Negative photosensitive polyimide photoresist, preparation method thereof, polyimide film and application

By introducing isomerized polyimide resin and low-temperature curing accelerator into negative photosensitive polyimide photoresist, low-temperature curing at below 250°C is achieved, and conventional photosensitive polyimides are solved at high temperatures The resulting wafer warping and solder joint cracking improves the performance and pattern resolution of microelectronic packaging.

CN119024643APending Publication Date: 2024-11-26HUANGPU INST OF MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411173792.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Conventional photosensitive polyimides cause wafer warping and solder joint cracking during high temperature curing, limiting their applications in the field of microelectronic packaging, especially in fan-out wafer-level packaging and fan-out flat-panel packaging. Low temperature curing cannot be achieved.

Method used

A negative photosensitive polyimide photoresist has been developed, including isomerized polyimide resin, photoinitiator, photocrosslinker, silane coupling agent, light stabilizer and low-temperature curing accelerator, through specific The polymerization and salt formation reaction steps are prepared to achieve low temperature curing at 250°C or less.

Benefits of technology

The photoresist combines excellent photosensitive performance and low-temperature curing performance, avoids wafer warping and solder joint cracking, significantly improves the performance of plastic packaging devices, and achieves high-resolution polyamides in microelectronic packaging amine pattern preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119024643A_ABST
    Figure CN119024643A_ABST
Patent Text Reader

Abstract

The invention relates to a negative photosensitive polyimide photoresist, a preparation method thereof, a polyimide film and application. The negative photosensitive polyimide photoresist comprises isomerized polyimide resin, a photoinitiator, a photocrosslinking agent, a silane coupling agent, a light stabilizer, a low-temperature curing accelerator and an organic solvent, and only part of retaining ring imidization diacyl contained in the isomerized polyimide resin forms a cyclic imide structure. One acyl of the other part forms an amide structure, and the other acyl and photosensitive tertiary amine small molecules form carboxylic acid quaternary ammonium salt; the low-temperature curing accelerator can promote the curing reaction of the isomerized polyimide resin at the curing temperature lower than or equal to 250 DEG C; the mass ratio of the low-temperature curing accelerator to the isomerized polyimide resin is (0.1-0.5): 5. The negative photosensitive polyimide photoresist has excellent photosensitive performance and low-temperature curing performance, and a cured product has relatively high glass transition temperature and thermal stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of photoresists, and in particular to a negative photosensitive polyimide photoresist and a preparation method thereof, a polyimide film and applications thereof. Background Art

[0002] With the continuous development of large-scale integrated circuits, the requirements for high-performance polymer packaging materials in the field of microelectronic packaging are getting higher and higher, requiring packaging materials to have excellent thermal stability, mechanical properties and dielectric properties. Based on its excellent comprehensive performance, polyimide (PI) materials have been widely used in semiconductor packaging fields such as integrated circuits and chip packaging. Photosensitive polyimide (PSPI) has photosensitive properties and does not require coating of photoresist to form patterns. It can avoid steps such as removing photoresist, thereby simplifying the application process, making the PSPI film layer as an insulating protective layer in the field of microelectronic packaging. The curing temperature of conventional PSPI is relatively high when applied, generally above 300°C; however, for application scenarios such as fan-out wafer-level packaging (FOWLP) and fan-out flat-panel packaging (FOPLP), during the high-temperature thermal imidization process, the wafer may warp, and the solder joints of the low-melting solder of the plastic-encapsulated circuit may crack, fall off, recrystallize, etc., which will seriously damage the performance of the plastic-encapsulated device. The inability to cure at low temperatures limits the application of conventional PSPI. Therefore, it is urgent to develop low-temperature curing PSPI to meet the application needs in related fields. Summary of the invention

[0003] Based on this, the present application at least provides a negative photosensitive polyimide photoresist and a preparation method thereof, a polyimide film and an application thereof. The negative photosensitive polyimide photoresist has both excellent photosensitivity and low-temperature curing performance.

[0004] In a first aspect of the present application, a negative photosensitive polyimide photoresist is provided, which comprises the following components: an isomerized polyimide resin, a photoinitiator, a photocrosslinker, a silane coupling agent, a light stabilizer, a low-temperature curing accelerator and an organic solvent.

[0005] In some embodiments, a negative photosensitive polyimide photoresist is provided, comprising the following components: an isomerized polyimide resin, a photoinitiator, a photocrosslinker, a silane coupling agent, a light stabilizer, a low temperature curing accelerator, and an organic solvent;

[0006] Wherein, the isomerized polyimide resin is a polymer having a structure shown in formula (I):

[0007]

[0008] In formula (I),

[0009] Each R3 is independently -L1-O-C(=O)-C(M)=CH2, where L1 is an alkylene group and M is H or methyl; each R1 and each R2 are independently an alkyl group. 1-6 Each Ar1 is independently a tetravalent aromatic group and has four single-bond sites on the aromatic ring. 1-3 Each Ar2 is independently a divalent aromatic group and has two single-bond sites on the aromatic ring.

[0010] m satisfies 0 < m < 1, optionally 0 < m ≤ 0.5 (furthermore, m can be a value selected from 0.01 to 0.5, and even further can be a value selected from 0.05 to 0.4), and n is an integer selected from 10 to 100.

[0011] Ar and Ar are each independently a capping group containing an aromatic group.

[0012] The low-temperature curing accelerator can promote the curing reaction of the isomerized polyimide resin at a curing temperature of 250 °C or lower, and the mass ratio of the low-temperature curing accelerator to the isomerized polyimide resin is (0.1 - 0.5):5.

[0013] In the second aspect of the present application, a method for preparing a negative photosensitive polyimide photoresist is provided, which includes the following steps: According to the components contained in the negative photosensitive polyimide photoresist described in the first aspect of the present application, the isomerized polyimide resin, the photoinitiator, the photocrosslinker, the silane coupling agent, the light stabilizer, the low-temperature curing accelerator, and the organic solvent are mixed to prepare the negative photosensitive polyimide photoresist. 31 Among them, the isomerized polyimide resin is prepared by a method including the following steps: 32 Under anhydrous, oxygen-free, and continuous dispersion conditions, an aromatic diamine monomer and an aromatic dianhydride monomer are mixed in a polymerization solvent at a molar ratio of 0.9:1 to 1:0.9, and a polymerization reaction is carried out at 0 °C to 100 °C for 6 h to 8 h to generate a polyamic acid chain. A capping molecule is added, and a capping reaction is carried out at 0 °C to 100 °C for 1 h to 2 h to obtain a first mixed solution containing a polyamic acid intermediate.

[0014]

[0015]

[0016]

[0017]

[0018] ​​​​A dehydrating agent and a catalyst are added to the first mixed solution, and a dehydration reaction is carried out at 0°C to 50°C for 1.5h to 2.5h to generate an isomerized polyamic acid, and a photosensitive tertiary amine small molecule containing R3 is added, and a salt-forming reaction is carried out at 0°C to 50°C for 3h to 5h in a dark environment to obtain a second mixed solution; wherein R3 is -L1-OC(=O)-C(M)=CH2, L1 is C 1-6 Alkylene, M is H or methyl; the molar ratio of the dehydrating agent to the aromatic dianhydride monomer is (0.01-1):1;

[0019] The second mixed liquid is mixed with an alcohol solvent to precipitate a polyimide salt, the solid-liquid separation is performed, and the solid phase is collected, washed, and dried to obtain the isomerized polyimide resin;

[0020] in,

[0021] The structure of the aromatic diamine monomer is

[0022] The structure of the aromatic dianhydride monomer is

[0023] The polyamic acid chain has a chain structure shown in formula (II-1): Wherein, each * represents a capping site;

[0024] The structure of the polyamic acid intermediate is shown in formula (II-2):

[0025]

[0026] The structure of the isomerized polyamic acid is shown in formula (II-3):

[0027]

[0028] In the third aspect of the present application, a polyimide film is provided, which is formed by curing the negative photosensitive polyimide photoresist described in the first aspect of the present application, or by curing the negative photosensitive polyimide photoresist prepared by the preparation method described in the second aspect of the present application; the curing temperature is lower than or equal to 250°C.

[0029] In a fourth aspect of the present application, there is provided an application of the negative photosensitive polyimide photoresist described in the first aspect of the present application or the negative photosensitive polyimide photoresist prepared by the preparation method described in the second aspect of the present application in preparing a polyimide micro pattern, wherein the application comprises the following steps: drying the negative photosensitive polyimide photoresist at 100° C. to 120° C. to form a photosensitive film, exposing, developing, cleaning, and curing at a curing temperature lower than or equal to 250° C.;

[0030] Optionally, curing is performed at a curing temperature of 100° C. to 250° C.;

[0031] Further optionally, curing is performed at a curing temperature of 200°C to 250°C.

[0032] In some embodiments, the application includes application in microelectronic packaging; wherein the microelectronic packaging includes at least one of a fan-out wafer-level packaging and a fan-out panel-level packaging;

[0033] The curing temperature includes one or more temperatures between 200°C and 250°C. By using an isomerized polyimide resin (also referred to as isomerized polyimide PII) and a low-temperature curing agent, the negative photosensitive polyimide photoresist has excellent photosensitivity and a low curing temperature. Moreover, while achieving low-temperature curing, the cured product has a relatively high glass transition temperature and thermal stability. The isomerized polyimide PII includes an aromatic structural unit having two pairs of acylated imide groups (referred to as U1) and an aromatic structural unit having two bondable amino groups (referred to as U2); wherein a portion of the acylated imide groups form a cyclic imide structure with the bondable amino groups, and another portion of the acylated imide groups are not acylated, one acylate group forms an amide bond (-CO-NH-) in the polymer main chain with the bondable amino group, and the other acylate group forms a carboxylic acid quaternary ammonium salt (-COO - / + NH(-)3), this structural design can effectively reduce the curing temperature. In addition, the isomerized polyimide PII can be converted into polyimide when heated at low temperature. There is no water vapor release in this process, and there will be no coating porosity problem. The isomerized polyimide PII has high solubility in solvents and a relatively stable structure. The cured polyimide has a high glass transition temperature and thermal stability. Furthermore, the curing temperature is further reduced by combining with a low-temperature curing accelerator. By synergistically controlling the proportion of the cyclic imide structure formed by the imidized diacyl group in the isomerized polyimide PII and the amount of low-temperature curing accelerator added, the negative photosensitive polyimide photoresist can have excellent photosensitivity and a low curing temperature at the same time, and a cured product with a high glass transition temperature and thermal stability can be obtained.

[0034] The imidization degree in the isomerized polyimide resin can be regulated by combining chemical imidization and thermal imidization to achieve partial imidization, thereby preparing the aforementioned isomerized polyimide resin and further obtaining a negative photosensitive polyimide photoresist that can be cured at low temperature.

[0035] The polyimide film or photoresist cured film formed by low temperature curing (such as curing temperature ≤ 250°C, and further, for example, curing temperature includes one or more temperatures between 200°C and 250°C) of the aforementioned negative photosensitive polyimide photoresist has a high glass transition temperature and thermal stability. When the negative photosensitive polyimide is used to prepare a polyimide micron pattern, a high-resolution polyimide pattern can be obtained. In addition, taking the plastic encapsulation device process as an example, during the low temperature curing process of the negative photosensitive polyimide photoresist, wafer warping can be avoided or suppressed, and cracking, shedding, recrystallization and other problems of the solder joints of the low-melting solder can also be avoided or suppressed, thereby significantly improving the performance of the plastic encapsulation device.

[0036] The low temperature curing negative photosensitive polyimide photoresist provided in the present application can be widely used to prepare micron patterns. As one of the non-limiting application modes, it can be applied to the field of microelectronic packaging, including but not limited to fan-out wafer level packaging (FOWLP) and fan-out flat panel packaging (FOPLP). BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the technical solutions in the implementation methods and examples of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for use in the description of the implementation methods or examples. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0038] Figure 1 Scanning of the negative photosensitive polyimide resin developed pattern for photolithography development in Example 1 (optical microscope).

[0039] Figure 2 Scanning of the negative photosensitive polyimide resin development pattern for photolithography development in Example 2 (optical microscope).

[0040] Figure 3 Scanning (optical microscope) of the negative photosensitive polyimide resin developed by lithography in Comparative Example 1.

