Photocurable resin composition, application thereof, and photosensitive dry film resist laminate
By optimizing the molecular structure of the photocuring resin composition, the wet pressure analysis and adhesion performance of photosensitive dry film resist on flexible circuit boards is solved, and rapid film removal and excellent cover hole properties are achieved, which is suitable for a variety of productions The process improves production efficiency and product yield.
Patent Information
- Application Number
- CN202411177804.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The existing photosensitive dry film resist is difficult to take into account the good wet pressure analysis, adhesion performance, wet pressure gland hole performance and flexibility on flexible circuit boards, and the film removal speed is slow and easy to remain, making it difficult to be suitable for wet filming technology and Soft plate roll-to-roll continuous production process.
Provided is a photocuring resin composition, including alkali-soluble resin, photopolymerized monomer, photosensitizer and additives, by optimizing molecular structure, introducing specific functional groups, and improving its reaction rate and adhesion properties in alkaline aqueous solutions. , suitable for continuous production processes of wet film and soft plate roll-to-roll.
It realizes rapid film removal, residue-free, excellent cover hole properties and adhesion properties of photosensitive dry film resist, and is suitable for the production of precision line flexible boards and rigid boards, improves product yield and production efficiency, and reduces production costs. .
Smart Images

Figure CN119024642A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photocurable resins, and in particular to a photocurable resin composition, application thereof and a photosensitive dry film resist laminate. Background Art
[0002] Photosensitive dry film resists are widely used as key materials for pattern transfer in printed circuit boards, lead frames, solar cells, conductor packages, BGA (Ball Grid Array), and CPS (Chip Size Package) packages. For example, when manufacturing printed circuit boards, first, the photosensitive dry film resist stacked on a substrate such as a copper-clad laminate and a flexible substrate is pattern exposed. The exposed portion of the photosensitive dry film resist is polymerized and cured. Next, the unexposed portion is removed with a developer to form a resist pattern on the substrate. Furthermore, after etching or plating is performed to form a conductor pattern, the resist pattern is peeled off and removed from the substrate. Through these processes, a conductor pattern is formed on the substrate.
[0003] When using photolithography to manufacture printed circuit boards, substrates with various shapes are used according to the wiring and product characteristics of the terminal product, such as flat, concave and convex, non-flat, rigid substrates with large through holes (6mm round holes or special-shaped holes), and flexible substrates with dense small-diameter through holes (100-200μm).
[0004] In recent years, as electronic products have become increasingly thinner and smaller, the wiring accuracy of printed circuit boards and the interconnection accuracy of electronic components have become increasingly higher. Flexible circuit boards (FPCs for short) have the advantages of high wiring density, light weight, thin thickness, less wiring space restrictions, and high flexibility. They fully meet the development trend of thinner and smaller electronic products, can meet the needs of miniaturization and mobility of electronic products, and are widely used in PCs and peripheral products, automotive electronics, medical devices, communication products, consumer electronics and other fields.
[0005] Flexible substrates used to make flexible circuit boards usually include dense small-diameter through holes, especially for flexible circuit boards with precision circuits. The number of through holes used to connect wiring layers is increased, and the aperture is further reduced to about 100μm. On the other hand, the copper layer on the flexible substrate is thin, the surface roughness of the copper layer is low, and it also contains an anti-oxidation layer. Generally, no pre-treatment operations such as grinding are performed before lamination with dry film resist. Therefore, in order to improve the adhesion of photosensitive dry film resist on flexible substrates and thus improve the product qualification rate, wet lamination method is usually used to make flexible circuit boards. The so-called wet lamination refers to coating a layer of water film on the surface of the copper foil of the substrate before lamination. When the substrate passes through the hot pressing roller, part of the water is evaporated and removed, and the remaining water will be absorbed by the photosensitive dry film resist, thus forming a vacuum on the original irregular or concave surface. At the same time, the water-soluble characteristics of the dry film are used to make the film surface partly in liquid form, thereby improving the fluidity when the film is pressed, so that the dry film and the copper surface can fit firmly. In addition, a small amount of water can significantly improve the adhesion between the photosensitive dry film and PET, preventing the abnormal situation that the photosensitive dry film accidentally collapses due to factors such as collision after exposure.
[0006] The photosensitive dry film resist used to make flexible circuit boards needs to have good flexibility. After wet lamination, the dry film resist with good flexibility can easily penetrate into the small holes of the flexible substrate. For the photosensitive dry film used in the wet pressing process of the flexible substrate, the inventor found the following actual situation and technical difficulties during the experiment: after the resist is stripped, sometimes the small hole curing resist is not completely stripped, but remains in some small-diameter through holes, especially for flexible circuit boards with precision circuits, whose circuit size is small and the through hole size is small, therefore, higher requirements are put forward for the analytical adhesion performance of the photosensitive dry film resist. However, when the adhesion performance of the photosensitive dry film resist is excellent, the corresponding film removal is difficult (i.e., difficult to strip), and it is particularly difficult to remove the curing resist that has penetrated into the small hole and completely remove it without residue. When the small through hole of the flexible substrate cannot be completely stripped clean (hole plugging phenomenon), it will seriously affect the manufacturing yield of the client's flexible circuit board, and even cause the electrical performance of the obtained flexible circuit board to be unqualified and scrapped.
[0007] At present, researchers have found that by introducing long-chain alkyl (meth)acrylates into the alkali-soluble resin of the dry film resist or introducing a certain amount of photopolymerizable monomers containing propylene oxide block copolymers as disclosed in the existing document (publication number CN108490737A), the film stripping speed can be significantly improved and the problem of incomplete film stripping (hole plugging) in the small holes of the flexible substrate can be improved. However, experimental results show that after the introduction of long-chain alkyl (meth)acrylates, the adhesion performance of the dry film resist on the substrate is significantly reduced, which is not conducive to the production of fine circuits, and the film stripping fragments are significantly larger.
[0008] The development trend of flexible circuit boards today is that their circuits are becoming more and more sophisticated, and a considerable number of flexible circuit board manufacturers with precise circuits use a roll-to-roll continuous production process for flexible circuits in order to improve production efficiency and yield. This type of roll-to-roll continuous production process not only requires fast film removal time, clean film removal of the cured resist in the small holes, and no residue (no plugging phenomenon), but also requires the size of the film removal sheet on the entire board to be very small. This is because if the size of the film removal sheet is too large, the large-size film removal sheet will frequently wrap around the roller, which will seriously affect the production efficiency of the production line.
[0009] In addition, there are also a number of rigid circuit board manufacturers with precision circuits that use wet lamination technology to make circuit boards. Their rigid substrates generally have many large through holes (4-6mm round holes or special-shaped holes). Such substrates and process conditions require dry film resists to have good wet pressure analysis, adhesion performance, and excellent wet pressure hole covering performance and flexibility. For photosensitive dry film resist manufacturers, if each formulation of photosensitive dry film resist products can take into account multiple key performance aspects and meet the production requirements of downstream flexible or rigid circuit board manufacturers with different production processes, it can greatly improve the production efficiency and slitting yield of photosensitive dry film resists and reduce production costs.
[0010] On this basis, it is of great significance to research and develop a photocurable resin composition with good wet pressing analysis and adhesion performance, fast film removal speed, easy and clean film removal of the cured anti-corrosion agent in the small holes, no residue at all (no hole plugging phenomenon), small film removal sheet size, and suitable for flexible board roll-to-roll continuous production process, as well as excellent wet pressing hole covering performance and flexibility.
[0011] Therefore, it is an urgent and practical research topic to optimize the core components of the photosensitive dry film resist for the wet lamination process and obtain a photosensitive dry film resist with excellent comprehensive performance that can meet the key performance requirements required for the production of flexible circuit boards with precision circuits and rigid circuit boards with precision circuits. Summary of the invention
[0012] The main purpose of the present invention is to provide a photocurable resin composition, its application and a photosensitive dry film resist laminate, so as to solve the problem that the existing photosensitive dry film resist in the prior art is difficult to have good wet pressure analysis, adhesion performance, wet pressure hole covering performance and flexibility, and has a slow film removal speed, is easy to leave residue, and is difficult to be applied to wet film lamination process and flexible board roll-to-roll continuous production process.
