, Nb 1-8at%.

[0010] Preferably, the thickness of the transition layer TiAlCrNb is 5-20 μm.

[0011] Preferably, in order to further improve the bonding performance and thermal cycle resistance of the coating, the TiAl alloy surface is roughened by sandblasting before the coating is deposited, so as to obtain a suitable surface with a roughness Ra of 0.2 to 5.0. When the roughness is high, there are more defects at the interface between the coating and the substrate, and when the roughness is low, the bite between the coating and the substrate is weak. Compared with other sandblasting processes, sandblasting causes less damage to the substrate surface and produces fewer defects such as holes.

[0012] Compared with the prior art, the TiAl surface double-layer anti-oxidation coating and preparation process of the present invention have the following beneficial effects:

[0013] 1. The double-layer coating of the present invention has a surface TiAlCrM anti-oxidation layer that can generate a continuous and dense oxide film in a high-temperature environment, which protects the interior of the coating; adding a TiAlCrNb transition layer between the surface TiAlCrM anti-oxidation layer and the TiAl alloy substrate can alleviate the stress concentration in the coating and at the coating-substrate interface during the thermal cycle, as well as the structural defects caused by stress, and can reduce the cracking and peeling of the coating during cyclic oxidation and thermal shock. At the same time, the transition layer can slow down the difference in element concentration between the alloy substrate and the surface layer, reduce the diffusion rate of interface elements, and is more conducive to the stability of the coating structure.

[0014] 2. The coating is prepared by magnetron sputtering and multi-arc ion plating technology. The prepared coating has the remarkable characteristics of high density, few defects such as holes, microcracks, and oxygen impurities, which is conducive to controlling the lower coating thickness and ensuring the service life of the coating. In addition, controlling the coating thickness is conducive to weight reduction. The surface roughness of the coating prepared by the physical vapor deposition method is low, which reduces the later grinding process, reduces the manufacturing cost, and eliminates the influence of the component surface on the microcirculation of the airflow.

[0015] 3. The sandblasting process is used to roughen the surface of the substrate. Under the condition of ensuring less damage to the substrate surface and fewer defects such as holes, the surface area can be increased, mechanical coupling can be produced, and the bonding performance and thermal shock resistance between the coating and the substrate can be effectively improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the surface morphology of the TiAlCrY / TiAlCrNb double-layer coating on the surface of the TiAl alloy in Example 1.

[0017] Figure 2 This is the cross-sectional morphology of the TiAlCrY / TiAlCrNb double-layer coating on the surface of the TiAl alloy in Example 1.

[0018] Figure 3 The surface morphology of the TiAlCrY / TiAlCrNb double-layer coating on the surface of the TiAl alloy in Example 1 during the 1000°C water quenching thermal shock process.

[0019] Figure 4 This is the cross-sectional morphology of the TiAlCrY / TiAlCrNb double-layer coating on the surface of the TiAl alloy in Example 1 during cyclic oxidation at 1000°C.

[0020] Figure 5 This is the surface morphology of the TiAlCrY single-layer coating on the surface of the TiAl alloy in Comparative Example 1 during the 1000°C water quenching thermal shock process.

[0021] Figure 6The surface morphology of the TiAlCrY / TiAlCrNb double-layer coating on the surface of the TiAl alloy in Comparative Example 2 during the 1000°C water quenching thermal shock process (the alloy surface roughness is 0.28±0.02 μm).

[0022] Figure 7 The cross-sectional morphology of the TiAlCrY / TiAlCrNb double-layer coating on the surface of the TiAl alloy in Comparative Example 3 during cyclic oxidation at 1000°C (the alloy surface roughness is 1.36±0.10 μm). DETAILED DESCRIPTION

[0023] The above scheme is further described below in conjunction with specific implementation examples. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only an example within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description of this article, and are not limited to the specific values ​​​​exemplified below.