[0041] Figure 4 Scanning (optical microscope) of the negative photosensitive polyimide resin developed by photolithography in Comparative Example 2. DETAILED DESCRIPTION

[0042] The present application will be further described in detail below in conjunction with the accompanying drawings, implementation modes and examples. It should be understood that these implementation modes and examples are only used to illustrate the present application and are not used to limit the scope of the present application. The purpose of providing these implementation modes and examples is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0043] In this application, "multiple", "multiple", "multiple times", "multiple", "several", etc., unless otherwise specified, refer to a quantity greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two. In this application, unless otherwise specified, "one or more" means any one of the listed items or any combination of the listed items. Similarly, "one or more" and other ways of indicating "one or more" are also understood in the same way unless otherwise specified.

[0044] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0045] In this application, unless otherwise specified, "room temperature" refers to 20°C to 30°C.

[0046] In this application, if the unit of the data range is followed only by the right endpoint, it means that the units of the left endpoint and the right endpoint are the same. For example, 3~5h means that the units of the left endpoint "3" and the right endpoint "5" are both h (hours), which have the same meaning as 3h~5h. In addition, similar descriptions involving other parameters such as temperature and size also apply to the above understanding.

[0047] In the present application, exemplary descriptions such as "in some implementation modes (or examples)" and "in one implementation mode (or example)" may include but are not limited to the following meanings: these solutions may be combined with other solutions in a suitable manner to form new technical solutions.

[0048] In the present application, the terms "first", "second", "third", "fourth", etc. in "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0049] In this application, unless otherwise specified, "about" means within a certain range above and below the number, and the fluctuation range may vary depending on the type and value of the number. For example, it can be allowed to be within a range of ±10%, ±5%, ±2%, ±1%, etc. For example, taking "about 20°C" and its approximate value of ±1°C as an example, the approximate values ​​of 19°C, 19.5°C, etc. within the approximate range shown in "about 20°C" should also be included in the range indicated by "about 20°C". For example, about 600Da can be selected from 600±60Da, 600±60Da.

[0050] In the present application, unless otherwise specified, wt% means weight percentage, and vol% means volume percentage.

[0051] In this application, “C 1-6 "Alkyl" refers to an alkyl group containing 1 to 6 carbon atoms, and each occurrence may be independently C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl or C6 alkyl. Suitable examples include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, -CH2CH(CH3)2, -CH(CH3)CH2CH3, tert-butyl, n-pentyl, -CH(CH3)CH2CH2CH3, -CH(CH2CH3)2, -C(CH3)2CH2CH3, -CH(CH3)CH(CH3)2, -CH 2CH2CH(CH3)2, -CH2CH(CH3)CH2CH3, n-hexyl, -CH(CH3)CH2CH2CH2CH3, -CH(CH2CH3)(CH2CH2CH3), -C(CH3)2CH2CH2CH3, -CH(CH3)CH(CH3)CH2CH3, -CH(CH3)CH2CH(CH3)2, -C(CH3)(CH2CH3)2, -CH(CH2CH3)CH(CH3)2, -C(CH3)2CH(CH3)2, etc.

[0052] In this application, “C 1-6 "Alkylene" means that the alkyl portion contains 1 to 6 carbon atoms and each occurrence can be independently C1 alkylene, C2 alkylene, C3 alkylene, C4 alkylene, C5 alkylene or C6 alkylene. Suitable examples include, but are not limited to, methylene (-CH2-), 1,1-ethylene (-CH(CH3)-), 1,2-ethylene (-CH2CH2-), 1,1-propylene (-CH(CH2CH3)-), 1,2-propylene (-CH2CH(CH3)-), 1,3-propylene (-CH2CH2CH2-) and 1,4-butylene (-CH2CH2CH2CH2-).

[0053] In the present application, "aromatic group" refers to a group with aromatic properties, "aromatic structure" refers to a structure with aromatic properties, and "aromatic ring" refers to a ring structure with aromatic properties, and those skilled in the art are familiar with their meanings.

[0054] In the present application, "aliphatic anhydride" refers to an anhydride without aromatic properties, including an anhydride structure represented by *-C(=O)-O-(O=)C-*, where * represents a single bond site connected to a carbon atom.

[0055] In the present application, a "substituent" corresponds to an atomic radical or a non-hydrogen atom.

[0056] In the present application, "non-hydrogen atoms" refer to atoms of other kinds than hydrogen atoms.

[0057] In the present application, "small molecule" refers to a relative molecular mass of less than 1000, or a molecular weight of less than 1000 Daltons (Da).

[0058] In the present application, the site of introducing a single bond from any suitable position on the ring can be etc., * indicates a single bond site. "Any suitable position on the ring" refers to a position that is allowed to be a single bond site, for example, for an aromatic ring, a position where no other substituents are set. For example, All six carbon atoms can serve as single bond sites. In the case of -OH, only five carbon atoms can serve as single bond sites (carbon atoms replaced by -OH cannot serve as single bond sites). It means that two benzene rings can be connected by any combination of sites, which can be but not limited to the following connection methods wait.

[0059] There are literature reports that by synthesizing soluble polyimide, the rigid structure of polyimide is destroyed, thereby reducing the curing temperature to below 300°C. However, the end-capping method used will lead to the sacrifice of the thermodynamic properties and photosensitivity of the cured product.

[0060] In the first aspect of the present application, a negative photosensitive polyimide photoresist is provided. The negative photosensitive polyimide photoresist comprises an isomerized polyimide resin, a photoinitiator, a photocrosslinking agent, a silane coupling agent, a light stabilizer, a low-temperature curing accelerator and an organic solvent, wherein the isomerized polyimide resin comprises an aromatic structural unit having two pairs of imidized diacyl groups (which can be denoted as U1, (-(O=)C)2Ar a (-C(=O)-)2) and aromatic structural units with two bondable amino groups (referred to as U2, (-)2N-Ar b -N(-)2), along the polymer main chain, U1 and U2 are connected by a cyclic imide structure ((-)2Ara (-C(=O)-)2N-Ar b -) or amide structure (-C(=O)-NH-), Ar in U1 a and Ar in U2 b Each independently represents an aromatic ring, which may be the same or different, Ar a With four single bond sites located on the aromatic ring, Ar b It has two single bond sites located on the aromatic ring; wherein a portion of the imide-capable diacyl groups and the bondable amino groups form a cyclic imide structure (Ar a (-C(=O)-)2N-), the other part of the imide diacyl group is not cleaved, one of the acyl groups forms an amide structure (-CO-NH-) with the bondable amino group, and the other acyl group forms a carboxylic acid quaternary ammonium salt (-COO - / + NH(-)3); that is, only a part of the acylated imide diacyl groups forms a cyclic imide structure, while a part of the bondable amino groups participates in the formation of the cyclic imide structure, a part participates in the formation of the amide structure, and a part participates in the formation of the photosensitive carboxylic acid quaternary ammonium salt structure, and at least one bondable amino group in each U2 unit participates in the formation of the cyclic imide structure or the amide structure; the low-temperature curing accelerator can promote the curing reaction of the isomerized polyimide resin at a curing temperature less than or equal to 250°C, such as a curing temperature ≤250°C, and further, for example, the curing temperature includes one or more temperatures between 200°C and 250°C; the mass ratio of the low-temperature curing accelerator and the isomerized polyimide resin is controlled at a suitable ratio, such as (0.1 to 0.5): 5. The negative photosensitive polyimide photoresist has both excellent photosensitivity and low-temperature curing performance, and the cured product has a relatively high glass transition temperature and thermal stability.

[0061] The isomerized polyimide resin used is an ionic negative low-temperature curing photosensitive polyimide in which a polyimide and a polyamic acid salt coexist. Among the acylated imidization diacyl groups contained in the isomerized polyimide resin, only a part forms a cyclic imide structure, an acyl group of the other part forms an amide structure, and another acyl group forms a carboxylic acid quaternary ammonium salt with a photosensitive tertiary amine small molecule. In the structure of the isomerized polyimide resin, the acylated imidization diacyl groups existing in the combination of the amide structure and the carboxylic acid quaternary ammonium salt can be referred to as "isomerized structure" relative to common cyclic imide structure. The aforementioned isomerized polyimide resin can reduce the curing temperature of the photoresist, and also has good solubility, which can improve the stability of the photoresist, but the higher the isomerized structure ratio, the lower the photosensitivity. By introducing a low-temperature curing accelerator, the photoresist can have good photosensitivity while reducing the curing temperature.

[0062] By using an isomerized polyimide resin (also denoted as isomerized polyimide PII) and a low-temperature curing agent, it is achieved that the negative photosensitive polyimide photoresist has both excellent photosensitivity and a low curing temperature. In addition, while achieving low-temperature curing, the cured product has a relatively high glass transition temperature and thermal stability. The isomerized polyimide PII includes an aromatic structural unit having two pairs of acylated imide groups (denoted as U1) and an aromatic structural unit having two bondable amino groups (denoted as U2); wherein a portion of the acylated imide groups and the bondable amino groups form a cyclic imide structure, and the other portion of the acylated imide groups are not acylated, one acylation group forms an amide bond (-CO-NH-) in the polymer main chain with the bondable amino group, and the other acylation group forms a carboxylic acid quaternary ammonium salt (-COO - / + NH(-)3), this structural design can effectively reduce the curing temperature. In addition, the isomerized polyimide PII can be converted into polyimide when heated at low temperature. There is no water vapor release in this process, and there will be no coating porosity problem. The isomerized polyimide PII has high solubility in solvents and a relatively stable structure. The cured polyimide has a high glass transition temperature and thermal stability. Furthermore, the curing temperature is further reduced by combining with a low-temperature curing accelerator. By synergistically controlling the proportion of the cyclic imide structure formed by the imidized diacyl group in the isomerized polyimide PII and the amount of low-temperature curing accelerator added, the negative photosensitive polyimide photoresist can have excellent photosensitivity and a low curing temperature at the same time, and a cured product with a high glass transition temperature and thermal stability can be obtained.

[0063] The negative photosensitive polyimide photoresist can be cured at a curing temperature less than or equal to 250° C. In a non-limiting manner, the curing temperature can be 100° C. to 250° C., and can further be 100° C. to 200° C., 200° C. to 250° C., etc. See also the curing temperature in the fourth aspect of the present application. In some embodiments, the curing temperature includes one or more temperatures in the range of 200° C. to 250° C.

[0064] In some embodiments, the structures of U1 and U2 may be as shown below, respectively:

[0065]

[0066] Wherein, Ar1 is a tetravalent aromatic group having four single bond sites on the aromatic ring; Ar2 is a divalent aromatic group having two single bond sites on the aromatic ring; Indicates a single bond site. Unless otherwise specified, the two It can be connected to two different atoms respectively, or to the same atom. Each in U2a is connected to different atoms respectively. Ar1 and Ar2 can also refer to the definitions in the context respectively. Ar1 and Ar2 each include an aromatic ring, and the aromatic rings in the two can be the same or different. For example, they can both be benzene rings, or one can be a benzene ring and the other can be a bicyclic biphenyl type.

[0067] In this application, Ar1 and have the same meaning and can be used interchangeably; Ar2 and have the same meaning and can be used interchangeably. If either of Ar1 and Ar2 is replaced with an aliphatic group, it will cause a decrease in the thermal stability of the isomerized polyimide resin.

[0068] In some embodiments, a negative photosensitive polyimide photoresist is provided, which comprises the following components: an isomerized polyimide resin, a photoinitiator, a photocrosslinking agent, a silane coupling agent, a light stabilizer, a low-temperature curing accelerator, and an organic solvent;

[0069] Among them, the isomerized polyimide resin is a polymer having the structure shown in formula (I):

[0070]

[0071] In formula (I),

[0072] any one of R3 is independently -L1-O-C(=O)-C(M)=CH2, L1 is C 1-6 alkylene, M is H or methyl; any one of R1 and any one of R2 are each independently C 1-3 alkyl;

[0073] any one of Ar1 is independently a tetravalent aromatic group and has four single bond sites located on the aromatic ring;

[0074] any one of Ar2 is independently a divalent aromatic group and has two single bond sites located on the aromatic ring;

[0075] m satisfies 0 < m < 1, optionally ≤ 0.5 (furthermore, m can be a value selected from 0.01 to 0.5), and n is an integer selected from 10 to 100;

[0076] Ar 31 and Ar 32 are each independently a capping group containing an aromatic group;

[0077] The low-temperature curing accelerator can promote the curing reaction of the isomerized polyimide resin at a curing temperature of less than or equal to 250 °C, and the mass ratio of the low-temperature curing accelerator to the isomerized polyimide resin is (0.1 - 0.5):5.