[0013] In order to achieve the above object, the present invention provides a photocurable resin composition, which comprises: an alkali-soluble resin, a photopolymerizable monomer, a photosensitizer and an additive; the alkali-soluble resin comprises compounds represented by general formula (I) and general formula (II):
[0014]
[0015] Among them, R 1 and R 2 are independently selected from H or C 1 ~C 4 Alkyl; R 3 Selected from C 1 ~C 18 Substituted or unsubstituted straight chain alkyl or branched chain alkyl, C 7 ~C 14 Aryl-substituted alkyl, C 5 ~C 14 Alkyl substituted or unsubstituted cycloalkyl, hydroxy substituted C 1 ~C 18 A straight chain alkyl or branched chain alkyl, or C 1 ~C 4 An amino group substituted with a straight-chain alkyl group or a branched-chain alkyl group; R 4 Selected from H, C 1 ~C 3 Alkyl, C 1 ~C 3 an alkoxy group, an amino group or a halogen atom, and z 1 R in the corresponding segment 4 The number of substitutions is any integer from 0 to 5; 4 'Selected from H or C 1 ~C 4 Alkyl; in terms of percentage of the molecular weight of the compound represented by the general formula (I), x 1 The content of the corresponding segment is 27-40wt%, y 1 The content of the corresponding segment is 20-73wt%, z 1 The content of the corresponding segment is 0 to 40 wt%;
[0016]
[0017] Among them, R 5 , R 6 , R 8 are independently selected from H or C 1 ~C 4 Alkyl; R 7 Selected from C 1 ~C 18 Substituted or unsubstituted straight chain alkyl or branched chain alkyl, C 7 ~C 14 Aryl-substituted alkyl, C 5 ~C 14 Alkyl substituted or unsubstituted cycloalkyl, hydroxy substituted C 1 ~C 18A straight chain alkyl group or a branched chain alkyl group; R 9 One selected from the following groups:
[0018]
[0019] R 10 Selected from C 2 ~C 10 A straight chain alkylene or branched chain alkylene, n is any integer from 2 to 5; in terms of percentage of the molecular weight of the compound represented by the general formula (II), x 2 The content of the corresponding segment is 22-27 wt%, y 2 The content of the corresponding segment is 21-65wt%, z 2 The content of the corresponding segment is 10 to 50 wt%.
[0020] In order to achieve the above-mentioned purpose, another aspect of the present invention further provides an application of the above-mentioned photocurable resin composition provided by the present application in the field of photocuring.
[0021] Another aspect of the present invention provides a photosensitive dry film resist laminate, which includes a support layer and a resist layer, and the resist layer is prepared from the above-mentioned photocurable resin composition provided in the present application.
[0022] Using the technical solution of the present invention, in the compound represented by the general formula (II) of the present application, z 2 The corresponding chain segments contain amide groups and ester groups, which can improve their flexibility. The photocurable composition containing the alkali-soluble resin has excellent pore-covering properties, thereby improving the yield of the product. At the same time, the compound represented by the general formula (II) is 2 The corresponding chain segment also contains hydroxyl groups. According to the principle of "like dissolves like", the introduction of polar groups in the alkali-soluble resin can significantly increase the reaction rate of the photocurable resin composition in the alkaline aqueous solution, thereby shortening the time for the film stripping sheet to be peeled off from the surface of the copper substrate. Moreover, the introduction of polar groups can also increase the sites for reaction with water, thereby achieving the effect of reducing the film stripping size. The anti-corrosion agent prepared by the photocurable composition containing the alkali-soluble resin is suitable for the roll-to-roll continuous production process of flexible boards, and can inhibit the film from wrapping around the roller. In addition, the introduction of polar groups in the alkali-soluble resin can also enhance the bonding force between the photocurable resin composition and the copper substrate or PET substrate, and improve the adhesion performance of the photocurable resin composition, thereby cleverly solving the contradiction between the film stripping performance (no pore plugging phenomenon) and the adhesion performance. Compared with other ranges, the x in the compound represented by the general formula (II) is 2 ,y 2 and z 2Limiting them respectively within the above ranges is beneficial to improving the flexibility, thereby improving the hole covering property of the resist and improving the yield rate of the product.
[0023] In the compound represented by the general formula (I) of the present application, x 1 The content of the corresponding chain segment is relatively high, which can improve the film stripping time and the size of the film stripping fragments, thereby significantly improving the plugging phenomenon of the resist prepared by the photocurable composition containing the alkali-soluble resin. 1 Corresponding chain segments and z 1 The content of the corresponding chain segment is relatively high, which can significantly improve the wet pressure analysis ability of the photocurable resin composition and its adhesion on the surface of the copper substrate, especially the adhesion performance on the surface of a flexible substrate with low roughness.
[0024] The alkali-soluble resin in the present application includes compounds represented by general formula (I) and general formula (II). The combination of the two can exert their synergistic effect. The present application optimizes the molecular structure and introduces the above-mentioned specific functional groups to significantly improve the various properties of the photocurable resin composition, making it suitable for wet film lamination process and flexible board roll-to-roll continuous production process, while taking into account the production needs of precision circuit flexible boards and rigid boards, and can improve product yield, and can significantly improve the production efficiency of ITO and other components in the fields of PCB manufacturing, lead frame manufacturing, semiconductor packaging, and flat panel displays, thereby reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0026] Figure 1 A schematic diagram of a sample of a substrate for evaluating wet-pressed hole-capping performance used in this application is shown. DETAILED DESCRIPTION
[0027] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0028] As described in the background technology, the existing photosensitive dry film resist has the problems of good wet pressure analysis, adhesion performance, wet pressure hole covering performance and flexibility, slow film removal speed, easy residue, and difficult to be applied to wet film lamination process and flexible board roll-to-roll continuous production process. In order to solve the above technical problems, the present application provides a photocurable resin composition, which includes: an alkali-soluble resin, a photopolymerizable monomer, a photosensitizer and an additive; the alkali-soluble resin includes compounds represented by general formula (I) and general formula (II):
[0029]
[0030] Among them, R 1 and R 2 are independently selected from H or C 1 ~C 4 Alkyl; R 3 Selected from C 1 ~C 18 Substituted or unsubstituted straight chain alkyl or branched chain alkyl, C 7 ~C 14 Aryl-substituted alkyl, C 5 ~C 14. Alkyl substituted or unsubstituted cycloalkyl, hydroxy substituted C 1 ~C 18 A straight chain alkyl or branched chain alkyl, or C 1 ~C 4 An amino group substituted with a straight-chain alkyl group or a branched-chain alkyl group; R 4 Selected from H, C 1 ~C 3 Alkyl, C 1 ~C 3 an alkoxy group, an amino group or a halogen atom, and z 1 R in the corresponding segment 4 The number of substitutions is any integer from 0 to 5; 4 'Selected from H or C 1 ~C 4 Alkyl; in terms of percentage of the molecular weight of the compound represented by the general formula (I), x 1 The content of the corresponding segment is 27-40wt%, y 1 The content of the corresponding segment is 20-73wt%, z 1 The content of the corresponding segment is 0 to 40 wt%;
[0031]
[0032] Among them, R 5 , R 6 , R 8 are independently selected from H or C 1 ~C 4 Alkyl; R 7 Selected from C 1 ~C 18 Substituted or unsubstituted straight chain alkyl or branched chain alkyl, C 7 ~C 14 Aryl-substituted alkyl, C 5 ~C 14 Alkyl substituted or unsubstituted cycloalkyl, hydroxy substituted C 1 ~C 18 A straight chain alkyl group or a branched chain alkyl group; R9 One selected from the following groups:
[0033]
[0034] R 10 Selected from C 2 ~C 10 A straight chain alkylene or branched chain alkylene, n is any integer from 2 to 5; in terms of percentage of the molecular weight of the compound represented by the general formula (II), x 2 The content of the corresponding segment is 22-27 wt%, y 2 The content of the corresponding segment is 21-65wt%, z 2 The content of the corresponding segment is 10 to 50 wt%.