[0024] The present invention adopts magnetron sputtering or multi-arc ion plating technology to prepare TiAlCrM / TiAlCrNb double-layer coating. The coating prepared by magnetron sputtering and multi-arc ion plating technology has the characteristics of high density and few defects, which can effectively improve the service life of the coating; with the double-layer structure coating, the internal TiAlCrNb transition layer can better alleviate the stress concentration of the coating, while reducing the element diffusion phenomenon caused by the concentration gradient, and the surface TiAlCrX coating can play a better antioxidant role. Therefore, the coating system has better thermal cycling performance and antioxidant performance. The sandblasting process is used to treat the substrate surface to obtain a roughened surface, which can further increase the interface bonding performance between the coating and the substrate.

[0025] The method for preparing a high-temperature anti-oxidation coating on the surface of a TiAl alloy according to the present invention comprises the following steps: 1. Target material preparation: preparing TiAlCrNb and TiAlCrM alloy targets;

[0026] 2. Substrate pretreatment: Sand blasting method is used, the distance between the spray gun and the surface is 30-50mm, the sand blasting direction is 60°-90° with the substrate surface, the sand blasting time is 3-5s, and the sand blasting pressure is 0.1~0.8MPa.

[0027] 3. Deposition coating

[0028] Close the furnace door, turn on the circulating cooling water, and use a vacuum unit consisting of a mechanical pump and a molecular pump to evacuate the deposition chamber to a vacuum of 5×10 -3Pa, after pre-sputtering, a transition layer TiAlCrNb and a surface anti-oxidation layer TiAlCrM are sequentially prepared on the substrate surface.

[0029] Preparation of TiAlCrNb transition layer: magnetron sputtering or multi-arc ion plating technology is used to deposit TiAlCrNb transition layer on the substrate surface with TiAlCrNb alloy target as target material. The process parameters include: deposition power: 100-250W, working gas pressure: 0.6-1.2Pa, target-substrate distance: 50-80mm, argon gas flow rate: 20-50sccm. The thickness of the TiAlCrNb transition layer is 5-20μm.

[0030] Preparation of the TiAlCrM coating on the surface: The TiAlCrM coating is prepared on the surface of the TiAlCrNb transition layer by magnetron sputtering or multi-arc ion plating technology. The process parameters include: deposition power: 100-250W, working gas pressure: 0.6-1.2Pa, target-substrate distance: 50-80mm, argon gas flow rate: 20-50sccm. The thickness of the TiAlCrM coating on the surface is 10-50μm.

[0031] Embodiment 1:

[0032] In this embodiment, a high temperature anti-oxidation coating on the surface of a TiAl alloy is prepared in the following steps:

[0033] 1. Target material preparation: The TiAlCrM coating is TiAlCrY (i.e., M is the Y element), and its specific composition is Ti-55Al-20Cr-0.4Y (at%) alloy target deposition; the TiAlCrNb transition layer is deposited using an alloy target with a composition of Ti-48Al-2Cr-2Nb (at%).

[0034] 2. Substrate pretreatment: Sand blasting method is used, the distance between the spray gun and the surface is 50mm, the sand blasting direction is 90° to the substrate surface, the sand blasting time is 5s, the sand blasting pressure is 0.4MPa, and the average surface roughness of the substrate after sand blasting is 0.54±0.03μm.

[0035] 3. Deposition coating

[0036] Close the furnace door, turn on the circulating cooling water, and use a vacuum unit consisting of a mechanical pump and a molecular pump to evacuate the sputtering chamber to a vacuum of 5×10 -3 Pa, after pre-sputtering, TiAlCrNb transition layer and coating are prepared in sequence on the substrate surface.

[0037] The magnetron sputtering technology is adopted, and a TiAlCrNb alloy target is used as a target material to deposit a TiAlCrNb transition layer on the surface of the substrate. A TiAlCrY alloy target is used as a target material to deposit a TiAlCrNb coating on the surface of the TiAlCrNb transition layer. The magnetron sputtering process parameters are shown in Table 1.

[0038] Table 1 Coating magnetron sputtering deposition process parameters

[0039] TiAlCrNb layer TiAlCrY layer Sputtering power, W 200 200 Working air pressure, Pa 1.2 1.0 Target-substrate distance, mm 60 60 Ar gas flow rate, sccm 20 20 Sedimentation time, h 4 6

[0040] Figure 1 This is the surface morphology of the TiAlCrY / TiAlCrNb double-layer coating prepared by this process. It can be found that the surface of the deposited coating is dense and shows an island-like growth mechanism.