[0078] In formula (I), m reflects the proportion of the ring-closure imidized diacyl to form a cyclic imide structure. The larger the value of m, the higher the degree of imidization; the smaller the value of m, the higher the degree of isomerization. Theoretically, when m = 0, it means that there is no cyclic imide structure in the structure of formula (I); when m = 1, it means that there is no isomerization structure in the structure of formula (I), and all the ring-closure imidized diacyls form cyclic imide structures. It can be understood that in the isomerized polyimide resin involved in this application, 0 < m < 1 is satisfied. For the traditional polyimide resin with m = 1, the curing temperature is usually above 300°C; in addition, during the high-temperature thermal imidization process, the wafer may also warp, which may cause phenomena such as cracking, peeling, and recrystallization of the solder joints.

[0079] In some embodiments of this application, m satisfies 0 < m < 0.7.

[0080] In some embodiments of this application, m satisfies 0 < m < 0.6.

[0081] By introducing a suitable proportion of isomerization structure into the isomerized polyimide resin, the curing temperature can be reduced to a certain extent, and a certain photosensitive property can be maintained. Further, a low-temperature curing accelerator can be synergistically used to further reduce the curing temperature, and a photosensitive quaternary ammonium carboxylate can be synergistically used to improve the photosensitive property, so that the photoresist has excellent photosensitive property and low-temperature curing property as a whole. In some embodiments of this application, m satisfies 0 < m ≤ 0.5. Further, m can be a value selected from 0.01 to 0.5, still further can be a value selected from 0.05 to 0.4, and can also be any one of the following values or an interval composed of any two of the following values: 0.01, 0.02, 0.04, 0.05, 0.06, 0.08, 0.09, 0.1, 0.12, 0.14, 0.15, 0.16, 0.18, 0.2, 0.25, 0.29, 0.3, 0.35, 0.36, 0.37, 0.38, 0.4, 0.45, 0.5, etc. Non-limitingly, m can also be selected from any one of the following ranges: 0.05 ≤ m ≤ 0.5, 0.05 ≤ m ≤ 0.4, 0.08 ≤ m ≤ 0.5, 0.08 ≤ m ≤ 0.4, 0.05 ≤ m ≤ 0.38, 0.08 ≤ m ≤ 0.38, 0.09 ≤ m ≤ 0.5, 0.09 ≤ m ≤ 0.4, 0.09 ≤ m ≤ 0.37, etc.

[0082] In the present application, the m value can be regulated by adjusting the degree of imidization or by controlling the degree of isomerization. In some embodiments of the present application, the degree of imidization is regulated by combining chemical imidization and thermal imidization; wherein, in the chemical imidization process, the m value can be regulated by adjusting one or more of the parameters such as the type and amount of the catalyst, the type and amount of the dehydrating agent, and the reaction time of the imidization; in the thermal imidization process, the m value can be regulated by adjusting one or more of the parameters such as the heat treatment temperature and time. In some embodiments, the m value is mainly regulated by adjusting the amount of the dehydrating agent and the catalyst.

[0083] In formula (I), n reflects the number of the smallest repeating units and can be used to adjust the molecular weight of the isomerized polyimide resin. The larger the n value, the higher the molecular weight of the isomerized polyimide resin.

[0084] In the present application, n can be an integer selected from 10 to 100, and can also be any of the following integers or an interval consisting of any two of the following integers: 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, etc.

[0085] In the present application, the n value can be controlled by adjusting one or more parameters such as the concentration of the polymerization reaction raw materials, the polymerization temperature, the polymerization time, the amount of the end-capping molecule, etc.

[0086] In some embodiments, in formula (I), any R3 is independently an alkyl group substituted with an unsaturated carboxylic acid ester group, for example, a C substituted with an acrylate group (CH2=CH-C(=O)-O-) 1-6 Alkyl or methacrylate (CH2=C(CH3)-C(=O)-O-) substituted C 1-6 In some embodiments, in formula (I), any one of R3 is independently -L1-OC(=O)-C(M)=CH2, L1 is C 1-6 Alkylene, M is H or methyl. Without limitation, L1 can be C 1-4 The alkylene group may further be a methylene group, an ethylene group, a propylene group or a butylene group, and may further be a 1,2-ethylene group.

[0087] In some embodiments, each R3 in Formula (I) is the same.

[0088] In some embodiments, in formula (I), any R1 and any R2 are each independently C 1-3 The alkyl group may further be independently methyl or ethyl. In some embodiments, R1 and R2 are both methyl.

[0089] In some embodiments, L1 is 1,2-ethylene, and R1 and R2 are both methyl. Available M may be a hydrogen atom (H) or a methyl group (-CH3).

[0090] In some embodiments, each R1 in formula (I) is the same, and each R2 is the same, that is, the combination of R1 and R2 is the same.

[0091] In some embodiments, in formula (I), each R1 is the same, each R2 is the same, and each R3 is the same, that is, are the same. It is possible to use a single type of tertiary amine molecule This is achieved by a salt-forming reaction with the carboxyl group on the Ar1 ring.

[0092] In some embodiments, in formula (I), any Ar1 may independently be a tetravalent aromatic group having four single bond sites on the aromatic ring. In some embodiments, in formula (I), any Ar1 may independently be a tetravalent aromatic group having 6 to 35 (optionally 6 to 30, further optionally 6 to 20, further optionally 6 to 14, further optionally 6 to 13, further optionally 6 to 12, further optionally 6) non-hydrogen atoms.

[0093] In some embodiments, the aromatic ring in Ar1 is provided by one or more benzene rings, and the number of benzene rings can be 1, 2 or 3; when the number of benzene rings is greater than 1, adjacent benzene rings can be connected by a single bond, a methylene (-CH2-), a -C(CH3)2-, a carbonyl, an oxy group (-O-), two independent oxy groups, or two independent methylene groups. When connected by two independent oxy groups, a six-membered ring is formed between the two oxygen atoms and the two adjacent benzene rings. When connected by two independent methylene groups, a six-membered ring is formed between the carbon atoms of the two methylene groups and the two adjacent benzene rings.

[0094] In some embodiments, the non-hydrogen atoms in Ar1 are selected from carbon atoms and oxygen atoms, and include at least carbon atoms, and may or may not include oxygen atoms.

[0095] In some embodiments, in formula (I), any Ar1 is independently any of the following structures:

[0096]

[0097] Each * represents a single bond site.

[0098] In some embodiments, each Ar1 in formula (I) is the same and can be formed by using a single type of aromatic dianhydride monomer.

[0099] In some embodiments, in formula (I), any Ar2 can be independently a divalent aromatic group with two single bond sites on the aromatic ring. In some embodiments, in formula (I), any Ar2 can be independently a divalent aromatic group with 6 to 25 (optionally 6 to 20, further optionally 6 to 15, further optionally 6 to 14, further optionally 6 to 13, further optionally 6 to 12, further optionally 6) non-hydrogen atoms.

[0100] In some embodiments, the aromatic ring in Ar2 is provided by one or more benzene rings, and the number of benzene rings can be 1, 2 or 3; when the number of benzene rings is greater than 1, adjacent benzene rings can be connected by a single bond, a methylene (-CH2-), a carbonyl group, an oxy group (-O-), a sulfenyl (-S-), or two independent oxy groups. When connected by two independent oxy groups, two oxygen atoms form a six-membered ring with two adjacent benzene rings.

[0101] In some embodiments, the non-hydrogen atoms in Ar2 are selected from carbon atoms, oxygen atoms and sulfur atoms, and at least include carbon atoms, and may or may not include heteroatoms. The heteroatoms may be selected from one or both of oxygen atoms and sulfur atoms. In some embodiments, the type of heteroatoms in Ar2 is 0 or 1. In some embodiments, Ar2 includes only one heteroatom, which may be an oxygen atom or a sulfur atom.

[0102] In some embodiments, in formula (I), any Ar2 is independently any of the following structures:

[0103]

[0104] Each * represents a single bond site.

[0105] In some embodiments, each Ar2 in formula (I) is the same and can be formed by using a single type of aromatic diamine monomer.

[0106] In some embodiments, Ar 31 and Ar 32 Each independently is a capping group containing -NH-Ar0, Ar0 is C 6-10 Aromatic groups. In some embodiments, Ar0 is 3-hydroxyphenyl, 2-hydroxyphenyl or 4-hydroxyphenyl. In some embodiments, Ar0 is 3-hydroxyphenyl, which can be formed by using m-aminophenol as a capping molecule, but is not limited thereto.

[0107] In some embodiments, in formula (I), each R1 is the same, each R2 is the same, each R3 is the same, each Ar1 is the same, and each Ar2 is the same. In this case, a single type of aromatic dianhydride monomer, a single type of aromatic diamine monomer, and a single type of photosensitive tertiary amine small molecule can be used.

[0108] In some embodiments, the negative photosensitive polyimide photoresist satisfies one, any suitable multiple or all of the following characteristics;

[0109] L1 is 1,2-ethylene, and R1 and R2 are both methyl groups;

[0110] In formula (I), any Ar1 is independently a tetravalent aromatic group having 6 to 35 non-hydrogen atoms;

[0111] In formula (I), any Ar2 is independently a divalent aromatic group having 6 to 25 non-hydrogen atoms;

[0112] Ar 31 and Ar 32 Each independently is a capping group containing -NH-Ar0, Ar0 is C 6-10 Aromatic groups;

[0113] In formula (I), each R1 is the same, each R2 is the same, each R3 is the same, each Ar1 is the same, and each Ar2 is the same;

[0114] m is a value selected from 0.01 to 0.5.

[0115] In the present application, "low temperature curing accelerator" is named because it can promote the curing reaction of isomerized polyimide resin at low temperature (such as at a curing temperature less than or equal to 250°C). Without limitation, the low temperature curing accelerator can be selected from but not limited to one or more of isoquinoline, p-quinoline and pyridine. In some embodiments, the low temperature curing accelerator is any one of isoquinoline, p-quinoline and pyridine. In some embodiments, the curing temperature includes one or more temperatures between 200°C and 250°C.

[0116] The content of unsaturated carbon-carbon double bonds in the photoresist can be increased by adding and adjusting the dosage of the photocrosslinking agent, which is beneficial to giving the negative photosensitive polyimide photoresist better photosensitivity.

[0117] In some embodiments, the photocrosslinker is an ester derivative of a polyol containing at least two alkenyl esters, and the structures of the at least two alkenyl esters are each independently -OC(=O)-C(M2)=CH2, wherein M2 is H or methyl. The molecular weight of the ester derivative of a polyol containing at least two alkenyl esters can be referred to the definition below.

[0118] In some embodiments, the polyol in the ester derivative of a polyol containing at least two alkenyl esters may be a diol, a triol, or a tetraol.

[0119] In the present application, the molecular weight of the ester derivative of the polyol containing at least two alkenyl esters is recorded as M1. Without limitation, M1 can satisfy M1≤1000Da, optionally M1≤800Da, and further optionally M1≤500Da. Without limitation, M1 can also be selected from any of the following ranges: 170Da to 1000Da, optionally 200Da to 1000Da, further optionally 250Da to 1000Da, further optionally 250Da to 500Da, and further optionally 250Da to 420Da.

[0120] In some embodiments, the polyol in the ester derivative of a polyol containing at least two alkenyl esters is ethylene glycol or oligoethylene glycol; further, the number of ethylene glycol units contained in the oligoethylene glycol may be 2 to 6, optionally 2 to 5, and further optionally 2 to 4. Non-limitingly, the number of ethylene glycol units contained in the oligoethylene glycol may be 2, 3, 4, 5 or 6. In some embodiments, the polyol in the ester derivative of a polyol containing at least two alkenyl esters is ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol (i.e., triethylene glycol), pentaethylene glycol or hexaethylene glycol.

[0121] In some embodiments, the photocrosslinker is CH2=C(M 21 )-C(=O)-O-(CH2CH2O) q -C(=O)-C(M 22 )=CH2, wherein q is an integer selected from 1 to 6 (such as 1, 2, 3, 4, 5 or 6), M 21 and M 22 Each independently represents H or methyl. q may also be an integer selected from 2 to 6, or an integer selected from 3 to 5. In some embodiments, q is equal to 4. M 21 and M 22 M may be the same or different. 21 and M 22 The same may further be H or methyl, and further may be methyl. In some embodiments, the photocrosslinking agent is tetraethylene glycol dimethacrylate.

[0122] Without limitation, the mass ratio of the photocrosslinking agent to the isomerized polyimide resin may be (1.2-2):5, i.e., 1.2:5 to 2:5, which also corresponds to (0.24-0.4):1. The mass ratio of the photocrosslinking agent to the isomerized polyimide resin may also be any of the following ratios or a ratio range selected from any two of the following ratios: 1.2:5, 1.25:5, 1.4:5, 1.5:5, 1.6:5, 1.7:5, 1.75:5, 1.8:5, 2:5, etc.

