Diamond-core-shell metal composite catalyst, preparation method and electrolytic cell

Through the diamond-core-shell metal composite catalyst, the conductive diamond support and metal core are combined to form an iridium encapsulation layer, which solves the problems of high loading and poor stability of precious metal catalysts, and realizes low-cost large-scale application and high-efficiency electrolysis of PEM-WE Hydrogen production from water.

CN119020816APending Publication Date: 2024-11-26GUANGZHOU DEPOSON ELECTRIC TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310587363.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The high load of the noble metal iridium catalyst in the anode in the existing proton exchange membrane electrolytic cell (PEM-WE) results in high material cost and poor stability in a high acidic environment, making it difficult to achieve large-scale application.

Method used

The diamond-core-shell metal composite catalyst is used to coat metal cores such as iron, cobalt, nickel, titanium, manganese, etc. through conductive diamond as a support, and the diamond-core-shell structure is formed by ion sputtering to reduce the accumulation of iridium catalysts. density.

Benefits of technology

It significantly reduces the use of iridium metals, improves the utilization rate and stability of catalysts, realizes large-scale application of PEM-WE, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020816A_ABST
    Figure CN119020816A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a diamond-core-shell metal composite catalyst. The preparation method comprises the following steps: S1, providing diamond particles or conductive diamond particles as a carrier; s2, providing one or more metal elementary substances or alloys of iron, cobalt, nickel, titanium, manganese and copper as an inner core, and loading the metal inner core on the surface of the carrier to obtain a diamond-metal inner core complex; and S3, carrying out ion sputtering iridium plating on the diamond-metal core composite body, so that the metal or alloy core is coated with an iridium plating layer, and the diamond-core shell metal composite catalyst is formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of materials for producing hydrogen by electrolysis of water, and in particular to catalyst materials for proton exchange membrane electrolyzers. Background Art

[0002] As a medium for large-scale energy storage, hydrogen is considered to be one of the important energy storage materials in the future green energy society dominated by renewable energy. Proton exchange membrane electrolyzer (PEM-WE) is a perfect technology for promoting large-scale renewable energy to produce hydrogen by electrolysis of water with its high power density and excellent start-stop response. However, high material cost is still the main challenge for large-scale production of technology applications. The energy conversion component of the proton exchange membrane electrolyzer is the membrane electrode assembly (Membrane Electrode Assembly), in which the core energy conversion material is a catalyst layer composed of catalysts and proton exchange resins as the main substances. The high material cost that restricts large-scale application comes from the noble metal iridium catalyst at the anode, which has an extremely fast electrocatalytic activity for the oxygen evolution reaction of water oxidation at the anode. At present, the iridium catalyst loading at the anode exceeds the standard for sustainable and large-scale application of PEM-WE. In order to achieve a membrane electrode with low noble metal loading, it is necessary to significantly reduce the stacking density of the iridium catalyst and develop in the direction of fuel cell-loaded alloy catalysts. However, there are very few carriers that can work for a long time in harsh acidic high-potential environments. For the currently popular antimony-doped tin oxide (ATO) carrier, there are problems such as poor structure and metal leaching poisoning the proton exchange membrane, which causes the conductivity of the catalyst layer to decrease. Its stability is not as good as pure iridium oxide. For alloyed catalyst design, other metals except precious metals do not have considerable durability. Precious metals must be coated on the surface of other metals to form a core-shell structure to maintain the metal stability of the catalyst, so that PEM-WE can achieve large-scale application at a lower cost. Summary of the invention

[0003] Based on the above-mentioned problems, it is necessary to provide a diamond-core-shell metal composite catalyst and a preparation method thereof, as well as an electrolytic cell using the diamond-core-shell metal composite catalyst. Conductive diamond, as a corrosion-resistant electrode material, is very suitable for supporting anode catalysts. The use of such carrier technology can significantly reduce the use of precious metals without affecting the electrolysis efficiency, thereby reducing the cost of PEM-WE and realizing a solution for large-scale application.

[0004] A method for preparing a diamond-core-shell metal composite catalyst comprises the following steps:

[0005] S1:

[0006] providing diamond particles or conductive diamond particles as a carrier;

[0007] S2:

[0008] Providing one or more metal single substances or alloys of iron, cobalt, nickel, titanium, manganese, and copper as a core, and supporting the metal core on the surface of the carrier to obtain a diamond-metal core composite;

[0009] S3:

[0010] The diamond-metal core composite is ion sputtered to plate iridium, so that the iridium coating covers the metal core to form a diamond-core-shell metal composite catalyst.

[0011] In one embodiment, in step S3, the process of ion sputtering plating is: magnetron sputtering deposition, using an Ir target with a purity of 99.99%, a size of 50mm*10mm*0.5mm, a substrate bias of -50 to -100V, an operating pressure of 0.3 to 0.5Pa, a sputtering current of 6 to 10A, and an oxygen flow rate of 20 to 40sccm.