[0035] In the compound represented by the general formula (II) of the present application, z 2 The corresponding chain segments contain amide groups and ester groups, which can improve their flexibility. The photocurable composition containing the alkali-soluble resin has excellent pore-covering properties, thereby improving the yield of the product. At the same time, the compound represented by the general formula (II) is 2 The corresponding chain segment also contains hydroxyl groups. According to the principle of "like dissolves like", the introduction of polar groups in the alkali-soluble resin can significantly increase the reaction rate of the photocurable resin composition in the alkaline aqueous solution, thereby shortening the time for the film stripping sheet to be peeled off from the surface of the copper substrate. Moreover, the introduction of polar groups can also increase the sites for reaction with water, thereby achieving the effect of reducing the film stripping size. The anti-corrosion agent prepared by the photocurable composition containing the alkali-soluble resin is suitable for the roll-to-roll continuous production process of flexible boards, and can inhibit the film from wrapping around the roller. In addition, the introduction of polar groups in the alkali-soluble resin can also enhance the bonding force between the photocurable resin composition and the copper substrate or PET substrate, and improve the adhesion performance of the photocurable resin composition, thereby cleverly solving the contradiction between the film stripping performance (no pore plugging phenomenon) and the adhesion performance. Compared with other ranges, the x in the compound represented by the general formula (II) is 2 ,y 2 and z 2 Limiting them respectively within the above ranges is beneficial to improving the flexibility, thereby improving the hole covering property of the resist and improving the yield rate of the product.
[0036] In the compound represented by the general formula (I) of the present application, x 1 The content of the corresponding chain segment is relatively high, which can improve the film stripping time and the size of the film stripping fragments, thereby significantly improving the plugging phenomenon of the resist prepared by the photocurable composition containing the alkali-soluble resin. 1 Corresponding chain segments and z 1The content of the corresponding chain segment is relatively high, which can significantly improve the wet pressure analysis ability of the photocurable resin composition and its adhesion on the surface of the copper substrate, especially the adhesion performance on the surface of a flexible substrate with low roughness.
[0037] The alkali-soluble resin in the present application includes compounds represented by general formula (I) and general formula (II). The combination of the two can exert their synergistic effect. The present application optimizes the molecular structure and introduces the above-mentioned specific functional groups to significantly improve the various properties of the photocurable resin composition, making it suitable for wet film lamination process and flexible board roll-to-roll continuous production process, while taking into account the production needs of precision circuit flexible boards and rigid boards, and can improve product yield, and can significantly improve the production efficiency of ITO and other components in the fields of PCB manufacturing, lead frame manufacturing, semiconductor packaging, and flat panel displays, thereby reducing production costs.
[0038] In a preferred embodiment, the weight ratio of the compound represented by the general formula (I) to the compound represented by the general formula (II) is (15-35):(15-40). Compared with other ranges, limiting the weight ratio of the compound represented by the general formula (I) to the compound represented by the general formula (II) within the above range is conducive to exerting the synergistic effect of the two, and is conducive to improving the flexibility of the alkali-soluble resin, thereby improving the pore-capping property of the photocurable resin composition, and is also conducive to increasing the reaction rate of the photocurable resin composition in an alkaline aqueous solution, shortening the time for the film stripping sheet to be peeled off from the surface of the copper substrate; at the same time, it is also conducive to reducing the film stripping size, improving the bonding force between the photocurable resin composition and the copper substrate, and facilitating its application in the roll-to-roll continuous production process of flexible boards.
[0039] In order to further shorten the film removal time, further reduce the size of the film removal fragments, and at the same time to further improve the plugging phenomenon of small holes, further reduce the residue of the photocurable resin composition, and further improve the toughness of the alkali-soluble resin and the wet pressing pore-capping ability of the photocurable resin composition, preferably, the acid value of the compound represented by general formula (I) is 210-310 mgKOH / g.
[0040] In order to further shorten the development time and the film stripping time, and further improve the flexibility of the alkali-soluble resin and the pore-capping and filling properties of the photocurable resin composition, preferably, the acid value of the compound represented by the general formula (II) is 170 to 210 mgKOH / g.
[0041] In a preferred embodiment, in the compound represented by general formula (I), R 1 Including but not limited to H or methyl, R 2 Including but not limited to H or methyl, R 3 Including but not limited to methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, isooctyl, C 12 Straight chain alkyl, C 18Straight chain alkyl, benzyl, epoxypropyl substituted methylene, hydroxyethyl, hydroxypropyl, hydroxybutyl, -N(CH 3 ) 2 , or -N(C 2 H 5 ) 2 , R 4 Including but not limited to H or methyl, and z 1 R in the corresponding segment 4 The number of substitutions is 0 or 1, R 4 'Including but not limited to H or methyl. Using the above types of R 1 , R 2 , R 3 , R 4 The group is beneficial to further shorten the film removal time, further reduce the size of the film removal fragments, and at the same time is beneficial to further improve the plugging phenomenon of small holes, further reduce the residue of the photocurable resin composition, and further improve the comprehensive properties of the photocurable resin composition such as wet pressure analysis ability and pore covering property.
[0042] In a preferred embodiment, in the compound represented by general formula (II), R 5 , R 6 , R 8 Each independently includes but is not limited to H or methyl, R 7 Including but not limited to methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, isooctyl, C 12 Straight chain alkyl, C 18 A straight-chain alkyl group, a benzyl group, a glycidyl-substituted methylene group, a hydroxyethyl group, a hydroxypropyl group, or a hydroxybutyl group, R 10 Including but not limited to ethylene, propylene or decylene. 5 , R 6 , R 7 , R 8 and R 10 The group is beneficial to improving the flexibility of the alkali-soluble resin, and is beneficial to the comprehensive properties of the photocurable resin, such as wet pressure analysis ability and pore covering property.
[0043] In a preferred embodiment, the weight average molecular weight of the compound represented by general formula (I) is 30,000 to 80,000, and the molecular weight distribution index is 1.3 to 2.5. The weight average molecular weight and molecular weight distribution index of the compound represented by general formula (I) include but are not limited to the above ranges, and limiting them within the above ranges is conducive to improving the film-forming properties of the photocurable resin composition, and is convenient for wet film lamination process and roll-to-roll continuous production process.
[0044] In order to reduce the occurrence of plugging and gel flow, preferably, the polymerization conversion rate of the compound represented by general formula (I) is ≥97%.
[0045] In a preferred embodiment, the weight average molecular weight of the compound represented by general formula (II) is 60,000 to 90,000, and the molecular weight distribution index is 1.3 to 2.5. The weight average molecular weight and molecular weight distribution index of the compound represented by general formula (II) include but are not limited to the above ranges, and limiting it within the above ranges is beneficial to improving the resolution of the photocurable resin composition, improving its hole covering performance and wet pressure analysis performance, and is beneficial to reducing the size of the film stripping sheet, which is convenient for roll-to-roll continuous production process.
[0046] In order to reduce the occurrence of plugging and gel flow, preferably, the polymerization conversion rate of the compound represented by general formula (II) is ≥97%.
[0047] It should be noted that the weight average molecular weight in this application is measured by gel permeation chromatography (GPC) with reference to SN / T 4183-2015.
[0048] In a preferred embodiment, the photocurable resin composition includes, by weight: 50-65 parts of alkali-soluble resin, 34-49 parts of photopolymerizable monomers, 0.3-5 parts of photosensitizers, and 0.5-5 parts of additives. Compared with other ranges, limiting the amount of each component in the photocurable resin composition to the above range is conducive to improving the comprehensive properties of the photocurable resin composition such as wet pressing analysis, adhesion performance, and wet pressing hole covering performance, and is convenient for wet film lamination process and roll-to-roll continuous production process.