[0123] In a non-limiting manner, the photoinitiator may be a benzophenone photoinitiator or a benzophenone photoinitiator. The mass ratio of the photoinitiator to the isomerized polyimide resin may be, but is not limited to, (0.18 to 0.22):5. The mass ratio of the photoinitiator to the isomerized polyimide resin may also be any of the following ratios or a ratio range selected from any two of the following ratios: 0.18:5, 0.19:5, 0.20:5, 0.21.7:5, 0.22:5, etc.

[0124] By introducing a coupling agent, the adhesion of the photoresist cured film to the substrate can be effectively improved.

[0125] In some embodiments, the silane coupling agent may be a silane coupling agent containing a hydrophilic group, and the hydrophilic group may be, but is not limited to, a hydroxyl group or an amino group. In some embodiments, the silane coupling agent includes one or both of diphenyldihydroxysilane and γ-aminopropyltriethoxysilane, and further, the silane coupling agent may be diphenyldihydroxysilane or γ-aminopropyltriethoxysilane. Non-limitingly, the mass ratio of the silane coupling agent to the isomerized polyimide resin may be (0.14 to 0.16):5, or any of the following ratios or a ratio range selected from any two of the following ratios: 0.14:5, 0.15:5, 0.16:5, etc.

[0126] In the negative photosensitive polyimide photoresist, the storage time of the glue solution can be extended by adding a light stabilizer. In some embodiments, the light stabilizer includes a phenolic light stabilizer. In some embodiments, the light stabilizer is a phenolic light stabilizer. Non-limitingly, the mass ratio of the light stabilizer to the isomerized polyimide resin can be (0.14-0.16):5, and can also be any of the following ratios or a ratio range selected from any two of the following ratios: 0.14:5, 0.15:5, 0.16:5, etc.

[0127] In a non-limiting manner, in the negative photosensitive polyimide photoresist, the organic solvent may be selected from one or more of N-methylpyrrolidone, γ-butyrolactone, dimethyl sulfoxide, N,N-dimethylformamide, etc., but is not limited thereto. In some embodiments, the mass ratio of the isomerized polyimide resin to the organic solvent may be 5:(12-18), or may be any of the following ratios or a ratio range consisting of any two of the following ratios: 5:12, 5:13, 5:14, 5:15, 5:16, 5:17, 5:18, etc.

[0128] In some embodiments, the mass ratio of the isomerized polyimide resin, the photoinitiator, the photocrosslinker, the silane coupling agent, the light stabilizer, the low-temperature curing accelerator and the solvent can be 5: (0.18-0.22): (1.2-2): (0.14-0.16): (0.14-0.16): (12-18). Among them, the mass ratio of any one of the photoinitiator, the photocrosslinker, the silane coupling agent, the light stabilizer, the low-temperature curing accelerator and the solvent relative to the isomerized polyimide resin can also refer to other descriptions in the context, and can be combined in a suitable manner. For example, when the mass ratio of the photoinitiator to the isomerized polyimide resin is 0.2:5, the above ratio can correspond to 5:0.2: (1.2-2): (0.14-0.16): (0.14-0.16): (12-18).

[0129] In a second aspect of the present application, a method for preparing a negative photosensitive polyimide photoresist is provided, which can be used to prepare the negative photosensitive polyimide photoresist described in the first aspect of the present application.

[0130] In some embodiments, a method for preparing a negative photosensitive polyimide photoresist is provided, comprising the following steps: according to the components contained in the negative photosensitive polyimide photoresist of the first aspect of the present application, an isomerized polyimide resin, a photoinitiator, a photocrosslinker, a silane coupling agent, a light stabilizer, a low-temperature curing accelerator and an organic solvent are mixed to obtain a negative photosensitive polyimide photoresist.

[0131] In some embodiments, the isomerized polyimide resin is prepared by a method comprising the following steps:

[0132] S100: in anhydrous and oxygen-free and continuous dispersion conditions, aromatic diamine monomers and aromatic dianhydride monomers are mixed in a polymerization solvent at a suitable molar ratio (for example, a molar ratio of 0.9:1 to 1:0.9), and polymerization is carried out at a suitable polymerization temperature (for example, 0° C. to 100° C.) to generate a polyamic acid chain (optionally, the polymerization reaction time may be 6 h to 8 h), and end-capping molecules are added, and end-capping reaction is carried out at a suitable end-capping temperature (for example, 0° C. to 100° C.) (optionally, the end-capping reaction time may be 1 h to 2 h), to obtain a first mixed solution containing a polyamic acid intermediate;

[0133] S200: adding a dehydrating agent and a catalyst to the first mixed solution, performing a dehydration reaction at a suitable dehydration temperature (e.g., 0°C to 50°C) (optionally, the dehydration reaction time may be 1.5h to 2.5h) to generate an isomerized polyamic acid, adding a photosensitive tertiary amine small molecule containing R3, performing a salt-forming reaction under light-shielding and suitable salt-forming temperature (e.g., 0°C to 50°C) conditions (optionally, the salt-forming reaction time may be 3h to 5h), and obtaining a second mixed solution; wherein R3 is -L1-OC(=O)-C(M)=CH2, L1 is C 1-6 Alkylene, M is H or methyl; optionally, the molar ratio of the dehydrating agent to the aromatic dianhydride monomer can be (0.01-1):1;

[0134] S300: mixing the second mixed liquid with an alcohol solvent to precipitate a polyimide salt, separating the solid from the liquid, collecting the solid phase, washing, and drying to obtain an isomerized polyimide resin.

[0135] In some embodiments, the isomerized polyimide resin is prepared by a method comprising the following steps:

[0136] S100: in anhydrous and oxygen-free and continuous dispersion conditions, aromatic diamine monomers and aromatic dianhydride monomers are mixed in a polymerization solvent at a suitable molar ratio (for example, a molar ratio of 0.9:1 to 1:0.9), and polymerization reaction is carried out at 0° C. to 100° C. (optionally, the polymerization reaction time may be 6 h to 8 h) to generate a polyamic acid chain, and end-capping molecules are added, and end-capping reaction is carried out at 0° C. to 100° C. (optionally, the end-capping reaction time may be 1 h to 2 h) to obtain a first mixed solution containing a polyamic acid intermediate;

[0137] S200: Add a dehydrating agent and a catalyst to the first mixed solution, perform a dehydration reaction at 0°C to 50°C (optionally, the dehydration reaction can be 1.5h to 2.5h) to generate an isomerized polyamic acid, add a photosensitive tertiary amine small molecule containing R3, perform a salt-forming reaction at 0°C to 50°C in a dark environment (optionally, the salt-forming reaction time can be 3h to 5h), and obtain a second mixed solution; wherein R3 is -L1-OC(=O)-C(M)=CH2, L1 is C1-6 Alkylene, M is H or methyl; the molar ratio of the dehydrating agent to the aromatic dianhydride monomer is (0.01-1):1;

[0138] S300: mixing the second mixed liquid with an alcohol solvent to precipitate a polyimide salt, separating the solid from the liquid, collecting the solid phase, washing, and drying to obtain an isomerized polyimide resin;

[0139] in,

[0140] The structure of aromatic diamine monomer is

[0141] The structure of aromatic dianhydride monomer is

[0142] The polyamic acid chain has a chain structure shown in formula (II-1): Wherein, each * represents a capping site;

[0143] The structure of the polyamic acid intermediate is shown in formula (II-2):

[0144]

[0145] The structure of isomerized polyamic acid is shown in formula (II-3):

[0146]

[0147] In the aforementioned preparation method, the degree of imidization in the isomerized polyimide resin can be regulated by combining chemical imidization and thermal imidization to achieve partial imidization, thereby preparing the aforementioned isomerized polyimide resin (which is an ionic negative low-temperature curing photosensitive polyimide in which polyimide and polyamic acid salt coexist), and then obtaining a negative photosensitive polyimide photoresist that can be cured at a low temperature.

[0148] After step S100, a polyamic acid intermediate with exposed carboxyl groups (such as formula (II-2)) can be obtained, and then after step S200, part of the carboxyl groups are subjected to a dehydration reaction to form an imide (to obtain an isomerized polyamic acid, such as formula (II-3)), and then the un-bonded carboxyl groups are subjected to a salt-forming reaction to graft photosensitive tertiary amine small molecules to form an isomerized polyimide having a structure shown in formula (I).

[0149] A conventional polyimide preparation method can be used to obtain a polyamic acid solution containing polyamic acid chains, such as, for example, mixing aromatic diamine monomers with a polymerization solvent, mechanically stirring to dissolve the raw materials, adding aromatic dianhydride monomers, and performing polymerization to generate polyamic acid chains to obtain a polyamic acid solution.

[0150] In some embodiments, in the step of mixing the aromatic diamine monomer and the aromatic dianhydride monomer in a polymerization solvent, the molar ratio of the aromatic diamine monomer to the aromatic dianhydride monomer is 0.9:1 to 1:0.9, optionally 0.95:1 to 1:0.95, further optionally 0.98:1 to 1:0.98, and further optionally 0.99:1 to 1:0.99.

[0151] In some embodiments, in the step of mixing the aromatic diamine monomer and the aromatic dianhydride monomer in a polymerization solvent, the molar ratio of the aromatic diamine monomer to the aromatic dianhydride monomer is 1:1.

[0152] In some embodiments, the polymerization solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, sulfolane, butyrolactone, cresol and cyclohexanone. Further, the polymerization solvent can be selected from one or more of N-methylpyrrolidone, N,N-dimethylformamide and N,N-dimethylacetamide.

[0153] Without limitation, the temperature for carrying out the polymerization reaction may be 0°C to 100°C, further 0°C to 50°C, and may also be selected from any one of the following temperatures or from an interval consisting of any two of the following temperatures: 0°C, 4°C, 5°C, 6°C, 8°C, 10°C, 15°C, 16°C, 18°C, 20°C, 25°C, 26°C, 28°C, 30°C, 35°C, 40°C, 45°C, 50°C, 60°C, 70°C, 80°C, etc. The temperature for carrying out the polymerization reaction may also be any one of the following ranges: 0°C to 4°C, 0°C to 5°C, 0°C to 10°C, 0°C to 20°C, 0°C to 25°C, 0°C to 30°C, 0°C to 40°C, etc.

[0154] After the end-capping reaction, the polyamic acid chain is end-capped by the Ar3 group. The end-capping molecule can be Ar3-NH2, where Ar3 is an aromatic group. The definition of Ar3 can also be found in Ar 31 or Ar 32 In some embodiments, Ar3 is C 6-10Aromatic groups, further, can be 3-hydroxyphenyl, 2-hydroxyphenyl or 4-hydroxyphenyl, and further can be 3-hydroxyphenyl. The temperature for carrying out the end-capping reaction can be consistent with the temperature for carrying out the polymerization reaction. In a non-limiting manner, the temperature for carrying out the end-capping reaction can be 0°C to 100°C, and can further be 0°C to 50°C, and can also be selected from any of the following temperatures or from the interval consisting of any two of the following temperatures: 0°C, 4°C, 5°C, 6°C, 8°C, 10°C, 15°C, 16°C, 18°C, 20°C, 25°C, 26°C, 28°C, 30°C, 35°C, 40°C, 45°C, 50°C, 60°C, 70°C, 80°C, etc. The temperature for carrying out the end-capping reaction can also be any of the following ranges: 0°C to 4°C, 0°C to 5°C, 0°C to 10°C, 0°C to 20°C, 0°C to 25°C, 0°C to 30°C, 0°C to 40°C, etc.

[0155] In some embodiments, the polymerization reaction is conducted at the same temperature as the capping reaction.

[0156] The timing and amount of adding the end-capping molecule can be used to adjust the molecular weight of the isomerized polyimide resin. In a non-limiting manner, the molar ratio of the end-capping molecule to the aromatic dianhydride monomer can be 0.01 to 0.03, such as 0.01, 0.015, 0.016, 0.018, 0.02, 0.022, 0.024, 0.025, 0.026, 0.028, 0.03, etc.

[0157] The step S200 includes: performing a chemical imidization reaction and a salt-forming reaction of the grafted photosensitive tertiary amine small molecule.