[0012] In one embodiment, the particle size of the metal core is 2-20 nm.

[0013] In one embodiment, the particle size of the metal core is 3-5 nm.

[0014] In one embodiment, the coating has a thickness ranging from 1 to 3.5 nm.

[0015] In one embodiment, the step S0 is further included:

[0016] Conductive diamond particles are obtained by hot wire chemical vapor deposition method, the parameters of which are: base temperature 500-800°C, hot wire temperature 180-2400°C, gas pressure 1-5kPa, hydrogen 100-1000sccm, methane 1-20sccm, borane 1-20sccm, and growth for more than 10 minutes.

[0017] In one embodiment, the step S0 is further included:

[0018] Conductive diamond particles are obtained by microwave plasma chemical vapor deposition, wherein the parameters of the microwave plasma chemical vapor deposition method are: microwave power 500-3000 watts, hydrogen 100-1000sccm, methane 1-20sccm, borane 1-10sccm, base temperature 500-700°C, gas pressure 4-6kPa, and growth time 3-10h.

[0019] A diamond-core-shell metal composite catalyst is prepared using any of the above-mentioned methods for preparing the diamond-core-shell metal composite catalyst.

[0020] A diamond-core-shell metal composite catalyst, comprising a carrier and an active material;

[0021] The carrier is conductive diamond loaded with particles of one or more metal elements or alloys of iron, cobalt, nickel, titanium, manganese and copper;

[0022] The active material is iridium oxide;

[0023] The active material wraps the surface of the carrier to form a diamond-core-shell metal composite catalyst.

[0024] An electrolytic cell comprises an anode and a cathode, wherein the catalyst layer of the anode and / or the cathode uses any one of the diamond-core-shell metal composite catalysts described above.

[0025] The beneficial effects of the present invention are:

[0026] 1. The present invention provides a highly active diamond-core-shell metal composite catalyst, which can significantly reduce the packing density of the iridium metal in the anode catalyst layer, and at the same time can achieve the same performance as the existing commercially available high-load iridium oxide catalyst, thereby effectively improving the utilization rate of the iridium catalyst, reducing the catalyst cost, and realizing the large-scale application of PEM-WE.

[0027] 2. Diamond is corrosion-resistant and oxidation-resistant, and has a long service life as a carrier. In addition, the metal core is loaded on the surface of the diamond to form a diamond-metal core complex, and an iridium coating structure is formed on the surface of the diamond-metal core complex, so that the base metal is completely encapsulated by the precious metal, which can protect the base metal from dissolution. Compared with pure precious metal nanoparticles, it has a higher precious metal crystal face atomic ratio, higher activity, and excellent stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0029] Figure 1 The present invention is a flow chart of Example 1 of the method for preparing the catalyst of the present invention.

[0030] Figure 2 Schematic diagram of the structure of a diamond-core-shell metal composite catalyst according to an embodiment of the present invention.

[0031] Figure 3 This is a TEM electron microscope photograph of a conductive diamond-loaded inner core metal manganese structure in one embodiment of the present invention.

[0032] Figure 4 This is a TEM electron microscope photograph of a conductive diamond-loaded inner core metal titanium structure in one embodiment of the present invention.

[0033] Figure 5 The polarization curves of the electrolytic cells using the diamond-core-shell metal composite catalyst of the present invention and the commercially available iridium oxide catalyst are shown in FIG.

[0034] Figure 6 AST accelerated durability test procedure designed for the present invention.

[0035] Figure 7 For Figure 6 The voltage variation diagram of the electrolytic cell using the diamond-core-shell metal composite catalyst of the present invention and the commercially available iridium oxide catalyst in the 300hAST test is shown. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The present invention provides a diamond-core-shell metal composite catalyst for hydrogen production by electrolysis of water, which is prepared by the preparation method of the diamond-core-shell metal composite catalyst provided by the present invention. In one embodiment, Figure 1 As shown, a method for preparing a diamond-core-shell metal composite catalyst comprises the following steps:

[0038] The steps include:

[0039] Step S1:

[0040] Non-conductive diamond particles or conductive diamond particles are provided as a carrier.

[0041] Wherein, the diamond / conductive diamond particles can be obtained from the market or prepared by themselves, for example, non-conductive diamond particles can be obtained by explosion method, for example, conductive diamond can be obtained by chemical vapor deposition method, for example, in one embodiment, step S0 is also included, the step S0: obtaining conductive diamond particles by hot wire chemical vapor deposition method. Specifically, the parameters of the hot wire chemical vapor deposition method are: base temperature 500-800°C, hot wire temperature 180-2400°C, gas pressure 1-5kPa, hydrogen 100-1000sccm, methane 1-20sccm, borane 1-20sccm, growth for more than 10min. For example, in another embodiment, step S0: obtaining conductive diamond particles by microwave plasma chemical vapor deposition method. Specifically, the parameters of the microwave plasma chemical vapor deposition method are: microwave power 500-3000 watts, hydrogen 100-1000 sccm, methane 1-20 sccm, borane 1-10 sccm, base temperature 500-700°C, gas pressure 4-6 kPa, and growth time 3-10 hours.