[0041] Figure 2 This is the cross-sectional morphology of the TiAlCrY / TiAlCrNb double-layer coating prepared under this process. It can be found that the coating cross-section is dense, without defects such as holes, and the coating is columnar. The thickness of the TiAlCrY anti-oxidation layer is about 10μm, and the thickness of the TiAlCrNb transition layer is about 8μm.

[0042] The prepared samples were subjected to a 1000℃ water quenching thermal cycle test to assess their thermal ring shock resistance. The specific process is as follows: set the furnace temperature, put the prepared samples into the resistance furnace, keep the temperature for 10 minutes, then take them out and put them into deionized water at room temperature to cool for 5 minutes, take them out and put them into a 120℃ drying oven to dry the moisture on the surface of the samples, observe the degree of coating peeling on the surface of the samples, and then repeat the process. The surface morphology of the samples during the water quenching thermal shock process is shown in Figure 1. Figure 3 shown. Figure 3 It can be found that no coating shedding was found after 20 water quenching thermal cycles. When the water quenching thermal shock was 40 times, cracks began to appear on the coating at the edge of the substrate, and small areas of peeling occurred. When the thermal shock was 80 times, the number of cracks on the coating surface and the shedding area increased, but the shedding area did not exceed 20% of the total coating area, and the coating still had a certain protective ability.

[0043] The prepared samples were subjected to a cyclic oxidation experiment at 1000℃ in air using a muffle furnace to evaluate their cyclic oxidation performance. The specific parameters were: 1000℃ for 1h, room temperature for 10min for 1 cycle, and a total of 200 cycles. The samples after 50, 100, 150 and 200 cycles were taken to characterize the phase composition, microstructure and composition of the coating surface and cross section. The results are shown in Figure 2. Figure 4 shown. Figure 4In the test, after 50-200 cycles of air thermal cycle oxidation at 1000°C, a surface oxide film with a thickness of about 2-5μm was generated. The coating was well bonded to the substrate without peeling, no cracks or other defects were generated in the coating, and the diffusion of components was not obvious.

[0044] Comparative Example 1:

[0045] The coating was prepared according to the steps in Example 1, except that in Comparative Example 1, a TiAlCrY single-layer anti-oxidation layer was directly deposited on the surface of the substrate after sandblasting and roughening.

[0046] The prepared TiAlCrY single-layer coating sample was subjected to a cyclic oxidation test under air conditions at 1000°C. The experimental parameters were the same as those in Example 1. The experimental results are shown in FIG. Figure 5 It can be found that for the Ra0.5 sample, after 50-100 cycles of cyclic oxidation of the surface coating, a large amount of Al2O3 is generated at the interface between the coating and the substrate, and cracks are generated in the coating. After 150-200 cycles, a large amount of Al2O3 is generated in the cracked area of ​​the coating, and some areas are warped, and the coating peels off from the substrate at the warped area.

[0047] Comparative Example 2:

[0048] A TiAlCrY / TiAlCrNb double-layer coating was prepared according to the steps in Example 1, except that the sandblasting pretreatment process of the substrate in Comparative Example 1 was as follows: the distance between the spray gun and the surface was 50 mm, the sandblasting direction was at an angle of 90° to the substrate surface, the sandblasting time was 5 s, the sandblasting pressure was 0.28 MPa, and the average surface roughness of the substrate after sandblasting was 0.28±0.02 μm.

[0049] The prepared TiAlCrY / TiAlCrNb double-layer coating was subjected to a 1000°C water quenching thermal cycle experiment. The experimental parameters were the same as those in Example 1. The experimental results are shown in FIG. Figure 6 It can be found that cracks appeared at the edge of the sample when the water quenching heat cycle was 40 times, and no obvious peeling occurred. However, when the number of water quenching heat cycles reached 80 times, the coating peeled off in a large area, and the area of ​​the peeling area exceeded 20% of the total coating area.