[0158] In some embodiments, the dehydrating agent is C 4-12 One or more of aliphatic anhydrides (such as acetic anhydride), xylene, etc. 4-12 The aliphatic anhydride may include acetic anhydride. Acetic anhydride is a C4 aliphatic anhydride. In some embodiments, the dehydrating agent is one or more of acetic anhydride, xylene, etc.

[0159] In some embodiments, the catalyst is one or more of triethylamine, pyridine, N,N-diisopropylethylamine, and the like.

[0160] Without limitation, the dehydrating agent may be C 4-12 The catalyst may be one of an aliphatic anhydride (such as acetic anhydride) and xylene, and may further be acetic anhydride. In a non-limiting manner, the catalyst may be one of triethylamine and pyridine, and may further be triethylamine. In some embodiments, the dehydrating agent is C 4-12One of aliphatic anhydride (such as acetic anhydride) and xylene, and the catalyst is one of triethylamine and pyridine. The molar ratio of the dehydrating agent, the catalyst and the aromatic dianhydride monomer can be (0.1-1): (0.1-1): 1, but not limited thereto. The molar ratio of the dehydrating agent and the aromatic dianhydride monomer can also be any of the following ratios or a ratio range selected from any two of the following ratios: 0.1:1, 0.2:1, 0.25:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.66:1, 0.67:1, 2 / 3:1, 0.75:1, 0.8:1, 0.9:1, 1:1, etc. The temperature for the dehydration reaction can be 0°C to 50°C, further 0°C to 10°C, further ice bath conditions, and can also be selected from any one of the following temperatures or an interval consisting of any two of the following temperatures: 0°C, 4°C, 5°C, 6°C, 8°C, 10°C, 15°C, 16°C, 18°C, 20°C, 25°C, 26°C, 28°C, 30°C, 35°C, 40°C, 45°C, 50°C, etc. The temperature for the dehydration reaction can also be any one of the following ranges: 0°C to 4°C, 0°C to 5°C, 0°C to 10°C, 0°C to 20°C, 0°C to 25°C, 0°C to 30°C, 0°C to 40°C, etc.

[0161] In some embodiments, the dehydration reaction is performed in an ice bath.

[0162] In some embodiments, the dehydrating agent is acetic anhydride, the catalyst is triethylamine, and the temperature for the dehydration reaction is 0° C. to 50° C., or any suitable temperature mentioned above.

[0163] Through the salt-forming reaction, the photosensitive tertiary amine small molecule containing R3 can be grafted to the exposed carboxyl group in the isomerized polyamic acid to obtain a second mixed solution containing isomerized polyimide. The isomerized polyimide is a polyimide salt, and further a photosensitive polyimide quaternary ammonium salt. The structure of the isomerized polyimide can be shown in formula (I).

[0164] The photosensitive tertiary amine small molecule containing R3 can be the aforementioned In some further examples, the photosensitive tertiary amine small molecule is (2-(dimethylamino)ethyl methacrylate, wherein R1 and R2 are methyl, and R3 is -CH2CH2O-C(=O)-C(CH3)=CH2) and (2-(dimethylamino)ethyl acrylate, wherein R1 and R2 are methyl groups, and R3 is -CH2CH2O-C(=O)-CH=CH2), one or two thereof, or any one thereof. The temperature for the salt-forming reaction may be 0°C to 50°C, further 0°C to 10°C, further ice bath conditions, or any one of the following temperatures or an interval consisting of any two of the following temperatures: 0°C, 4°C, 5°C, 6°C, 8°C, 10°C, 15°C, 16°C, 18°C, 20°C, 25°C, 26°C, 28°C, 30°C, 35°C, 40°C, 45°C, 50°C, etc. The temperature for the salt-forming reaction may also be any one of the following ranges: 0°C to 4°C, 0°C to 5°C, 0°C to 10°C, 0°C to 20°C, 0°C to 25°C, 0°C to 30°C, 0°C to 40°C, etc.

[0165] In some embodiments, the salt-forming reaction is performed in an ice bath.

[0166] Without limitation, the molar ratio of the photosensitive tertiary amine small molecule containing R3 to the aromatic dianhydride monomer can be 1.5 to 2.5, such as 1.5, 1.6, 1.8, 2, 2.0, 2.2, 2.4, 2.5, etc., and can also be an interval consisting of any two of the aforementioned values.

[0167] The isomerized polyimide (a polyimide salt) can be precipitated from the polymerization system using an alcohol solvent. 1-6 Alkyl alcohol. 1-6 The alkyl alcohol may include methanol. In some embodiments, the alcohol solvent is methanol.

[0168] In a non-limiting manner, in step S300, the drying method may be vacuum drying at 80°C to 250°C. The drying temperature may also be 80°C to 200°C, further 80°C to 150°C, and further 80°C to 100°C. The drying temperature may also be any of the following temperatures or a range consisting of any two of the following temperatures: 80°C, 90°C, 100°C, 120°C, 140°C, 150°C, 160°C, 180°C, 200°C, 220°C, 240°C, 250°C, etc.

[0169] In step S300 , thermal imidization may occur, and the degree of imidization may be further finely adjusted to obtain an isomerized polyimide resin having a target m value.

[0170] Since the curing temperature of conventional PSPI is generally above 300°C, in order to meet the requirements of low-temperature curing of PSPI, relevant preparation methods need to be designed. The preparation methods of low-temperature curing PSPI mainly include the following: synthesizing soluble PI resin, optimizing PI molecular structure and formula, and catalyzing polyamic acid (PAA) reaction.

[0171] In another aspect of the present application, a method for preparing an isomerized polyimide resin is provided. The definition of the isomerized polyimide resin can be found in the first and second aspects of the present application. The method for preparing the isomerized polyimide resin can be found in the second aspect of the present application.

[0172] In the third aspect of the present application, a polyimide film is provided, which is formed by curing the negative photosensitive polyimide photoresist described in the first aspect of the present application, or by curing the negative photosensitive polyimide photoresist prepared by the preparation method described in the second aspect of the present application; the curing temperature may be lower than or equal to 250° C. Optionally, the curing temperature may include 200° C. to 250° C., and further optionally, the curing temperature may include one or more temperatures in the range of 200° C. to 250° C.

[0173] In another aspect of the present application, a method for preparing the polyimide film is also provided, which can be referred to the relevant description in the context.

[0174] In another aspect of the present application, a photoresist cured film is provided, which is formed by curing the negative photosensitive polyimide photoresist described in the first aspect of the present application, or by curing the negative photosensitive polyimide photoresist prepared by the preparation method described in the second aspect of the present application. The curing temperature may be lower than or equal to 250°C. Alternatively, the curing temperature may include 200°C to 250°C, and further optionally, the curing temperature may include one or more temperatures in the range of 200°C to 250°C.

[0175] In another aspect of the present application, a method for preparing the above-mentioned photoresist cured film is also provided. Please refer to the relevant description above.

[0176] The negative photosensitive polyimide photoresist can be exposed and cured to obtain a polyimide film or a photoresist cured film. The exposure energy for exposure can be 750mJ / cm 2 ~850mJ / cm 2 , such as 800mJ / cm 2 . Curing can be performed in an inert atmosphere. Without limitation, curing can be performed under nitrogen atmosphere conditions. In some embodiments, curing is performed under nitrogen atmosphere conditions at a curing temperature of less than or equal to 250° C. For example, curing can be performed at a curing temperature of 100° C. to 250° C. Optionally, the curing temperature may include 200° C. to 250° C. The curing temperature can also be referred to in the context of the present application, such as the fourth aspect of the present application.

[0177] In another aspect of the present application, a polyimide micron pattern is provided, which can be obtained by exposing, developing and curing a negative photosensitive polyimide photoresist. The implementation methods of exposure, development and curing can refer to the fourth aspect of the present application.

[0178] In another aspect of the present application, a method for preparing the polyimide micron pattern is also provided, which can be referred to the relevant description in the context.

[0179] In the present application, unless otherwise specified, "micrometer pattern" refers to a pattern with a micrometer-level topological structure, wherein the topological structure has micrometer-scale patterns or pattern intervals. "Micrometer level" or "micrometer scale", unless otherwise specified, generally refers to a size in the range of 0.1 micrometer (μm) to 1000 micrometers, for example, a size in the range of 1 micrometer (μm) to 1000 micrometers, and another example is a size in the range of 0.1 micrometer to 100 micrometers.

[0180] The polyimide film or photoresist cured film formed by low temperature curing (such as curing temperature ≤ 250°C) of the aforementioned negative photosensitive polyimide photoresist has a high glass transition temperature and thermal stability. When the negative photosensitive polyimide is used to prepare a polyimide micro pattern, a high-resolution polyimide pattern can be obtained. In addition, taking the plastic encapsulation device process as an example, during the low temperature curing process of the negative photosensitive polyimide photoresist, wafer warping can be avoided or suppressed, and cracking, shedding, recrystallization and other problems of the solder joints of the low-melting solder can also be avoided or suppressed, thereby significantly improving the performance of the plastic encapsulation device.

[0181] In a fourth aspect of the present application, there is provided the use of the negative photosensitive polyimide photoresist described in the first aspect of the present application or the negative photosensitive polyimide photoresist prepared by the preparation method described in the second aspect of the present application in preparing a polyimide micro pattern.

[0182] The negative photosensitive polyimide photoresist can be exposed, developed, and cured to obtain a polyimide micro pattern. The negative photosensitive polyimide photoresist can be spin-coated to form a coating liquid, and then pre-baked at a pre-baking temperature lower than the curing temperature (such as pre-baking at 100° C. to 120° C.) to form a photosensitive film, exposed and developed to form a pattern, and then cured at a curing temperature (such as ≤250° C., further such as 100° C. to 250° C.) to obtain a polyimide pattern. The substrate for spin coating can be a silicon wafer, but is not limited thereto. The organic solvent in the photoresist is volatilized by pre-baking to obtain a dry photosensitive film.

[0183] In some embodiments, the application includes the following steps: drying the negative photosensitive polyimide photoresist at a pre-baking temperature (such as 100° C. to 120° C.) to form a photosensitive film, exposing, developing, cleaning, and curing at a curing temperature (such as ≤250° C.).

[0184] The drying time at the pre-drying temperature can be 2 minutes to 4 minutes, such as 3 minutes.

[0185] The exposure energy for exposure can be 750mJ / cm 2 ~850mJ / cm 2 , such as 800mJ / cm 2 .

[0186] The developer used for development may be an alkaline aqueous solution, such as a tetramethylammonium hydroxide (TMAH) aqueous solution, and further may be a 0.25 wt % TMAH aqueous solution.

[0187] After the development is completed, washing is performed to remove residual reagents. The liquid used for washing can be water, such as deionized water.

[0188] The curing may be performed in an inert atmosphere. Without limitation, the curing may be performed in a nitrogen atmosphere.

[0189] In some embodiments, curing is performed under nitrogen atmosphere at a curing temperature lower than or equal to 250° C., and optionally, at a curing temperature lower than or equal to 200° C. The curing temperature can also refer to the relevant description in the context of this application.

[0190] In some embodiments, curing is performed at a curing temperature of 100°C to 250°C.

[0191] In some embodiments, the curing temperature is 100°C to 250°C, optionally 100°C to 200°C.

[0192] In some embodiments, the curing temperature is one or more temperatures in the range of 100°C to 250°C, and may be one or more temperatures in the range of 100°C to 200°C.

[0193] In some embodiments, the curing temperature is one or more temperatures in the range of 100°C to 250°C. Further, the curing temperature may include one or more temperatures in the range of 200°C to 250°C.

[0194] In some embodiments, the curing temperature includes one or more temperatures between 100°C and 150°C, and includes one or more temperatures between 200°C and 250°C.

[0195] In some embodiments, the curing temperature includes a first curing temperature T1 and a second curing temperature T2, and optionally, 100≤T1<150°C, 200≤T2≤250°C.

[0196] In some embodiments, the curing temperature includes a first curing temperature T1, a second curing temperature T2, and a third curing temperature T3. Optionally, 100≤T1<150°C, 200≤T2≤250°C, and 150≤T3<200°C.

[0197] In some embodiments, the curing temperature is lower than or equal to 200°C, and further, the curing temperature is one or more temperatures between 100°C and 200°C.

[0198] During curing, the curing temperature may be a constant temperature, or different temperatures may be used within the aforementioned curing temperature range for segmented curing.

[0199] In some embodiments, the curing temperature includes at least 100° C. and 200° C. In some embodiments, the curing temperature includes 100° C., 150° C. and 200° C., and further, each curing temperature can be cured for 1 hour respectively. In some embodiments, the curing temperature is 100° C., 150° C. and 200° C. for 1 hour respectively.