[0049] In a preferred embodiment, the photopolymerizable monomer includes one or more of the compounds represented by the following general formulas (B1), (B2), (B3), (B4), (B5), and (B6):
[0050]
[0051] Among them, m 1 and m 2 Each independently takes any integer from 1 to 30, n 1 and n 2 Each independently takes any integer from 0 to 20, m 1 +m 2 Take any integer from 2 to 30, n 1 +n 2 Take any integer from 0 to 20, n 1 Corresponding segment and m 1 The corresponding segments can be arranged randomly or in blocks, n 2 Corresponding segment and m 2 The corresponding segments can be arranged randomly or in blocks;
[0052]
[0053] Among them, m 3 and m 4 Each independently takes any integer from 1 to 30, m 3 +m 4 Take any integer from 15 to 30,
[0054]
[0055] Among them, a 1 and b 1 Each independently takes any integer from 0 to 20, a 1 The corresponding segment and b 1 The corresponding segments can be arranged randomly or in blocks;
[0056]
[0057] Among them, a 2 and c 2 Each independently takes any integer from 0 to 20, b 2 Take any integer from 1 to 20, a 2 +c 2 is any integer from 2 to 30, a 2 Corresponding segment, b 2 The corresponding segment and c 2 The corresponding segments can be arranged randomly or in blocks;
[0058]
[0059] Among them, b 3 Take any integer from 1 to 20, a 3 and c 3 Each independently takes any integer from 1 to 20, a 3 +c 3 Take any integer from 2 to 30, b 3 Take any integer from 2 to 20, a 3 Corresponding segment, b 3 The corresponding chain segment and c 3 The corresponding segments can be arranged randomly or in blocks;
[0060]
[0061] Among them, a 4 Take any integer from 2 to 30, b 4 Take any integer from 0 to 20, a 4 The corresponding segment and b 4 The corresponding segments can be arranged randomly or in blocks;
[0062] In the compounds represented by the general formula (B1), (B2), (B3), (B4), (B5), and (B6), R b Each independently includes but is not limited to H or C 1 ~C 4 The alkyl group of EO represents an ethoxy group and the PO represents a propoxy group.
[0063] Compared with other types of photopolymerizable monomers, the above-mentioned types of photopolymerizable monomers contain ethoxy groups, or a combination of ethoxy groups and propoxy groups, which is beneficial to improving the water absorption and hydrophilicity of the photopolymerizable monomers, thereby improving the wet pressure filling performance of the photocurable resin composition, and further helping to reduce the occurrence of plugging.
[0064] In order to further improve the hydrophilicity of the photopolymer elastomer, and further improve the wet pressure filling performance of the photocurable resin composition, and reduce the occurrence of plugging, preferably, the content of the compound represented by general formula (B2) is 5 to 15 wt % based on the total weight of the photocurable resin composition.
[0065] In a preferred embodiment, the photopolymerizable monomer further comprises a monofunctional, difunctional or multifunctional (meth)acrylate ethylenically unsaturated double-bond monomer other than the above structural formula, more preferably lauryl (meth)acrylate, octadecyl (meth)acrylate, nonylphenol acrylate, isobornyl ester, tetrahydrofuran methyl acrylate, bisphenol A di(meth)acrylate, polyethylene glycol (propylene glycol) di(meth)acrylate, ethoxylated (propoxylated) neopentyl glycol diacrylate, trimethylolpropane tri(meth)acrylate, ethoxylated (propoxylated) trimethylolpropane tri(meth)acrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, and one or more of the group consisting of polyurethane acrylate. Compared with other types, the use of the above types of photopolymerizable monomers is conducive to reducing the tendency of glue overflow, and is also conducive to improving the photosensitivity and resolution of the photocurable resin composition.
[0066] In a preferred embodiment, the photosensitizer includes a photoinitiator or a hexaarylbisimidazole photoinitiator and a sensitizer represented by the general formula (C1) or the general formula (C2):
[0067]
[0068] Among them, R c Including but not limited to H, C 1 ~C 6 Alkyl, C 2 ~C 3 The halogenated alkyl, C 1 ~C 3 substituted or unsubstituted aryl, halogenated aryl, or pyridyl; Rc ’ Including but not limited to C 3 ~C 10 A straight chain alkylene group.
[0069] In order to further improve the sensitivity of the photocurable resin composition in the wavelength range of 350 to 420 nm, preferably, Rc includes but is not limited to methyl, ethyl, phenyl, chloroethyl, methoxy, ethoxy, methylphenyl, ethylphenyl, n-propylphenyl, n-butylphenyl, tert-butylphenyl, methoxyphenyl, ethoxyphenyl, and chlorophenyl.
[0070] In order to further improve the photosensitivity of the photocurable resin composition in the 350-420 nm band, and further improve the photosensitivity, resolution and adhesion of the photocurable resin composition on the substrate surface, in a preferred embodiment, the sensitizer includes but is not limited to aromatic ketone compounds, anthraquinone compounds, coumarin compounds, N-phenylglycine compounds, anthracene compounds, pyrazoline compounds, amino acid compounds, quinone compounds, acetophenone compounds, acylphosphine oxide compounds, benzoin compounds, benzoin ether compounds, dialkyl ketal compounds, thioxanthone compounds, and dialkylaminobenzoate compounds. One or more of the group consisting of 5-(4-methoxyphenyl)-3-[2-(4-methoxyphenyl)vinyl]-1-phenyl-pyrazoline, 5 One or more of the group consisting of 1-phenyl-3-biphenyl-1-phenyl-pyrazoline, 1-phenyl-3-(4-tert-butylphenylphenyl)-5-(4-tert-butylphenyl)-pyrazoline, 1-(4-(benzoxazol-2-yl)phenyl)-3-(4-tert-butylphenylphenyl)-5-(4-tert-butylphenyl)-pyrazoline, 1-phenyl-3-(4-biphenylyl)-5-(4-tert-butylphenyl)-pyrazoline, 1-phenyl-3-(4-biphenylyl)-5-(4-tert-octylphenyl)-pyrazoline, N-phenylglycine, N-methyl-N-phenylglycine, N-ethyl-N-phenylglycine, benzophenone, Michler's ketone [4,4'-bis(dimethylamino)benzophenone], 4,4'-bis(diethylamino)benzophenone and 4-methoxy-4'-dimethylaminobenzophenone.
[0071] In a preferred embodiment, the compound represented by the general formula (C1) includes, but is not limited to, one or more of the group consisting of 9-methylacridine, 9-ethylacridine, 9-phenylacridine, 9-chloroethylacridine, 9-methoxyacridine, 9-ethoxyacridine, 9-(4-methylphenyl)acridine, 9-(4-ethylphenyl)acridine, 9-(4-n-propylphenyl)acridine, 9-(4-n-butylphenyl)acridine, 9-(4-tert-butylphenyl)acridine, 9-(4-methoxyphenyl)acridine, 9-(4-ethoxyphenyl)acridine, 9-m-tolylacridine, 9-o-tolylacridine, 9-p-phenylacridine, and 9-p-chlorophenylacridine. Compared with other types, using the compound represented by the general formula (C1) of the above type as the main component of the photosensitizer is beneficial to further improve the sensitivity of the photocurable resin composition in the wavelength range of 350 to 420 nm.
[0072] In a preferred embodiment, the compound represented by the general formula (C2) includes but is not limited to 1,7-bis(9,9'-acridinyl)heptane. Compared with other types, using the compound represented by the general formula (C2) as the main component of the photosensitizer is beneficial to further improve the sensitivity of the photocurable resin composition in the wavelength range of 350 to 420 nm.
[0073] In order to further improve the sensitivity of the photocurable resin composition in the wavelength range of 350 to 420 nm, and to further adapt to traditional UV and LED exposure machines and laser direct imaging (LDI) exposure machines, thereby further improving the photosensitivity, resolution and adhesion of the photocurable resin composition to the substrate surface, preferably, the ratio of the total weight of the compounds represented by the general formula (C1) and the general formula (C2) and the sensitizer to the sum of the weights of the alkali-soluble resin and the photopolymerizable monomer is (0.3 to 2):100.
[0074] In order to further improve the photosensitivity of the photocurable resin composition in the 350-420 nm band, further improve the photosensitivity, resolution and adhesion of the photocurable resin composition on the surface of the substrate, and its compatibility with traditional UV and LED exposure machines, preferably, the hexaarylbisimidazole photoinitiator includes but is not limited to 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer, 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenyl-1,1'-diimidazole. One or more of the group consisting.