[0042] The conductive diamond can also be prepared by other methods, for example, by using a high temperature and high pressure method, under high temperature and high pressure (above 500°C, exceeding 10GPa), the catalyst / graphite / boron source is used to obtain conductive diamond particles through an oil hydraulic machine, and then the conductive diamond particles are broken up by physical means.

[0043] S2:

[0044] One or more metal single substances or alloys selected from iron, cobalt, nickel, titanium, manganese, and copper are provided as cores, and the metal cores are supported on the surface of the conductive diamond to obtain a diamond-metal core composite. That is, one or more metal single substances or alloys selected from iron, cobalt, nickel, titanium, manganese, and copper are supported on the surface of the conductive diamond to obtain a diamond-metal core composite.

[0045] For example, a manganese alloy is provided as a metal core and supported on the surface of a conductive diamond to obtain a diamond-metal core composite. For example, a titanium alloy is provided as a metal core and supported on the surface of a conductive diamond to obtain a diamond-metal core composite. For example, an iron alloy is provided as a metal core and supported on the surface of a conductive diamond to obtain a diamond-metal core composite. This embodiment is not described in detail. Among them, the material of the metal core can use commercially available pure metal nanoparticles, or use a common reducing agent (such as NaBH4, hydrazine hydrate, etc.) to reduce the salt corresponding to the metal (such as cobalt nitrate, cobalt chloride, etc.)

[0046] S3:

[0047] The diamond-metal core composite is ion sputtered to plate iridium, so that the iridium coating covers the metal core to form a diamond-core-shell metal composite catalyst.

[0048] In this step, iridium as an active material is formed on the surface of the diamond-metal core composite, especially on the surface of the metal core, by ion sputtering coating, thereby forming a coating layer to obtain a diamond-core-shell metal composite catalyst.

[0049] That is, the diamond-core-shell metal composite catalyst prepared by the above method has a structure including a carrier and an active material, the carrier is conductive diamond loaded with particles of one or more metal elements or alloys of iron, cobalt, nickel, titanium, manganese, and copper, the active material is iridium oxide, and the active material wraps the surface of the carrier to form a diamond-core-shell metal composite catalyst.

[0050] In one embodiment, the ion sputtering plating process of step S3 is: magnetron sputtering deposition, using an Ir target with a purity of 99.99%, a size of 50mm*10mm*0.5mm, a substrate bias of -50 to -100V, an operating pressure of 0.3 to 0.5Pa, a sputtering current of 6 to 10A, and an oxygen flow rate of 20 to 40sccm.

[0051] For example, in a preferred embodiment, the particle size of the metal core is 2-20 nm, and more preferably, the particle size of the metal core is 3-5 nm.

[0052] For example, in a preferred embodiment, the thickness of the coating layer is in the range of 1-3.5 nm.

[0053] The present invention provides an electrolytic cell, comprising an anode and a cathode, wherein the catalyst layer of the anode and / or the cathode uses the diamond-core-shell metal composite catalyst described above.

[0054] Embodiment 1:

[0055] The electrolytic cell using the diamond-core-shell metal composite catalyst of the present invention has an iridium loading of 0.15 mg Ir / cm 2 .

[0056] Example 2

[0057] The electrolytic cell of the diamond-core-shell metal composite catalyst of the present invention used has an iridium loading of 0.2 mg. Ir / cm 2 .

[0058] Comparative Example

[0059] The electrolyzer used a commercially available iridium oxide catalyst with an iridium loading of 2.3 mg Ir / cm 2 .

[0060] like Figure 5 As shown, it is a polarization curve diagram of Example 1, Example 2 and Comparative Example of the present invention. It can be seen that the catalyst of the present invention can maintain performance comparable to that of commercially available iridium oxide with high loading when using extremely low loading iridium in the electrolytic cell.

[0061] like Figure 6 As shown in FIG. 1 , it is the AST accelerated durability test procedure designed by the present invention, wherein the constant current density is set at 0.3 A / cm in stage A. 2 In stage B, the constant current density is set to 2A / cm 2 , with AB lasting 15 minutes each, forming a 30-minute cycle, for a total of 300 hours.

