Semiconductor device and manufacturing method thereof

By forming a second epitaxial layer and an oxide layer with different conductivity types in the semiconductor device and forming a PN junction using the trench structure, the problem of insufficient high-voltage resistance of semiconductor devices in the prior art is solved, and higher resistivity and resistance are achieved High voltage performance.

CN119029045APending Publication Date: 2024-11-26ZHUHAI GREE ELECTRONIC COMPONENTS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411418313.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing semiconductor devices have poor high voltage resistance and are difficult to meet the application requirements such as low power consumption, high frequency, high temperature, and miniaturization.

Method used

By forming a first trench and a second trench on the substrate, a second epitaxial layer and an oxide layer of different conductivity types are formed in the trench and on the side walls, respectively, to form a PN junction to improve the high voltage resistance of the device.

Benefits of technology

Since the depth of the trench is controllable, the doping concentration of the second epitaxial layer is more uniform, and the width of the depletion region formed is more uniform and controllable, which improves the resistivity and high voltage resistance of the semiconductor device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119029045A_ABST
    Figure CN119029045A_ABST
Patent Text Reader

Abstract

The invention provides a semiconductor device and a manufacturing method thereof. The semiconductor device includes: a substrate; the first epitaxial layer comprises an epitaxial layer body and a first groove, the epitaxial layer body is located on the surface of one side of the substrate, and the first groove is located in the epitaxial layer body; the oxide layer is located on the side wall of the first groove; the second epitaxial layer is located in the first groove, the second epitaxial layer makes contact with the oxide layer and the bottom face of the first groove, and the conduction type of the second epitaxial layer is different from that of the first epitaxial layer. The semiconductor device at least solves the problem that in the prior art, a semiconductor device is poor in high voltage resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a semiconductor device and a method for manufacturing the same. Background Art

[0002] Power diodes are key components of circuit systems and are widely used in civilian products such as high-frequency inverters, digital products, generators, and televisions, as well as various advanced equipment control systems and military instrumentation equipment such as satellite receiving devices, missiles, and aircraft. Power diodes are expanding in two important directions: (1) Developing towards tens of millions or even tens of thousands of amperes, they can be used in high-temperature arc wind tunnels, resistance welding machines, and other occasions; (2) The reverse recovery time is getting shorter and shorter, showing a trend towards ultra-fast, ultra-soft, and ultra-durable development, making them not only used in rectification occasions, but also playing different roles in various switching circuits. In order to meet the requirements of low power consumption, high frequency, high temperature, and miniaturization, their withstand voltage, on-resistance, turn-on voltage drop, reverse recovery characteristics, and high temperature characteristics are getting higher and higher.

[0003] At present, as microelectronic devices develop towards low power consumption, high voltage resistance and high reliability, the requirements for semiconductor materials are gradually increasing. Microelectronic devices are increasingly used in special environments such as high temperature, high radiation, high frequency and high power. How to optimize the high voltage resistance of semiconductor devices is a technical problem that needs to be solved urgently. Summary of the invention

[0004] The main purpose of the present application is to provide a semiconductor device and a method for manufacturing the same, so as to at least solve the problem of poor high voltage resistance of semiconductor devices in the prior art.

[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present application, a semiconductor device is provided, including: a substrate; a first epitaxial layer, including an epitaxial layer body and a first trench, the epitaxial layer body is located on a side surface of the substrate, and the first trench is located in the epitaxial layer body; an oxide layer is located on the side wall of the first trench; a second epitaxial layer is located in the first trench, the second epitaxial layer is respectively in contact with the oxide layer and the bottom surface of the first trench, and the conductivity type of the second epitaxial layer is different from the conductivity type of the first epitaxial layer.

[0006] Optionally, the first epitaxial layer also includes a second trench, which is located in the epitaxial layer body and spaced apart from the first trench, and the second epitaxial layer is also located on the side walls and bottom surface of the second trench. The semiconductor device also includes: a first metal layer, which is located in the second trench and contacts the second epitaxial layer in the second trench, and the contact surface between the first metal layer and the second epitaxial layer is an ohmic contact surface.

[0007] Optionally, the depth of the first groove is equal to the depth of the second groove, and the width of the first groove is equal to the width of the second groove.

[0008] Optionally, the semiconductor device also includes: a second metal layer, located on the surface of the first epitaxial layer away from the substrate, and the contact surface between the second metal layer and the epitaxial layer body is a Schottky contact surface; a third metal layer, located on the surface of the substrate away from the first epitaxial layer, and the contact surface between the third metal layer and the substrate is an ohmic contact surface.

[0009] Optionally, the second metal layer includes: a first metal sublayer, located on the surface of the first epitaxial layer away from the substrate, and in contact with the second epitaxial layer and the oxide layer respectively; a second metal sublayer, located on the surface of the first metal sublayer away from the first epitaxial layer, and the third metal layer includes: a third metal sublayer, located on the surface of the substrate away from the first epitaxial layer; a fourth metal sublayer, located on the surface of the third metal sublayer away from the substrate; and a fifth metal sublayer, located on the surface of the fourth metal sublayer away from the third metal sublayer.

[0010] Optionally, the material of the first metal sublayer includes titanium, the material of the second metal sublayer includes aluminum, the material of the third metal sublayer includes titanium, the material of the fourth metal sublayer includes nickel, and the material of the fifth metal sublayer includes silver.

[0011] Optionally, materials of the substrate, the first epitaxial layer and the second epitaxial layer respectively include silicon carbide.