[0075] In a preferred embodiment, the additives include, but are not limited to, one or more of the group consisting of a coloring agent, a dye, a plasticizer, a light and heat stabilizer, an adhesion promoter, a leveling agent, a defoamer, and an inhibitor. Introducing the above additives into the photocurable resin composition is beneficial to production and processing, and is beneficial to improving its processability. The above types of additives can be compounded in any ratio.
[0076] The second aspect of the present application also provides an application of the above-mentioned photocurable resin composition provided by the present application in the field of photocuring. The above-mentioned photocurable resin composition provided by the present application has excellent hole covering performance, film removal performance, and adhesion performance, and is suitable for a roll-to-roll continuous production process of a flexible board. The application of the above-mentioned photocurable resin composition in the field of photocuring can take into account the production needs of precision circuit flexible boards and rigid boards, can improve product yield, can significantly improve the production efficiency of PCB manufacturing, lead frame manufacturing, semiconductor packaging, ITO and other components in the field of flat panel displays, and reduce production costs.
[0077] The third aspect of the present application also provides a photosensitive dry film resist laminate, which includes a support layer and a resist layer, and the resist layer is prepared from the above-mentioned photocurable resin composition provided by the present application. The above-mentioned photocurable resin composition provided by the present application has excellent hole covering performance, film removal performance, and adhesion performance, and is suitable for a roll-to-roll continuous production process of a flexible board. The application of the above-mentioned photocurable resin composition in the preparation of the resist layer of the photosensitive dry film resist laminate can take into account the production requirements of precision circuit flexible boards and rigid boards, can improve product yield, can significantly improve the production efficiency of PCB manufacturing, lead frame manufacturing, semiconductor packaging, ITO and other components in the field of flat panel displays, and reduce production costs.
[0078] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0079] (I) Alkali-soluble resin preparation example
[0080] The synthesis method of the alkali-soluble resin (A1-1) used in the examples of the present application comprises:
[0081] Methacrylic acid, methyl methacrylate, butyl methacrylate and styrene are mixed in a weight ratio of 30:30:10:30, and mixed with 1.0 g of azobisisobutyronitrile (AIBN) initiator, 90 g of butanone and 15 g of ethanol to obtain a mixed solution; 35% by mass of the mixed solution is added into a three-necked flask with nitrogen protection and a condensation reflux device through a peristaltic pump, and the oil bath is heated to 80° C., and the remaining mixed solution is added dropwise after stirring for 1 hour, and the addition is completed within 3 hours; after continuing to keep the temperature for 4 hours, the temperature is raised to 90° C., and 5 g of butanone solution dissolved with 0.2 g of AIBN initiator is added twice, with an interval of 1 hour between the two times. After the addition is completed, the mixture is kept warm and stirred for 2 hours to terminate the reaction to obtain an alkali-soluble resin (A1-1).
[0082] The weight average molecular weight and molecular weight distribution index were tested by GPC method, and the solid content was obtained by drying and weighing.
[0083] The synthesis method of the alkali-soluble resin (A2-1) used in the examples of the present application comprises:
[0084] (1) Preparation of a semi-addition product of a diol and an isocyanate: 20 g of butanone and 9.1 g of ethylene glycol (1.15 equivalents) were added to a three-necked flask, nitrogen was introduced, and 6.66 mg of dibutyltin dilaurate and 22.2 g of toluene diisocyanate (1.0 equivalent) were slowly added dropwise under stirring conditions. The mixture was reacted at 45° C. for 6 h until no change in the -NCO content was detected. The reaction was stopped to obtain a solution of a semi-addition product of a diol and an isocyanate, which was sealed and stored for use in the next step as soon as possible.
[0085] (2) Preparation of alkali-soluble resin (A2-1): 30 g of butanone was added to a three-necked flask, nitrogen was introduced, the temperature was raised to 80°C, and 25 g of methacrylic acid, 30 g of methyl methacrylate, 14.8 g of hydroxyethyl methacrylate, 0.7 g of A mixture of AIBN initiator, 30g butanone and 10g ethanol was added dropwise within 1 hour, and the mixture was reacted at 80°C for 12 hours to obtain a product system of acrylic resin containing carboxyl and hydroxyl groups; the product system was cooled to room temperature, 2 drops of dibutyltin dilaurate, 10g butanone and an appropriate amount of p-hydroxyanisole inhibitor (so that the content of the inhibitor in the system is 100-200ppm) were added, and the temperature was raised to 60°C, and the semi-addition product of the diol and isocyanate obtained in step (1) was added dropwise within 1 hour. After the addition was completed, the reaction was continued at 60°C with stirring for 4 hours. The reaction was stopped when the absorption peak of -NCO at 2274cm-1 detected by infrared spectroscopy basically disappeared, and an alkali-soluble resin (A2-1) was obtained.
[0086] Alkali-soluble resins A1-1 to A1-5 were synthesized according to the formula shown in Table 1 as examples, alkali-soluble resins A2-1 to A2-6 were synthesized according to the formula shown in Table 2 as examples, and alkali-soluble resins AX-1 to AX-4 were synthesized according to the formula shown in Table 3 as comparative examples.
[0087] Table 1
[0088]
[0089] Table 2
[0090]
[0091]
[0092] Table 3
[0093]
[0094] (II) Preparation Example of Photocurable Resin Composition
[0095] According to the formulas in Tables 4, 5 and 6 below, the components were mixed in proportion, 40 parts by weight of butanone was added, and then stirred until completely dissolved to prepare a resin composition solution with a solid content of 40wt%. It was evenly coated on the surface of a 15μm thick PET support film using a coating machine, and placed in a 90℃ oven for 10 minutes to form a 30μm thick photosensitive dry film resist layer, which appeared blue-green under a yellow light. Then, a 20μm thick polyethylene film protective layer was attached to its surface to obtain a 3-layer photosensitive film.
[0096] Photopolymerizable monomers:
[0097] B-1: (20) ethoxylated bisphenol A diacrylate (Meiyuan), corresponding to general formula (B2), m 3 +m 4 =20;
[0098] B-2: (30) ethoxylated bisphenol A diacrylate (Meiyuan), corresponding to the general formula (B2), m 3 +m 4 =30;
[0099] B-3: (10) ethoxylated bisphenol A diacrylate (Meiyuan), corresponding to the general formula (B1), m 1 +m 2 =10,n 1 +n 2 =0;
[0100] B-4: (10) ethoxylated (4) propoxylated bisphenol A diacrylate (Meiyuan), corresponding to the general formula (B1), m 1 +m2 =10,n 1 +n 2 =4;
[0101] B-5: Polyethylene glycol (400) dimethacrylate (Meiyuan), corresponding to general formula (B3), a 1 =9, b 1 =0;
[0102] B-6: Polypropylene glycol (700) (6) ethoxylated dimethacrylate (Meiyuan), corresponding to general formula (B4), b 2 =12, a 2 +c 2 =6;
[0103] B-7: (8) Ethoxylated nonylphenol acrylate (Meiyuan), corresponding to general formula (B6), a 4 =8, b 4 =0;
[0104] Photosensitizer:
[0105] C-1: 9-phenylacridine;
[0106] C-2: N-phenylglycine;
[0107] C-3: 2,2'-bis(2-chlorophenyl)-4,4'-5,5'-tetraphenyl-1,1'-diimidazole (Changzhou Qiangli Electronic New Materials);
[0108] C-4: 5-(4-methoxyphenyl)-3-[2-(4-methoxyphenyl)vinyl]-1-phenyl-pyrazoline;
[0109] additive:
[0110] D-1: brilliant green pigment (Shanghai Bailingwei Chemical Technology Co., Ltd.);
[0111] D-2: Leuco crystal violet (Shanghai J&K Chemical Technology Co., Ltd.);
[0112] D-3: p-Toluenesulfonamide (Shanghai TCI Chemical).
[0113] Table 4
[0114]
[0115] Table 5
[0116]
[0117] Table 6
[0118]
[0119] The following describes the sample preparation method (including film lamination, exposure, development, and copper electroplating), the sample evaluation method, and the evaluation results of the examples and comparative examples.
[0120] (1) Sample preparation method
[0121]
Substrate
[0122] 1. Is there a substrate for the plugging hole test, film removal time and film removal fragment evaluation?