[0050] Comparative Example 3:

[0051] A TiAlCrY / TiAlCrNb double-layer coating sample was prepared according to the steps for preparing the sample in Example 1, except that, in the pretreatment process of the substrate in Example 1, the distance between the spray gun and the surface was 50 mm, the sandblasting direction was at an angle of 90° to the substrate surface, the sandblasting time was 5 s, and the sandblasting pressure was 0.01 MPa; the average surface roughness of the substrate after sandblasting was 1.36±0.10 μm.

[0052] The prepared TiAlCrY / TiAlCrNb double-layer coating was subjected to a cyclic oxidation experiment under air conditions at 1000°C. The experimental parameters were the same as those in Example 1. The experimental results are shown in FIG. Figure 7 As shown. When the coating is oxidized by air thermal cycle for 50-100 cycles, multiple longitudinal cracks appear inside, a small amount of oxide is generated in the cracks and at the interface between the coating and the substrate, and the coating is slightly bent; after 150 cycles, the longitudinal cracks in the coating widen, the coating bends more, and part of the coating peels off from the substrate, generating wide transverse cracks between the substrate and the substrate, and oxides are generated at the interface.

[0053] Compared with Comparative Example 1, the TiAlCrY / TiAlCrNb double-layer coating in Example 1 is more tightly bonded to the substrate, almost no Al2O3 is generated at the coating-substrate interface, and the coating does not peel off or crack during the cyclic oxidation process.

[0054] Compared with Comparative Example 2, the TiAlCrY / TiAlCrNb double-layer coating in Example 1 did not peel off after 80 cycles of water quenching thermal cycling and still had good protection ability.

[0055] Compared with Comparative Example 3, the TiAlCrY / TiAlCrNb double-layer coating in Example 1 did not generate cracks during the water quenching thermal cycle, and almost no Al2O3 was generated at the coating-substrate interface.

Claims

1. A high temperature anti-oxidation coating on the surface of TiAl alloy, It is characterized in that The coating comprises a transition layer TiAlCrNb and an anti-oxidation layer TiAlCrM from the inside to the outside.

2. The high temperature oxidation resistant coating on the TiAl alloy surface as claimed in claim 1, It is characterized in that The main chemical components of the anti-oxidation layer TiAlCrM are: Ti 22-47at%, Al 45-55at%, Cr 10-27at%, M is a trace element with a content of less than 1at%, and the trace element is selected from at least one of Gd, Y and Hf.

3. The high temperature oxidation resistant coating on the TiAl alloy surface as claimed in claim 1, It is characterized in that The thickness of the anti-oxidation layer TiAlCrM is 10-50 μm.

4. The high temperature oxidation resistant coating on the TiAl alloy surface as claimed in claim 1, It is characterized in that The main chemical components of the transition layer TiAlCrNb are: Ti 20-40at%, Al 40-60at%, Cr 1-30at%, and Nb 1-8at%.

5. The high temperature oxidation resistant coating on the TiAl alloy surface as claimed in claim 1, It is characterized in that The thickness of the transition layer TiAlCrNb is 5-20 μm.

6. A method for preparing a high temperature anti-oxidation coating on a TiAl alloy surface as claimed in any one of claims 1 to 5, It is characterized in that The physical vapor deposition technology is used to prepare the transition layer TiAlCrNb on the surface of the TiAl alloy substrate, and then the anti-oxidation layer TiAlCrM is prepared on the surface of the transition layer TiAlCrNb.

7. The method according to claim 6, It is characterized in that The physical vapor deposition technology is magnetron sputtering or multi-arc ion plating.

8. The method according to claim 6, It is characterized in that The TiAl alloy surface was roughened by sandblasting before the coating was deposited, and the surface roughness Ra after roughening was 0.2~5.0.

Citation Information

Patent Citations

  • Oxidation-resistant coating and formation method thereof, thermal barrier coating, heat-resistant member, and gas turbine

    CA2576004A1

  • Aluminum / aluminum oxide diffusion blocking layer for titanium-aluminum alloy and preparation method thereof

    CN101310970A

  • TiAlCr anti-oxidation coating for TiAl alloy surface and preparation method of TiAlCr anti-oxidation coating

    CN113584416A

  • Double-layer anti-oxidation coating for TiAl alloy and preparation method of double-layer anti-oxidation coating

    CN114134371A

  • Thermal barrier coating for TiAl alloy and preparation method of thermal barrier coating