[0200] In some embodiments, the curing temperature includes 100°C and 250°C. In some embodiments, the curing temperature includes 100°C, 150°C, 200°C and 250°C, and further, each curing temperature can be cured for 1 hour. In some embodiments, the curing temperature is 100°C, 150°C, 200°C and 250°C for 1 hour.

[0201] In some embodiments, the curing temperature includes 200°C and 250°C.

[0202] In some embodiments, a step-by-step temperature curing method is adopted. One or more heat preservation platforms may be set in the curing process, and each heat preservation platform is continuous (that is, curing is carried out without interruption); optionally, each heat preservation platform can be carried out in sequence from low to high according to the curing temperature. In some embodiments, the temperature of any heat preservation platform is less than or equal to 250°C, and optionally, the temperature of any heat preservation platform is less than or equal to 200°C. In some embodiments, the temperature of any heat preservation platform is selected from 100°C to 250°C, and optionally, the temperature of any heat preservation platform is selected from 100°C to 200°C. In some embodiments, the curing process includes the following heat preservation platforms: (100±ΔT1)°C, (150±ΔT2)°C, and (200±ΔT3)°C. In some embodiments, the curing process includes the following heat preservation platforms: (100±ΔT1)°C, (150±ΔT2)°C, (200±ΔT3)°C, and (250±ΔT4)°C. ΔT1, ΔT2 and ΔT3 can each independently be a value selected from 0 to 5, non-limiting examples such as 0, 0.5, 1, 1.5, 2, 2.5, 3, 4, 5, etc. ΔT4 can be a value selected from 0 to 10, non-limiting examples such as 0, 0.5, 1, 1.5, 2, 2.5, 3, 4, 5, 6, 7, 8, 9, 10, etc. The insulation time of each insulation platform can be, but is not limited to, 0.5h to 1.5h, such as 1h. In some embodiments, the curing process includes: heat treatment at 100°C, 150°C and 200°C for 1h respectively. In some embodiments, the curing process includes: heat treatment at 100°C, 150°C, 200°C and 250°C for 1h respectively. In some embodiments, the insulation platform is (100±ΔT1)°C, (150±ΔT2)°C and (200±ΔT3)°C. In some embodiments, the insulation platform is (100±ΔT1)°C, (150±ΔT2)°C, (200±ΔT3)°C, and (250±ΔT4)°C. In some embodiments, the insulation platform includes 100°C and 200°C. In some embodiments, the insulation platform includes 200°C and 250°C. In some embodiments, the insulation platform includes 100°C and 250°C. In some embodiments, the insulation platform includes 100°C, 150°C, and 200°C. In some embodiments, the insulation platform includes 100°C, 150°C, 200°C, and 250°C.

[0203] In some embodiments, the application described in the fourth aspect of the present application includes application in microelectronic packaging; wherein the microelectronic packaging includes at least one of a fan-out wafer-level packaging and a fan-out flat-panel-level packaging.

[0204] The low temperature curing negative photosensitive polyimide photoresist provided in the present application can be widely used to prepare micron patterns. As one of the non-limiting application modes, it can be applied to the field of microelectronic packaging, including but not limited to fan-out wafer level packaging (FOWLP) and fan-out flat panel packaging (FOPLP).

[0205] The embodiments of the present application will be described in detail below in conjunction with some examples. It should be understood that these examples are only used to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which the conditions are not specified in the following examples are preferably referred to the guidance given in the present application, and can also be based on the experimental manual or normal conditions in the art, or can also be based on the conditions recommended by the manufacturer, or with reference to experimental methods known in the art.

[0206] 1. Preparation and testing of isomerized polyimide resin and photoresist

[0207] Example 1.

[0208] (1) Preparation of isomerized polyimide resin (negative photosensitive resin).

[0209] In this example, the aromatic dianhydride monomer is ODPA, the aromatic diamine monomer is ODA, the polymerization solvent is N,N'-dimethylacetamide, the end-capping molecule is m-aminophenol, the dehydrating agent is acetic anhydride, the catalyst is triethylamine, the photosensitive tertiary amine small molecule is 2-(dimethylamino)ethyl methacrylate, and the alcohol solvent is methanol.

[0210] Under anhydrous and oxygen-free conditions, 20.02 g (0.1 mol) of 4,4'-diaminodiphenyl ether diamine (ODA) was added and dissolved in 200 g of N,N'-dimethylacetamide. 31.02 g (0.1 mol) of 4,4'-oxydiphthalic anhydride (ODPA) was slowly added while stirring continuously in an ice bath. The reaction was carried out for 6 h until the solution became stable and viscous. Then, 0.2183 g (2 mmol) of m-aminophenol was added and the reaction was continued for 1 h (end-capping reaction) to generate a polyamic acid intermediate.

[0211] Add 5.10g (0.05mol) of acetic anhydride and 5.06g (0.05mol) of triethylamine to the polymerization reaction system, react for 2h (dehydration reaction to achieve partial imidization) to generate isomerized polyamic acid; then add 31.44g (0.2mol) of 2-(dimethylamino)ethyl methacrylate to the solution, and continue to react for 3h under light-proof conditions (salt-forming reaction) to generate isomerized polyimide. After stopping the reaction, pour the solution into a large amount of methanol solution while stirring continuously to precipitate, and filter the precipitated solid, wash with ultrapure water, and then place it in a vacuum oven at 80°C for 12h to obtain an isomerized polyimide resin (also recorded as negative photosensitive resin), in which the isomerized polyimide molecules are polyamic acid salts.

[0212] (2) Preparation of negative photosensitive polyimide photoresist.

[0213] In this example, 2-hydroxy-2-methylpropiophenone is a photoinitiator, tetraethylene glycol dimethacrylate is a photocrosslinker, diphenyl dihydroxysilane is a silane coupling agent, 2,6-di-tert-butyl-p-cresol is a light stabilizer, and isoquinoline is a low-temperature curing accelerator. A silicon wafer is used as a substrate for preparing a cured film.

[0214] The negative photosensitive resin prepared in step (1) is dissolved in N-methylpyrrolidone (organic solvent), and a photoinitiator, a photocrosslinker, a silane coupling agent, a light stabilizer and a low-temperature curing accelerator are added and mixed into a solution to prepare a photoresist (also referred to as a photoresist solution), wherein the photoresist is a negative photosensitive polyimide photoresist; wherein the mass ratio of the negative photosensitive resin, the photoinitiator, the photocrosslinker, the silane coupling agent, the light stabilizer, the low-temperature curing accelerator and the organic solvent is 5:0.2:1.5:0.15:0.01:0.1:15.

[0215] (3) Photolithography (exposure), development, and optical microscope observation.

[0216] The photoresist prepared in step (2) was spin-coated on the surface of the silicon wafer, pre-baked at 120°C for 3 minutes to form a photosensitive film layer, and then placed on a broad spectrum exposure machine for photolithography with an exposure energy of 800 mJ / cm 2 Then, a 0.25 wt % tetramethylammonium hydroxide aqueous solution (TMAH aqueous solution) was used as a developer, and the film was developed for 15 seconds, and then washed with deionized water to obtain a developed pattern, which was a polyimide pattern.

[0217] The photolithographic resolution of the cured film was measured using an optical microscope (Axiolab 5). Figure 1 As shown, the resolution results of the pattern layer can be referred to Table 1. In the pattern area, the stripe width is 5 μm to 25 μm, and the stripe spacing is 5 μm to 25 μm. In the pattern area of ​​this example, the stripe width is equal to the stripe spacing.

[0218] (4) Photolithography (exposure), development, curing, and mechanical properties testing

[0219] The photoresist solution prepared in step (2) was spin-coated on the surface of the silicon wafer, pre-baked at 120°C for 3 minutes to form a photosensitive film layer, and then placed on a broad spectrum exposure machine for photolithography at an exposure energy of 800 mJ / cm 2, put the exposed silicon wafer into a high temperature oven, and heat it up at a heating rate of 5°C / min in a nitrogen atmosphere, and cure it at 100°C, 150°C, and 200°C for 1 hour each. Post-treatment: The resin film obtained after curing is immersed in a 4.9 vol% hydrofluoric acid solution for 30 minutes, and after drying, a cured resin film (a photoresist cured film, which is a polyimide film) with a thickness of 10 μm is obtained.

[0220] The tensile strength and elongation at break of the cured resin film were tested using a universal tensile testing machine at 25°C and 60RH according to the JIS-K6251 standard. The specimen was in the shape of a strip with a width of 10 mm and a length of 50 mm. The test rate was 10 mm / min. Five samples of the same batch of cured resin film were prepared and measured five times, and the average value was taken. The test results can be found in Table 1.

[0221] Tensile strength: refers to the maximum tensile stress that a specimen can withstand when it breaks or ruptures.

[0222] Elongation at break is calculated according to the above JIS-K6251 standard: E b =(L b -L0) / L0×100;

[0223] Among them, E b is the elongation at break (%), L0 is the initial length of the sample, L b is the length at rupture.

[0224] Example 2.

[0225] (1) Preparation of isomerized polyimide resin (negative photosensitive resin).

[0226] Under anhydrous and oxygen-free conditions, 21.23 g (0.1 mol) of 4,4'-diamino-2,2'-dimethylbiphenyl (M-Tolidine) was added and dissolved in 130 g of N,N'-dimethylacetamide. 21.82 g (0.1 mol) of phthalic anhydride (PMDA) was slowly added while stirring in an ice bath. The reaction was continued for 8 hours until the solution became stable and viscous. Then 0.2183 g (2 mmol) of m-aminophenol was added and the reaction was continued for 1 hour. 1.02 g (0.01 mol) of acetic anhydride and 1.01 g (0.01 mol) of triethylamine were added to the polymerization reaction system and the reaction was continued for 2 hours. Then 28.64 g (0.2 mol) of 2-(dimethylamino)ethyl acrylate was added to the solution and the reaction was continued for 3 hours under light-proof conditions. After stopping the reaction, the solution was poured into a large amount of methanol solution for precipitation while continuously stirring, and the precipitated solid was filtered, washed with ultrapure water, and then placed in a vacuum oven at 80° C. for drying for 12 h to obtain a negative photosensitive resin (polyamic acid salt).

[0227] (2) Preparation of negative photosensitive polyimide photoresist.

[0228] The negative photosensitive resin prepared in step (1) is dissolved in N-methylpyrrolidone (organic solvent), and a photoinitiator, a photocrosslinker, a silane coupling agent, a light stabilizer and a low-temperature curing accelerator are added, and mixed into a solution to prepare a photoresist; wherein the mass ratio of the negative photosensitive resin, the photoinitiator, the photocrosslinker, the silane coupling agent, the light stabilizer and the low-temperature curing accelerator to the organic solvent is 5:0.2:1.2:0.15:0.01:0.5:15; Michler's ketone (MK) is the photoinitiator, tetraethylene glycol dimethacrylate is the photocrosslinker, γ-aminopropyltriethoxysilane is the silane coupling agent, 1-nitroso-2-naphthol is the light stabilizer, and isoquinoline is the low-temperature curing accelerator.

[0229] (3) Photolithography, development, and optical microscope observation.

[0230] The photoresist prepared in step (2) was used for photolithography and development in the same manner as in Example 1, and then observed under an optical microscope. The optical microscope image of the developed pattern in Example 2 is shown in FIG. Figure 2 As shown, the resolution results of the graphics layer can be found in Table 1.

[0231] (4) Photolithography, development, curing, and mechanical properties testing.

[0232] The photoresist solution prepared in step (2) was spin-coated on the surface of the silicon wafer, pre-baked at 120°C for 3 minutes to form a photosensitive film layer, and then placed on a broad spectrum exposure machine for photolithography at an exposure energy of 800 mJ / cm 2 , put the exposed silicon wafer into a high temperature oven, and heat it up at a heating rate of 5°C / min in a nitrogen atmosphere, and cure it at 100°C, 150°C, 200°C, and 250°C for 1 hour each. Post-treatment: The cured resin film was immersed in a 4.9 vol% hydrofluoric acid solution for 30 minutes, and dried to obtain a cured resin film with a thickness of 10 μm.

[0233] The tensile strength and elongation at break were tested using the same method as in Example 1. The test results can be found in Table 1.

[0234] Example 3.

[0235] (1) Preparation of isomerized polyimide resin (negative photosensitive resin).