[0123] A double-sided flexible copper-clad laminate with a thickness of 50 μm and 200 small-diameter through holes with a diameter of 0.1 mm, laminated with 18 μm rolled copper foil and 10 μm copper plating.
[0124] 2. Substrates for photosensitivity, wet pressure analysis, wet pressure adhesion performance, and flexibility evaluation:
[0125] A 50μm thick smooth double-sided flexible copper clad laminate with no small diameter through holes, laminated with 18μm rolled copper foil and 10μm copper plating.
[0126] 3. Substrate for wet pressing hole capping performance evaluation:
[0127] The plate thickness is 1.6mm rigid shaped hole plate. The shaped hole plate used in the test has round holes and shaped holes with diameters of 6.0mm, 5.0mm, and 4.0mm. The specific samples are as follows Figure 1 After 30 minutes of film application, the film was exposed at an exposure energy of 18 frames. After 30 minutes of exposure, the film was developed at 4 times the shortest development time, and the hole-breaking rate was calculated to evaluate the hole-masking performance.
[0128]
Wet film lamination
[0129] 1. Wet pressing flexible substrate film:
[0130] a. Cut the double-sided flexible copper clad laminate (FCCL) into a rectangle of 250mm×280mm without any pre-treatment such as grinding or micro-etching; b. Add deionized water or distilled water to the sponge roller, then pass the flexible substrate through the sponge roller to evenly coat a layer of water film on the copper surface; c. Set the laminating temperature of the laminating machine to 100℃ and the pressure to 4.0kg / cm 2 , speed is 1.0m / min.
[0131] 2. Cover hole test rigid substrate wet pressure film
[0132] a. Polish the copper surface of the customized rigid substrate with special-shaped holes with a grinder, wash it with water, micro-etch it, blow it dry, and other pre-treatment operations to obtain a bright and fresh copper surface; b. Add deionized water or distilled water to the sponge roller, then pass the flexible substrate through the sponge roller to evenly coat a layer of water film on the copper surface; c. Set the film laminating machine to a laminating temperature of 100°C and a pressure of 4.0kg / cm 2 , speed is 1.0m / min.
[0133]
exposure
[0134] 1. Use laser direct imaging (LDI) exposure machine for exposure
[0135] After film application, the sample was left to stand for more than 15 minutes. The resolution and adhesion performance were tested by using a Japanese Adtec exposure machine, model: IP-6, a laser direct imaging (LDI) exposure machine with a wavelength of 405nm. A stouffer 41-step exposure ruler was used for photosensitivity testing, and the number of exposure grids was controlled at 18 grids.
[0136] 2. Use conventional UV exposure machine for exposure
[0137] After film application, the sample was left to stand for more than 15 minutes, and then exposed using the M-552 parallel light exposure machine of Zhisheng Technology. The number of exposure grids was measured using a stouffer 41-step exposure ruler, and the number of exposure grids was controlled at 18 to 19 grids.
[0138] 3. Use conventional LED exposure machine for exposure
[0139] After film application, the sample was left to stand for more than 15 minutes, and then exposed using an LED exposure machine (model: Hongshengxiang HSX-LEDS5) with an exposure intensity of 40%. A stouffer 41-step exposure ruler was used to measure the number of exposure grids, which was controlled at 18 to 19 grids.
[0140]
development
[0141] After exposure, the sample was left to stand for more than 15 minutes, the developing temperature was 30°C, and the pressure was 1.2 kg / cm 2 The developer is a 1 wt% sodium carbonate aqueous solution, the developing time is 1.5 to 2.0 times the minimum developing time, and the film is washed and dried after developing. The minimum developing time is the minimum time required for the unexposed part of the resist layer to be completely dissolved.
[0142]
Acid etching
[0143] The developed copper plate was subjected to an etching process, the etching solution was cupric chloride, the etching speed was 1.0 m / min, the etching temperature was 48°C, the spray pressure was 1.5 bar, the specific gravity was 1.3 g / mL, the acidity was 2 mol / L, the copper ion was 140 g / L, and the etching machine model was Dongguan Universe GL181946.
[0144]
Removal of film
[0145] The stripping solution is NaOH, the concentration is 3.0wt%, the temperature is 50℃, and the pressure is 1.2kg / cm 2 The film stripping time is 1.5 to 2.0 times of the minimum film stripping time. After film stripping, wash and dry.
[0146] (2) Evaluation method
[0147]
Photosensitivity and matching evaluation of different exposure machines
[0148] After film pasting, the sample was left to stand for more than 15 minutes, and then exposed using Adtec IP-6 405nm LDI exposure machine, Zhisheng Technology M-552 model, and UV light exposure machine Hongshengxiang HSX-LEDS5 LED exposure machine. The sensitivity test was performed using a stouffer 41-step exposure ruler. After exposure, it was sprayed with a 1wt% sodium carbonate aqueous solution at 30°C, and the development time was 2.0 times the minimum development time to remove the unexposed part. After this operation, a cured film formed by the cured product of the photosensitive resin composition was formed on the copper surface of the substrate. The exposure amount (mJ / cm 2 ), the sensitivity of the photosensitive resin composition was evaluated. The smaller the exposure energy value, the better the sensitivity.
[0149] The evaluation criteria are as follows: “○” indicates that the exposure energy of the LDI exposure machine is 20 to 40 mJ / cm 2 , UV and LED exposure machine exposure energy 15 ~ 30mJ / cm 2 , no poor analysis; "△" means LDI exposure energy 40~60mJ / cm 2 , UV and LED exposure machine exposure energy 25 ~ 50mJ / cm 2 ; “×” indicates LDI exposure energy>60mJ / cm 2 , UV and LED exposure machine exposure energy 25 ~ 50mJ / cm 2 .
[0150] [Test and evaluation of whether there is a small hole plugging phenomenon]
[0151] After the wet pressing and laminating, the test substrate used for the above test of whether there is a phenomenon of plugging of small holes was placed at 25°C and 60% relative humidity for 48 hours, and then an Adtec IP-6 405nm LDI exposure machine was used (IP-6 has a good exposure curing depth, and it is more difficult to remove the film in the small holes). The exposure energy was the energy corresponding to 19 grids using a stouffer 41-step exposure ruler for sensitivity testing. The above-mentioned exposure, development and film removal were performed, and the ratio of the number of small holes with incomplete film removal (the number of plugged holes) to the total number of small through holes was evaluated according to the following judgment criteria.
[0152] The evaluation criteria are as follows: "○" indicates qualified, that is, there is no plugging phenomenon in the small holes, and there is no film fragmentation residue on the flexible board surface, that is, the number of plugged holes is zero; "△" indicates poor quality, that is, there is plugging phenomenon, but the proportion of the number of plugged holes is less than 10%; "×" indicates completely unqualified, that is, there is plugging phenomenon, the proportion of the number of plugged holes is more than 10%, and there are obvious film fragmentation residues on the flexible board surface.
[0153]
Test and evaluation of film removal time and film removal fragment size
[0154] After wet pressing the test substrate used for the above test of film stripping time and film stripping fragments, the sample was left to stand for 24 hours after film stripping, and an Adtec IP-6 405nm LDI exposure machine was used. The exposure energy was the energy corresponding to 19 grids using a stouffer 41-step exposure ruler for sensitivity testing. The above exposure, development and film stripping were performed, and the film stripping time and film stripping piece size of the photosensitive dry film resist were evaluated according to the following judgment criteria.
[0155] The evaluation criteria are as follows: "○" means that the film removal time is ≤35s, the size of the film removal fragments is 5-15mm, and it can be applied to the flexible board roll-to-roll continuous process; "△" means that the film removal time is 35s>≤50s, the size of the film removal fragments is 15-30mm, the film removal time is too long, the film is too large, and the production efficiency is low; "×" means that the film removal time is greater than 50s, or the size of the film removal fragments is greater than 30mm, which seriously affects the production efficiency or yield.