[0062] Figure 7 For Example 1, Example 2 and Comparative Example of the present invention Figure 6 The voltage change diagram of the 300h AST test is shown in the following table. The voltage change diagram of Example 1, Example 2 and the comparative example after AST test for 300h is 1.85A / cm 2 Percentage of voltage maintenance rate under current density. It can be seen from the data that after 300h of AST test, the voltage maintenance rate of the electrolytic cell embodiments using the diamond-core-shell metal composite catalyst of the present invention is higher than that of the comparative example, indicating that the stability of the electrolytic cell using the low-loaded catalyst of the present invention is better than that of the electrolytic cell using the high-loaded commercial pure iridium oxide.

[0063]

[0064] AST Durability Comparison Example 1 Example 2 Comparative Example Voltage maintenance rate percentage 90.7% 91.9% 86.5%

[0065] Table 1

[0066] The beneficial effects of the present invention are:

[0067] 1. The present invention provides a highly active diamond-core-shell metal composite catalyst, which can significantly reduce the packing density of the iridium metal in the anode catalyst layer, and at the same time can achieve the same performance as the existing commercially available high-load iridium oxide catalyst, thereby effectively improving the utilization rate of the iridium catalyst, reducing the catalyst cost, and realizing the large-scale application of PEM-WE.

[0068] 2. Diamond is corrosion-resistant and oxidation-resistant, and has a long service life as a carrier. In addition, the metal core is loaded on the surface of the diamond to form a diamond-metal core complex, and an iridium coating structure is formed on the surface of the diamond-metal core complex, so that the base metal is completely encapsulated by the precious metal, which can protect the base metal from dissolution. Compared with pure precious metal nanoparticles, it has a higher precious metal crystal face atomic ratio, higher activity, and excellent stability.

[0069] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0070] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a diamond-core-shell metal composite catalyst, characterized in that: The steps include: S1: providing diamond particles or conductive diamond particles as a carrier; S2: Providing one or more metal single substances or alloys of iron, cobalt, nickel, titanium, manganese, and copper as a core, and supporting the metal core on the surface of the carrier to obtain a diamond-metal core composite; S3: The diamond-metal core composite is ion sputtered to plate iridium, so that the iridium coating covers the metal core to form a diamond-core-shell metal composite catalyst.

2. The method for preparing the diamond-core-shell metal composite catalyst according to claim 1, characterized in that: In step S3, the process of ion sputtering plating is: magnetron sputtering deposition, using an Ir target with a purity of 99.99%, a size of 50mm*10mm*0.5mm, a substrate bias of -50 to -100V, a working pressure of 0.3 to 0.5Pa, a sputtering current of 6 to 10A, and an oxygen flow rate of 20 to 40sccm.

3. The method for preparing the diamond-core-shell metal composite catalyst according to claim 1, characterized in that: The particle size of the metal core is 2-20 nm.

4. The method for preparing the diamond-core-shell metal composite catalyst according to claim 1, characterized in that: The particle size of the metal core is 3-5 nm.

5. The method for preparing the diamond-core-shell metal composite catalyst according to claim 1, characterized in that: The thickness of the coating is in the range of 1-3.5 nm.

6. The method for preparing the diamond-core-shell metal composite catalyst according to claim 1, characterized in that: It also includes step S0: Conductive diamond particles are obtained by hot wire chemical vapor deposition method, the parameters of which are: base temperature 500-800°C, hot wire temperature 180-2400°C, gas pressure 1-5kPa, hydrogen 100-1000sccm, methane 1-20sccm, borane 1-20sccm, and growth for more than 10 minutes.

7. The method for preparing the diamond-core-shell metal composite catalyst according to claim 1, characterized in that: It also includes step S0: Conductive diamond particles are obtained by microwave plasma chemical vapor deposition, wherein the parameters of the microwave plasma chemical vapor deposition method are: microwave power 500-3000 watts, hydrogen 100-1000sccm, methane 1-20sccm, borane 1-10sccm, base temperature 500-700°C, gas pressure 4-6kPa, and growth time 3-10h.

8. A diamond-core-shell metal composite catalyst, characterized in that: The catalyst is prepared by the method for preparing the diamond-core-shell metal composite catalyst according to any one of claims 1 to 10.

9. A diamond-core-shell metal composite catalyst, characterized in that: including a carrier and an active material; The carrier is conductive diamond loaded with particles of one or more metal elements or alloys of iron, cobalt, nickel, titanium, manganese and copper; The active material is iridium oxide; The active material wraps the surface of the carrier to form a diamond-core-shell metal composite catalyst.

10. An electrolytic cell, characterized in that: The invention comprises an anode and a cathode, wherein the catalyst layer of the anode and / or the cathode uses the diamond-core-shell metal composite catalyst according to any one of claims 1 to 9.

Citation Information

Cited By

  • Molybdenum-doped iridium-based multicomponent alloy core-shell structure PEM water electrolysis catalyst and preparation method thereof

    CN119776899A