[0236] Under anhydrous and oxygen-free conditions, 41.05 g (0.1 mol) of 2,2'-bis[4-(4-aminophenoxyphenyl)]propane (BAPP) was added to 130 g of N,N'-dimethylformamide (DMF) to dissolve. 29.42 g (0.1 mol) of 3,3,4,4-biphenyltetracarboxylic dianhydride (BPDA) was slowly added while stirring in an ice bath. The reaction was continued for 8 hours until the solution became stable and viscous. Then, 0.2183 g (2 mmol) of m-aminophenol was added and the reaction was continued for 1 hour. 10.21 g (0.1 mol) of acetic anhydride and 10.12 g (0.1 mol) of triethylamine were added to the polymerization reaction system and the reaction was continued for 2 hours. Then, 31.44 g (0.2 mol) of 2-(dimethylamino)ethyl methacrylate was added to the solution and the reaction was continued for 3 hours under light-proof conditions. After stopping the reaction, the solution was poured into a large amount of methanol solution for precipitation while being continuously stirred, and the precipitated solid was filtered, washed with ultrapure water, and then placed in a vacuum oven at 80° C. for drying for 12 h to obtain a polyamic acid salt.

[0237] (2) Preparation of negative photosensitive polyimide photoresist.

[0238] The negative photosensitive resin prepared in step (1) is dissolved in N-methylpyrrolidone (organic solvent), and a photoinitiator, a photocrosslinker, a silane coupling agent, a light stabilizer and a low-temperature curing accelerator are added, and mixed into a solution to prepare a photoresist. The mass ratio of the negative photosensitive resin, the photoinitiator, the photocrosslinker, the silane coupling agent, the light stabilizer, the low-temperature curing accelerator and the organic solvent is 5:0.2:2:0.15:0.01:0.3:15; 2-hydroxy-2-methylpropiophenone is a photoinitiator, tetraethylene glycol dimethacrylate is a photocrosslinker, diphenyl dihydroxysilane is a silane coupling agent, 2,6-di-tert-butyl-p-cresol is a light stabilizer, and isoquinoline is a low-temperature curing accelerator.

[0239] (3) Photolithography, development, and optical microscope observation.

[0240] The photoresist prepared in step (2) was used for photolithography and development in the same manner as in Example 1, and then observed under an optical microscope.

[0241] (4) Photolithography, development, curing, and mechanical properties testing.

[0242] The photoresist solution prepared in step (2) was used to perform photolithography, development, curing and post-treatment in the same manner as in Example 1. The mechanical properties test was performed in the same manner as in Example 1 to obtain tensile strength and elongation at break. The test results can be found in Table 1.

[0243] Example 4.

[0244] (1) Preparation of isomerized polyimide resin (negative photosensitive resin).

[0245] Under anhydrous and oxygen-free conditions, 20.02 g (0.1 mol) of 3,3'-diaminodiphenyl sulfone (3,3'-DDS) was added to 130 g of N-methylpyrrolidone (NMP) to dissolve. 32.22 g (0.1 mol) of 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA) was slowly added while stirring in an ice bath. The reaction was continued for 8 hours until the solution became stable and viscous. Then 0.2183 g (2 mmol) of m-aminophenol was added and the reaction was continued for 1 hour. 2.04 g (0.02 mol) of acetic anhydride and 2.02 g (0.02 mol) of triethylamine were added to the polymerization reaction system and the reaction was continued for 2 hours. Then 31.44 g (0.2 mol) of 2-(dimethylamino)ethyl methacrylate was added to the solution and the reaction was continued for 3 hours under light-proof conditions. After stopping the reaction, the solution was poured into a large amount of methanol solution for precipitation while being continuously stirred, and the precipitated solid was filtered, washed with ultrapure water, and then placed in a vacuum oven at 80° C. for drying for 12 h to obtain a polyamic acid salt.

[0246] (2) Preparation of negative photosensitive polyimide photoresist.

[0247] The negative photosensitive resin prepared in step (1) is dissolved in N-methylpyrrolidone (organic solvent), and a photoinitiator, a photocrosslinker, a silane coupling agent, a light stabilizer and a low-temperature curing accelerator are added, and the mixture is mixed to form a solution to prepare a photoresist; wherein the mass ratio of the negative photosensitive resin, the photoinitiator, the photocrosslinker, the silane coupling agent, the light stabilizer, the low-temperature curing accelerator and the organic solvent is 5:0.2:1.2:0.15:0.01:0.3:15; 2-hydroxy-2-methylpropiophenone is the photoinitiator, tetraethylene glycol dimethacrylate is the photocrosslinker, diphenyl dihydroxysilane is the silane coupling agent, 2,6-di-tert-butyl-p-cresol is the light stabilizer, and pyridine is the low-temperature curing accelerator.

[0248] (3) Photolithography, development, and optical microscope observation.

[0249] The photoresist prepared in step (2) was used for photolithography and development in the same manner as in Example 2, and then observed under an optical microscope.

[0250] (4) Photolithography, development, curing, and mechanical properties testing.

[0251] The photoresist solution prepared in step (2) was used to perform photolithography, development, curing and post-treatment in the same manner as in Example 2, and the mechanical properties test was performed in the same manner as in Example 1 to obtain tensile strength and elongation at break. The test results can be found in Table 1.

[0252] Example 5.

[0253] (1) Preparation of isomerized polyimide resin (negative photosensitive resin).

[0254] Under anhydrous and oxygen-free conditions, 29.23 g (0.1 mol) of 1,4-bis(4-aminophenoxy)benzene (TPE-Q) was added to 130 g of N-methylpyrrolidone (NMP) to dissolve. 29.42 g (0.1 mol) of 3,3,4,4-biphenyltetracarboxylic dianhydride (BPDA) was slowly added while stirring in an ice bath. The reaction was continued for 8 hours until the solution became stable and viscous. Then, 0.2183 g (2 mmol) of m-aminophenol was added and the reaction was continued for 1 hour. 8.17 g (0.08 mol) of acetic anhydride and 8.10 g (0.08 mol) of triethylamine were added to the polymerization reaction system. The reaction was continued for 2 hours. Then, 31.44 g (0.2 mol) of 2-(dimethylamino)ethyl methacrylate was added to the solution. The reaction was continued for 3 hours under light-proof conditions. After stopping the reaction, the solution was poured into a large amount of methanol solution for precipitation while being continuously stirred, and the precipitated solid was filtered, washed with ultrapure water, and then placed in a vacuum oven at 80° C. for drying for 12 h to obtain a polyamic acid salt.

[0255] (2) Preparation of negative photosensitive polyimide photoresist.

[0256] The negative photosensitive resin prepared in step (1) is dissolved in N-methylpyrrolidone (organic solvent), and a photoinitiator, a photocrosslinker, a silane coupling agent, a light stabilizer and a low-temperature curing accelerator are added, and mixed into a solution to prepare a photoresist; wherein the mass ratio of the negative photosensitive resin, the photoinitiator, the photocrosslinker, the silane coupling agent, the light stabilizer, the low-temperature curing accelerator and the organic solvent is 5:0.2:1.5:0.15:0.01:0.3:15. 2-Hydroxy-2-methylpropiophenone is a photoinitiator, tetraethylene glycol dimethacrylate is a photocrosslinker, diphenyl dihydroxysilane is a silane coupling agent, 2,6-di-tert-butyl-p-cresol is a light stabilizer, and isoquinoline is a low-temperature curing accelerator.

[0257] (3) Photolithography, development, and optical microscope observation.

[0258] The photoresist prepared in step (2) was used for photolithography and development in the same manner as in Example 2, and then observed under an optical microscope.

[0259] (4) Photolithography, development, curing, and mechanical properties testing.

[0260] The photoresist solution prepared in step (2) was used to perform photolithography, development, curing and post-treatment in the same manner as in Example 2, and the mechanical properties test was performed in the same manner as in Example 1 to obtain tensile strength and elongation at break. The test results can be found in Table 1.

[0261] Comparative Example 1. Omit the dehydrating agent and the catalyst.

[0262] The isomerized polyimide resin (negative photosensitive resin) and the negative photosensitive polyimide photoresist are prepared by the same method as in Example 1, except that acetic anhydride and triethylamine are not added in step (1). Steps (2), (3) and (4) are the same as in Example 1.

[0263] Comparative Example 2: Omitting the low temperature curing accelerator.

[0264] The isomerized polyimide resin (negative photosensitive resin) and the negative photosensitive polyimide photoresist are prepared by the same method as in Example 1, except that no low temperature curing accelerator is added in step (2). Steps (1), (3) and (4) are the same as in Example 1.

[0265] Comparative Example 3: Omitting the photosensitive tertiary amine small molecule

[0266] The isomerized polyimide resin (negative photosensitive resin) and the negative photosensitive polyimide photoresist are prepared by a method substantially the same as that in Example 1, except that the step of salt-forming reaction of the photosensitive tertiary amine small molecule is omitted in step (1).

[0267] (1) Under anhydrous and oxygen-free conditions, 20.02 g (0.1 mol) of 4,4'-diaminodiphenyl ether diamine (ODA) was added and dissolved in 200 g of N,N'-dimethylacetamide. 31.02 g (0.1 mol) of 4,4'-oxydiphthalic anhydride (ODPA) was slowly added while stirring in an ice bath. The reaction was continued for 6 h until the solution became stable and viscous. Then, 0.2183 g (2 mmol) of m-aminophenol was added and the reaction was continued for 1 h (capping reaction) to generate a polyamic acid intermediate.

[0268] Add 5.10g (0.05mol) of acetic anhydride and 5.06g (0.05mol) of triethylamine to the polymerization reaction system, and react for 2h (dehydration reaction to achieve partial imidization) to generate isomerized polyamic acid. After stopping the reaction, pour the solution into a large amount of methanol solution while stirring continuously to precipitate, and filter the precipitated solid, wash it with ultrapure water, and then place it in a vacuum oven at 80°C for drying for 12h to obtain isomerized polyamic acid resin (also recorded as negative photosensitive resin), in which the isomerized polyamic acid molecules are not grafted with photosensitive tertiary amine small molecules.

[0269] Steps (2), (3) and (4) are the same as in Example 1.

[0270] In the above embodiments and comparative examples, the thickness of the cured resin film obtained in step (4) is 10 μm.

[0271] 2. Test method:

[0272] 1. Structural analysis of isomerized polyimide resin

[0273] The isomerized polyimide resin in the embodiment has the structure shown in the above formula (I), wherein m and n are confirmed by the test analysis results of Fourier transform infrared spectroscopy (FT-IR) and gel permeation chromatography (GPC), respectively, and can be further confirmed by combining other structural analysis methods in the art. The test analysis results can be found in Table 1.

[0274] The FT-IR was tested by KBr pellet method. The solvent for GPC was tetrahydrofuran (other solvents such as N-methylpyrrolidone were allowed to be added or used to promote dissolution).

[0275] (1) The value of m in formula (I)

[0276] The m value corresponds to the degree of imidization

[0277] In the infrared spectrum, 1375cm -1 The absorption peak at 1720 cm-1 is attributed to the stretching vibration absorption peak of the carbon-nitrogen bond of the imide ring of polyimide. -1 1780cm -1 The absorption peaks at are all attributed to the symmetric stretching and asymmetric stretching vibration absorption peaks of the polyimide ring carbonyl group. The m value can be obtained by calculating the peak area integral ratio of the absorption peaks in the infrared absorption spectrum.

[0278] (2) The value of n in formula (I) and the average molecular weight of the isomerized polyimide resin

[0279] The value of n corresponds to the degree of polymerization of the isomerized polyimide resin.

[0280] After measuring the number average molecular weight using GPC, the structural unit is calculated based on the m value. The corresponding molecular weight can be converted to obtain the n value.

[0281] 2. Photosensitivity test: Use an optical microscope to measure the photolithography resolution. The instrument model is Axiolab 5.

[0282] 3. Glass transition temperature (Tg): DSC Perkin-Elmer DSC-7 was used to test polyimide film in a nitrogen atmosphere at a heating rate of 10°C / min.

[0283] The Tg of polyimide film can indirectly reflect the required curing temperature. A higher Tg of polyimide film means a higher curing temperature is required to prepare the film. A Tg that is too high (such as over 280°C) will result in poor low-temperature curing performance.

[0284] 4. Thermal gravimetric analysis (TGA): TGA Perkin-Elemer TGA-2 was used to test polyimide film in nitrogen atmosphere at 50°C to 700°C with a heating rate of 10°C / min.

[0285] The higher the thermal gravimetric loss temperature (TGA), the better the thermal stability.

[0286] 5. Tensile test

[0287] Please refer to the description of step (4) in Example 1.