[0156]
Evaluation of wet pressure analysis capability
[0157] The wet press analysis evaluation substrate was placed for 24 hours after wet press lamination, and exposed using an Adtec IP-6405nm LDI exposure machine. The sensitivity test was performed using a stouffer 41-step exposure ruler. The exposure was performed using a mask with a wiring pattern with a width of 1:1 between the exposed and unexposed parts, corresponding to a sensitivity of 18 to 19 grids. A 1wt% sodium carbonate aqueous solution was sprayed at 30°C, and the development time was 2.0 times the minimum development time to remove the unexposed part. The minimum mask width that normally formed a cured resist line was used as the resolution value, and the image was observed using a two-dimensional imager or a scanning electron microscope (SEM). The smaller the number read, the better the wet press analysis performance.
[0158]
Evaluation of wet pressure adhesion
[0159] The above-mentioned substrate for evaluating wet-press adhesion performance was placed for 24 hours after wet-press lamination, and exposed using an Adtec IP-6405nm LDI exposure machine. A sensitivity test was performed using a stouffer 41-step exposure ruler. Exposure was performed using a mask having a wiring pattern with a width of n:400μm between the exposed and unexposed parts, corresponding to a sensitivity of 18 to 19 grids. After development with twice the minimum development time, observation was performed using a magnifying glass, and the minimum mask width at which a complete cured resist line was formed was taken as the adhesion value. The smaller the number read, the better the adhesion.
[0160]
Evaluation of wet-pressing capping performance
[0161] The above-mentioned substrate for evaluating wet-pressing hole-capping performance, the irregular hole plate, was left to stand for 24 hours after wet-pressing and laminating, and then exposed using an Adtec IP-6405nm LDI exposure machine with an exposure energy corresponding to a sensitivity of 18 to 19 grids. After 30 minutes of exposure, it was developed for 4 times the shortest development time, and the hole-breaking rate was counted to evaluate the wet-pressing hole-capping performance. Generally speaking, masking irregular holes requires higher performance in terms of the flexibility of the photosensitive dry film than masking round holes, and it is also more difficult.
[0162] The evaluation criteria are as follows: "○" indicates that the hole rate is ≤2% (occasionally there may be a few holes caused by production conditions); "△" indicates that the hole rate is 2%>≤10%; "×" indicates that the entire board surface has obvious holes.
[0163]
Evaluation of flexibility
[0164] After wet pressing and laminating the film on the flexible substrate (FPC) for flexibility evaluation, let it stand for more than 15 minutes, and then use AdtecIP-6405nm LDI exposure machine to expose it with exposure energy corresponding to 18-19 grids of sensitivity. After exposure for 30 minutes, it is developed with a development time twice the minimum development time to obtain a flexibility evaluation substrate with dry film resist laminated on the FPC substrate. The flexibility is evaluated using a mandrel tester. The flexibility evaluation substrate is cut into strips with a width of 2 cm and a length of 10 cm. After rubbing it with a cylindrical rod at 180° for 10 times, the condition of the dry film resist on the substrate is confirmed, and the diameter of the corresponding round rod where the dry film has no glass or cracks is recorded.
[0165] The evaluation criteria are as follows: "○" indicates no cracking at 3 mm or less, "△" indicates no cracking at 4 mm, and "×" indicates no cracking at 5 mm or more.
[0166] (3) The results of performance evaluation such as photosensitivity, whether there is pore plugging, film removal performance, wet pressure analysis, wet pressure adhesion, wet pressure pore covering, and flexibility are shown in Tables 7 and 8
[0167] Table 7
[0168]
[0169] Table 8
[0170]
[0171] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0172] By comparing Examples 1 to 10 with Comparative Examples 1 to 8, it can be seen that the photosensitive dry film resists obtained in Examples 1 to 10 all have the following key properties: good wet pressing analysis and adhesion performance, fast film removal speed, clean film removal of the cured resist in the small holes without any residue (no hole plugging phenomenon), small film removal sheet size, can be applied to the roll-to-roll continuous production process of flexible boards, and excellent wet pressing hole covering performance and flexibility.
[0173] The photocurable resin compositions prepared in the above-mentioned embodiments 1 to 10 of the present application have excellent comprehensive properties, and are stable in performance when applied to the wet pressing lamination process. Therefore, the performance of the obtained photosensitive dry film resist fully meets the performance requirements of the photosensitive dry film resist for producing flexible circuit boards and rigid circuit boards with fine circuits using the wet pressing process, and meets the use requirements of the flexible board roll-to-roll continuous production process.
[0174] The alkali-soluble resins used in Comparative Examples 1 to 3 are alkali-soluble resins conventionally used in photosensitive dry film resists for manufacturing precision flexible or rigid circuit boards. From the test results, although the wet pressing analysis and adhesion performance basically meet the requirements, the phenomenon of small hole plugging is obvious, and the film removal time is relatively long. The flexibility and wet pressing hole covering performance are extremely poor, which will seriously affect the production yield and efficiency of manufacturing precision flexible circuit boards.
[0175] In Comparative Examples 4 to 6, in order to improve the film removal performance and reduce the occurrence of plugging, long-chain alkyl (meth)acrylates (AX-3 and AX-4) or styrene-containing alkali-soluble resins (AX-2) are compounded. From the experimental results, the adhesion performance of the photocurable resin composition is significantly reduced, and it is not suitable for the production of fine circuit boards. In addition, the film removal fragments are obviously larger, the film removal is more difficult, and the plugging problem is prone to occur. It is not suitable for roll-to-roll continuous production process.
[0176] In Comparative Example 7, only alkali-soluble resin A1-1 is used as the alkali-soluble resin. From the experimental results, there are no abnormalities in photosensitivity, wet pressing analysis and adhesion performance, but there is an obvious pore plugging phenomenon, the film removal time is also very long, and the wet pressing pore covering ability and flexibility are extremely poor.
[0177] In Comparative Example 8, only alkali-soluble resin A2-1 is used as the alkali-soluble resin. From the experimental results, it can be seen that the wet pressing pore covering and flexibility properties are better, the small hole plugging phenomenon and film removal performance are slightly better than those of Comparative Example 7, but there is still a slight pore plugging phenomenon, the film removal piece is slightly larger, and the wet pressing analysis and adhesion performance are slightly reduced.
[0178] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.
[0179] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A photocurable resin composition, It is characterized in that The photocurable resin composition comprises: an alkali-soluble resin, a photopolymerizable monomer, a photosensitizer and an additive; the alkali-soluble resin comprises compounds represented by general formula (I) and general formula (II): Among them, R 1 and R 2 are independently selected from H or C 1 ~C 4 The alkyl group; R 3 Selected from C 1 ~C 18 Substituted or unsubstituted straight chain alkyl or branched chain alkyl, C 7 ~C 14 Aryl-substituted alkyl, C 5 ~C 14 Alkyl substituted or unsubstituted cycloalkyl, hydroxy substituted C 1 ~C 18 A straight chain alkyl or branched chain alkyl, or C 1 ~C 4 An amino group substituted with a straight-chain alkyl group or a branched-chain alkyl group; R 4 Selected from H, C 1 ~C 3 Alkyl, C 1 ~C 3 an alkoxy group, an amino group or a halogen atom, and z 1 The R in the corresponding segment 4 The number of substitutions is any integer from 0 to 5; R 4 'Selected from H or C 1 ~C 4 The alkyl group; In terms of percentage of the molecular weight of the compound represented by the general formula (I), x 1 The content of the corresponding segment is 27-40wt%, y 1 The content of the corresponding segment is 20 to 73 wt %, and the z 1 The content of the corresponding segment is 0 to 40 wt%; Among them, R 5 , R 6 , R 8 are independently selected from H or C 1 ~C 4 The alkyl group; R 7 Selected from C 1 ~C 18 Substituted or unsubstituted straight chain alkyl or branched chain alkyl, C 7 ~C 14 Aryl-substituted alkyl, C 5 ~C 14 Alkyl substituted or unsubstituted cycloalkyl, hydroxy substituted C 1 ~C 18 A straight chain alkyl group or a branched chain alkyl group; R 9 One selected from the following groups: R 10 Selected from C 2 ~C 10 A straight chain alkylene or branched chain alkylene, wherein n is any integer from 2 to 5; In terms of percentage of the molecular weight of the compound represented by the general formula (II), x 2 The content of the corresponding segment is 22-27 wt%, y 2 The content of the corresponding segment is 21-65wt%, z 2 The content of the corresponding segment is 10 to 50 wt%.
2. The photocurable resin composition according to claim 1, It is characterized in that The weight ratio of the compound represented by the general formula (I) to the compound represented by the general formula (II) is (15-35):(15-40); Preferably, the acid value of the compound represented by the general formula (I) is 210 to 310 mgKOH / g; Preferably, the acid value of the compound represented by the general formula (II) is 170 to 210 mgKOH / g.
3. The photocurable resin composition according to claim 1, It is characterized in that In the compound represented by the general formula (I), R 1 is selected from H or methyl, said R 2 is selected from H or methyl, said R 3 is selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, isooctyl, C 12 Straight chain alkyl, C 18 Straight chain alkyl, benzyl, epoxypropyl substituted methylene, hydroxyethyl, hydroxypropyl, hydroxybutyl, -N(CH 3 ) 2 , or -N(C 2 H 5 ) 2 , the R 4 is selected from H or methyl, and said z 1 The R in the corresponding segment 4 The number of substitutions is 0 or 1, and the R 4 ' is selected from H or methyl; Preferably, in the compound represented by the general formula (II), R 5 , R 6 , R 8 are independently selected from H or methyl, the R 7 is selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, isooctyl, C 12 Straight chain alkyl, C 18 A straight-chain alkyl group, a benzyl group, a glycidyl-substituted methylene group, a hydroxyethyl group, a hydroxypropyl group, or a hydroxybutyl group, R 10 Selected from ethylene, propylene or decylene.
4. The photocurable resin composition according to any one of claims 1 to 3, It is characterized in that The weight average molecular weight of the compound represented by the general formula (I) is 30,000 to 80,000, and the molecular weight distribution index is 1.3 to 2.5; Preferably, the weight average molecular weight of the compound represented by general formula (II) is 60,000 to 90,000, and the molecular weight distribution index is 1.3 to 2.
5.
5. The photocurable resin composition according to claim 4, It is characterized in that The photocurable resin composition comprises, by weight, 50 to 65 parts of the alkali-soluble resin, 34 to 49 parts of the photopolymerizable monomer, 0.3 to 5 parts of the photosensitizer and 0.5 to 5 parts of the additive.
6. The photocurable resin composition according to claim 5, It is characterized in that The photopolymerizable monomer includes one or more compounds represented by the following general formulas (B1), (B2), (B3), (B4), (B5), and (B6): Among them, m 1 and m 2 Each independently takes any integer from 1 to 30, n 1 and n 2 Each independently takes any integer from 0 to 20, m 1 +m 2 Take any integer from 2 to 30, n 1 +n 2 Take any integer from 0 to 20, the n 1 The corresponding segment and the m 1 The corresponding segments can be arranged randomly or in blocks, and the n 2 The corresponding segment and the m 2 The corresponding segments can be arranged randomly or in blocks; Among them, m 3 and m 4 Each independently takes any integer from 1 to 30, m 3 +m 4 Take any integer from 15 to 30, Among them, a 1 and b 1 Each independently takes any integer from 0 to 20, wherein a 1 The corresponding segment and b 1 The corresponding segments can be arranged randomly or in blocks; Among them, a 2 and c 2 Each independently takes any integer from 0 to 20, b 2 Take any integer from 1 to 20, a 2 +c 2 is any integer from 2 to 30, wherein a 2 The corresponding segment, the b 2 The corresponding segment and the c 2 The corresponding segments can be arranged randomly or in blocks; Among them, b 3 Take any integer from 1 to 20, a 3 and c 3 Each independently takes any integer from 1 to 20, a 3 +c 3 Take any integer from 2 to 30, b 3 Take any integer from 2 to 20, where a 3 The corresponding segment, the b 3 The corresponding segment and the c 3 The corresponding segments can be arranged randomly or in blocks; Among them, a 4 Take any integer from 2 to 30, b 4 Take any integer from 0 to 20, where a 4 The corresponding segment and b 4 The corresponding segments can be arranged randomly or in blocks; In the compounds represented by the general formula (B1), (B2), (B3), (B4), (B5), and (B6), R b are independently selected from H or C 1 ~C 4 EO represents an ethoxy group, and PO represents a propoxy group; Preferably, the photopolymerizable monomer also includes a monofunctional, difunctional or multifunctional (meth)acrylate-based ethylenically unsaturated double-bond monomer, more preferably lauryl (meth)acrylate, octadecyl (meth)acrylate, nonylphenol acrylate, isobornyl ester, tetrahydrofuran methyl acrylate, bisphenol A di(meth)acrylate, polyethylene glycol (propylene glycol) di(meth)acrylate, ethoxylated (propoxylated) neopentyl glycol diacrylate, trimethylolpropane tri(meth)acrylate, ethoxylated (propoxylated) trimethylolpropane tri(meth)acrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, and one or more of the group consisting of polyurethane acrylate.
7. The photocurable resin composition according to claim 5 or 6, It is characterized in that The photosensitizer includes a photoinitiator or a hexaarylbisimidazole photoinitiator and a sensitizer represented by the general formula (C1) or the general formula (C2): Among them, R c Selected from H, C 1 ~C 6 Alkyl, C 2 ~C 3 The halogenated alkyl, C 1 ~C 3 substituted or unsubstituted aryl, halogenated aryl, or pyridyl; R c ’ Selected from C 3 ~C 10 A straight chain alkylene group; Preferably, the sensitizer is selected from one or more of the group consisting of aromatic ketone compounds, anthraquinone compounds, coumarin compounds, N-phenylglycine compounds, anthracene compounds, pyrazoline compounds, amino acid compounds, quinone compounds, acetophenone compounds, acylphosphine oxide compounds, benzoin compounds, benzoin ether compounds, dialkyl ketal compounds, thioxanthone compounds, and dialkylaminobenzoate compounds; More preferably, the sensitizer is selected from 5-(4-methoxyphenyl)-3-[2-(4-methoxyphenyl)vinyl]-1-phenyl-pyrazoline, 5-phenyl-3-biphenyl-1-phenyl-pyrazoline, 1-phenyl-3-(4-tert-butylphenylphenyl)-5-(4-tert-butylphenyl)-pyrazoline, 1-(4-(benzoxazol-2-yl)phenyl)-3-(4-tert-butylphenylphenyl)-5-(4-tert-butylphenyl)-pyrazoline, 1-phenyl-3-( One or more of the group consisting of 1-phenyl-3-(4-biphenyl)-5-(4-tert-butylphenyl)-pyrazoline, 1-phenyl-3-(4-biphenyl)-5-(4-tert-octylphenyl)-pyrazoline, N-phenylglycine, N-methyl-N-phenylglycine, N-ethyl-N-phenylglycine, benzophenone, Michler's ketone [4,4'-bis(dimethylamino)benzophenone], 4,4'-bis(diethylamino)benzophenone and 4-methoxy-4'-dimethylaminobenzophenone; More preferably, the ratio of the total weight of the compounds represented by the general formula (C1) and the general formula (C2) and the sensitizer to the sum of the weights of the alkali-soluble resin and the photopolymerizable monomer is (0.3-2):
100.
8. The photocurable resin composition according to any one of claims 1 to 7, It is characterized in that The additive is selected from one or more of the group consisting of a coloring agent, a dye, a plasticizer, a light and heat stabilizer, an adhesion promoter, a leveling agent, a defoaming agent, and an inhibitor.
9. Use of the photocurable resin composition according to any one of claims 1 to 8 in the field of photocuring.
10. A photosensitive dry film resist laminate, It is characterized in that The photosensitive dry film resist laminate comprises a support layer and a resist layer, and the resist layer is prepared from the photocurable resin composition according to any one of claims 1 to 8.
Citation Information
Patent Citations
Light-cured resin composition and application thereof
CN116184763A
Photosensitive composition using polysiloxane, resin membrane comprising the same and display element having its resin membrane
JP2008209739A
Exhaust filter system for radioactive material in the nuclear power plant
KR102171512B1