[0288] The tensile strength and elongation at break of the cured resin film were tested using a universal tensile testing machine at 25°C and 60RH according to the JIS-K6251 standard. The specimen was in the shape of a strip with a width of 10 mm and a length of 50 mm. The test rate was 10 mm / min. Five samples of the same batch of cured resin film were prepared and measured five times, and the average value was taken.

[0289] The elongation at break is calculated according to the above standard: E b =(L b -L0) / L0×100;

[0290] Tensile strength: refers to the maximum tensile force that a specimen can withstand when it breaks or ruptures.

[0291] Elongation at break is calculated according to the above JIS-K6251 standard: E b =(L b -L0) / L0×100;

[0292] Among them, E b is the elongation at break (%), L0 is the initial length of the sample, L b is the length at rupture.

[0293] 3. Test results analysis

[0294] By introducing the isomerized polyimide resin, the negative photosensitive polyimide photoresist prepared in each of Examples 1-5 can be cured at a low temperature of ≤250°C and has good photosensitivity, and the prepared development pattern has a high resolution (5μm). In addition, the polyimide film obtained by using the negative photosensitive polyimide photoresist prepared in each of Examples 1-5 has a high glass transition temperature and thermal stability.

[0295] The polyimide films of Comparative Examples 1-3 have too high Tg, resulting in poor curing performance under low temperature conditions of ≤250° C., and the mechanical properties of the cured products decrease to varying degrees.

[0296] In Comparative Example 1, acetic anhydride and triethylamine were not added, that is, the chemical imidization process was omitted, and almost no chemical imidization reaction occurred. Then the value of m was close to 0, and the low-temperature curing performance was poor. The mechanical properties of the polyimide film cured under the low-temperature condition of ≤250 °C were significantly deteriorated, and both the tensile strength and the elongation at break were relatively low.

[0297] In Comparative Example 2, a low-temperature curing accelerator was not added, resulting in poor low-temperature curing performance. The mechanical properties of the polyimide film cured under the low-temperature condition of ≤250 °C were significantly deteriorated, and both the tensile strength and the elongation at break were relatively low.

[0298] In Comparative Example 3, the photosensitive tertiary amine small molecule was omitted, resulting in insufficient photosensitivity, a slow low-temperature curing process, poor low-temperature curing behavior, and a decrease in mechanical properties (tensile strength and elongation at break).

[0299] Table 1.

[0300]

[0301] According to other experiments of the inventors, the value of m was adjusted based on the foregoing several embodiments. When m = 1, there was no isomerization, and the polyimide resin underwent a complete imidization reaction in advance, and the reaction of forming a salt could not be carried out. Instead of the polyimide resin precursor polyamic acid salt, a polyimide resin was obtained, and thus the process of photoinitiated curing could not be carried out. In addition, in the range of 0.5 < m < 1, when m was relatively high (such as m = 0.7), the curing temperature was likely to be relatively high.

[0302] The technical features of the above embodiments and examples can be combined in any suitable manner. For the sake of brevity of description, not all possible combinations of the technical features in the above embodiments and examples are described. However, as long as there is no contradiction in the combination of these technical features, it should be considered to be within the scope described in this specification. The above embodiments and examples only represent several embodiments of the present application, which are convenient for understanding the technical solutions of the present application in detail, but should not be construed as a limitation on the protection scope of the present application. In addition, it should be understood that after reading the above teachings of the present application, those skilled in the art can make various changes or modifications to the present application, and the equivalent forms obtained also fall within the protection scope of the present application. It should also be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments based on the technical solutions provided in the present application are all within the protection scope of the appended claims of the present application. Therefore, the protection scope of the present patent application should be subject to the content of the appended claims, and the specification and drawings can be used to explain the content of the claims.

Claims

1. A negative photosensitive polyimide photoresist, characterized in that: It contains the following components: isomerized polyimide resin, photoinitiator, photocrosslinking agent, silane coupling agent, light stabilizer, low-temperature curing accelerator and organic solvent; Among them, the isomerized polyimide resin is a polymer having the structure shown in formula (I): In formula (I), Any one of R3 is independently -L1-OC(=O)-C(M)=CH2, L1 is C 1-6 Alkylene, M is H or methyl; any one R1 and any one R2 are independently C 1-3 alkyl; Any one of Ar1 is independently a tetravalent aromatic group and has four single bond sites located on the aromatic ring; Any one of Ar2 is independently a divalent aromatic group and has two single bond sites located on the aromatic ring; m satisfies 0 < m ≤ 0.5, and n is an integer selected from 10 to 100; Ar 31 and Ar 32 Each is independently a capping group containing an aromatic group; The low-temperature curing accelerator can promote the curing reaction of the isomerized polyimide resin at a curing temperature of less than or equal to 250 °C, and the mass ratio of the low-temperature curing accelerator to the isomerized polyimide resin is (0.1 - 0.5):

5.

2. The negative photosensitive polyimide photoresist according to claim 1, characterized in that: It satisfies one of the following characteristics, any suitable multiple or all; L1 is 1,2-ethylene, and both R1 and R2 are methyl; In formula (I), any one of Ar1 is independently a tetravalent aromatic group having 6 - 35 non-hydrogen atoms; In formula (I), any one of Ar2 is independently a divalent aromatic group having 6 - 25 non-hydrogen atoms; Ar 31 and Ar 32 Each independently is a capping group containing -NH-Ar0, Ar0 is C 6-10 Aromatic groups; In formula (I), each R1 is the same, each R2 is the same, each R3 is the same, each Ar1 is the same, and each Ar2 is the same; m is a value selected from 0.01 - 0.5, and can be a value selected from 0.05 - 0.

4.

3. The negative photosensitive polyimide photoresist according to claim 2, characterized in that: In formula (I), Any one of Ar1 is independently any one of the following structures: Any one of Ar2 is independently any one of the following structures: Each * represents a single bond site; Ar0 is 3-hydroxyphenyl, 2-hydroxyphenyl or 4-hydroxyphenyl.

4. The negative photosensitive polyimide photoresist according to any one of claims 1 to 3, characterized in that: It satisfies one or more of the following characteristics: The low-temperature curing accelerator is selected from one or more of isoquinoline, p-quinoline and pyridine; The photocrosslinking agent is an ester derivative of a polyol containing at least two vinyl esters, and the structures of the at least two vinyl esters are each independently -O-C(=O)-C(M2)=CH2, where M2 is H or methyl, and the molecular weight of the ester derivative of the polyol containing at least two vinyl esters is 170 Da - 1000 Da; The mass ratio of the photocrosslinking agent to the isomerized polyimide resin is (1.2 - 2):5; The curing temperature includes one or more temperatures in the range of 200 °C - 250 °C.

5. The negative photosensitive polyimide photoresist according to claim 4, characterized in that: It satisfies one or more of the following characteristics: The photocrosslinking agent is CH2=C(M 21 )-C(=O)-O-(CH2CH2O) q -C(=O)-C(M 22 )=CH2, wherein q is selected from 1, 2, 3, 4, 5 or 6, M 21 and M 22 are each independently H or methyl; The photoinitiator is a benzophenone-type photoinitiator or a benzophenone-based photoinitiator; The mass ratio of the photoinitiator to the isomerized polyimide resin is (0.18 - 0.22):5; The silane coupling agent is a silane coupling agent containing a hydrophilic group, and the hydrophilic group is a hydroxyl group or an amino group; The mass ratio of the silane coupling agent to the isomerized polyimide resin is (0.14 - 0.16):5; The light stabilizer is a phenolic light stabilizer; The mass ratio of the light stabilizer to the isomerized polyimide resin is (0.14 - 0.16):5; The organic solvent is selected from one or more of N-methylpyrrolidone, γ-butyrolactone, dimethyl sulfoxide and N,N-dimethylformamide; The mass ratio of the isomerized polyimide resin to the organic solvent is 5:(12-18).

6. A method for preparing a negative photosensitive polyimide photoresist, characterized in that: The method comprises the following steps: according to the components contained in the negative photosensitive polyimide photoresist according to any one of claims 1 to 5, the isomerized polyimide resin, the photoinitiator, the photocrosslinking agent, the silane coupling agent, the light stabilizer, the low-temperature curing accelerator and the organic solvent are mixed to prepare the negative photosensitive polyimide photoresist; Wherein, the isomerized polyimide resin is prepared by a method comprising the following steps: In anhydrous and oxygen-free conditions and under continuous dispersion, aromatic diamine monomers and aromatic dianhydride monomers are mixed in a polymerization solvent at a molar ratio of 0.9:1 to 1:0.9, and a polymerization reaction is carried out at 0°C to 100°C for 6h to 8h to generate a polyamic acid chain, and an end-capping molecule is added, and an end-capping reaction is carried out at 0°C to 100°C for 1h to 2h to obtain a first mixed solution containing a polyamic acid intermediate; A dehydrating agent and a catalyst are added to the first mixed solution, and a dehydration reaction is carried out at 0°C to 50°C for 1.5h to 2.5h to generate an isomerized polyamic acid, and a photosensitive tertiary amine small molecule containing R3 is added, and a salt-forming reaction is carried out at 0°C to 50°C for 3h to 5h in a dark environment to obtain a second mixed solution; wherein R3 is -L1-OC(=O)-C(M)=CH2, L1 is C 1-6 Alkylene, M is H or methyl; the molar ratio of the dehydrating agent to the aromatic dianhydride monomer is (0.01-1):1; The second mixed solution is mixed with an alcohol solvent to precipitate a polyimide salt, and the solid-liquid separation is performed, and the solid phase is collected, washed, and dried to obtain the isomerized polyimide resin; in, The structure of the aromatic diamine monomer is The structure of the aromatic dianhydride monomer is The polyamic acid chain has a chain structure shown in formula (II-1): Wherein, each * represents a capping site; The structure of the polyamic acid intermediate is shown in formula (II-2): The structure of the isomerized polyamic acid is shown in formula (II-3):

7. The preparation method according to claim 6, characterized in that: Meet one or more of the following characteristics: In the step of mixing the aromatic diamine monomer and the aromatic dianhydride monomer in the polymerization solvent, the molar ratio of the aromatic diamine monomer to the aromatic dianhydride monomer is 1:1; The polymerization solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, sulfolane, butyrolactone, cresol and cyclohexanone; The polymerization reaction is carried out at a temperature of 0°C to 50°C; The end-capping molecule is Ar3-NH2, wherein Ar3 is C 6-10 Aromatic groups; The molar ratio of the end-capping molecule to the aromatic dianhydride monomer is 0.01 to 0.03; The temperature for carrying out the end-capping reaction is 0°C to 50°C; The temperature for carrying out the polymerization reaction is the same as the temperature for carrying out the end-capping reaction; The dehydrating agent is C 4-12 One or more of aliphatic anhydride and xylene; The catalyst is one or more of triethylamine, pyridine and N,N-diisopropylethylamine; The molar ratio of the dehydrating agent, the catalyst and the aromatic dianhydride monomer is (0.1-1): (0.1-1): 1; The temperature for carrying out the dehydration reaction is 0°C to 10°C, which can be an ice bath condition; The photosensitive tertiary amine small molecule containing R3 is The molar ratio of the photosensitive tertiary amine small molecule containing R3 to the aromatic dianhydride monomer is 1.5 to 2.5; The temperature for the salt-forming reaction is 0°C to 10°C, which may be an ice bath condition; The alcohol solvent is one or more of methanol and ethanol; The drying method is to perform vacuum drying at 80°C to 250°C.

8. A polyimide film, characterized in that: The negative photosensitive polyimide photoresist according to any one of claims 1 to 5 is cured, or the negative photosensitive polyimide photoresist prepared by the preparation method according to claim 6 or 7 is cured; the curing temperature is lower than or equal to 250°C.

9. Use of the negative photosensitive polyimide photoresist according to any one of claims 1 to 5 or the negative photosensitive polyimide photoresist prepared by the preparation method according to claim 6 or 7 in preparing a polyimide micro pattern, the application comprising the following steps: drying the negative photosensitive polyimide photoresist at 100° C. to 120° C. to form a photosensitive film, exposing, developing, washing, and curing at a curing temperature lower than or equal to 250° C.; Optionally, curing is performed at a curing temperature of 100° C. to 250° C.; Further optionally, curing is performed at a curing temperature of 200°C to 250°C.

10. The use according to claim 9, characterized in that: Said applications include applications in microelectronic packaging; Wherein, the microelectronic package includes at least one of a fan-out wafer-level package and a fan-out flat-panel-level package; The curing temperature includes one or more temperatures in the range of 200°C to 250°C.