[0012] According to another aspect of the present application, a method for manufacturing a semiconductor device is provided, and the semiconductor device is any one of the semiconductor devices described above, and the method includes: providing a substrate; forming an epitaxial layer body on a surface of one side of the substrate, and removing part of the epitaxial layer body to form a first trench in at least the epitaxial layer body to obtain a first epitaxial layer; forming an oxide layer on the side wall of the first trench; forming a second epitaxial layer at least in the first trench where the oxide layer is formed, the second epitaxial layer respectively contacts the oxide layer and the bottom surface of the first trench, and the conductivity type of the second epitaxial layer is different from the conductivity type of the first epitaxial layer.

[0013] Optionally, a portion of the epitaxial layer body is removed to form a first groove at least in the epitaxial layer body to obtain a first epitaxial layer, comprising: dry etching the epitaxial layer body to form the first and second grooves spaced apart in the epitaxial layer body to obtain the first epitaxial layer including the first groove, the second groove and the epitaxial layer body; forming a second epitaxial layer at least in the first groove where the oxide layer is formed, comprising: forming an initial epitaxial layer in the first groove where the oxide layer is formed and in the second groove; removing a portion of the initial epitaxial layer in the second groove to obtain a third groove, and the remaining initial epitaxial layer forms a second epitaxial layer; after forming the second epitaxial layer at least in the first groove where the oxide layer is formed, the method further comprises: filling a metal material in the third groove to obtain a first metal layer, the first metal layer being in contact with the second epitaxial layer located in the second groove; and thermally annealing the structure where the first metal layer is formed to form an ohmic contact at a contact surface between the first metal layer and the second epitaxial layer.

[0014] Optionally, an oxide layer is formed on the sidewall of the first trench, including: thermally oxidizing the first epitaxial layer formed with the first trench and the second trench to form an initial oxide layer on the surface of the first epitaxial layer away from the substrate; removing the initial oxide layer on the bottom surface of the first trench, the initial oxide layer in the second trench, and the initial oxide layer on the surface of the epitaxial layer body away from the substrate, and the remaining initial oxide layer constitutes the oxide layer.

[0015] Optionally, after forming a second epitaxial layer at least in the first trench in which the oxide layer is formed, the method further includes: forming a second metal layer on a surface of the first epitaxial layer away from the substrate and performing a thermal annealing process to form a Schottky contact at a contact surface between the second metal layer and the epitaxial layer body; forming a third metal layer on a surface of the substrate away from the first epitaxial layer and performing a thermal annealing process to form an ohmic contact at a contact surface between the third metal layer and the substrate.

[0016] Optionally, a second metal layer is formed on the surface of the first epitaxial layer away from the substrate and a thermal annealing process is performed to form a Schottky contact at the contact surface between the second metal layer and the epitaxial layer body, including: forming a first metal sublayer on the surface of the first epitaxial layer away from the substrate, the first metal sublayer is in contact with the second epitaxial layer and the oxide layer respectively; forming a second metal sublayer on the surface of the first metal sublayer away from the first epitaxial layer, and performing the thermal annealing process during the formation of the second metal sublayer, so that the contact surface between the first metal sublayer and the epitaxial layer body forms a Schottky contact; forming a third metal layer on the surface of the substrate away from the first epitaxial layer and a thermal annealing process is performed, including: stacking a third metal sublayer, a fourth metal sublayer and a fifth metal sublayer in sequence on the surface of the substrate away from the first epitaxial layer, and performing the thermal annealing process, so that the contact surface between the third metal sublayer and the substrate forms an ohmic contact.

[0017] By applying the technical solution of the present application, in the semiconductor device of the present application, a first epitaxial layer having a first trench is located on a substrate, an oxide layer is located on a sidewall of the first trench, a second epitaxial layer having a conductivity type different from that of the first epitaxial layer is located on the bottom surface of the first trench and in contact with the oxide layer, and a PN junction is formed at the junction of the first epitaxial layer and the second epitaxial layer. Compared with the solution of forming an ion implantation region in the first epitaxial layer in the prior art to form a PN junction, the present application fills the second epitaxial layer having a conductivity type different from that of the first epitaxial layer in the trench of the first epitaxial layer to form a PN junction. Since the depth of the trench has a large controllable range, the depth of the second epitaxial layer located in the trench can be made deeper, and compared with the ion implantation region, the doping concentration of the epitaxial layer is more uniform, so that the width of the depletion region formed by the PN junction of the present application is more uniform and controllable, and the resistivity of the device is higher, thereby ensuring that the semiconductor device has a better high-voltage resistance capability, and solving the problem of poor high-voltage resistance capability of the semiconductor device in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The drawings constituting part of the present application are used to provide a further understanding of the present application. The exemplary embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0019] Figure 1 A schematic structural diagram of a semiconductor device provided according to an embodiment of the present application is shown;

[0020] Figure 2 A schematic structural diagram of another semiconductor device provided according to an embodiment of the present application is shown;

[0021] Figure 3 A schematic flow chart of a method for manufacturing a semiconductor device according to an embodiment of the present application is shown;

[0022] Figures 4 to 11 The schematic diagrams of the structures obtained after each process step of the method for manufacturing a semiconductor device according to the present application are respectively shown.

[0023] The above drawings include the following reference numerals:

[0024] 10. Substrate; 11. First epitaxial layer; 12. Epitaxial layer body; 13. First trench; 14. Second trench; 15. Oxide layer; 16. Second epitaxial layer; 17. First metal layer; 18. Second metal layer; 19. Third metal layer; 20. First metal sublayer; 21. Second metal sublayer; 22. Third metal sublayer; 23. Fourth metal sublayer; 24. Fifth metal sublayer; 25. Initial epitaxial layer; 26. Initial oxide layer; 27. Third trench. DETAILED DESCRIPTION

[0025] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0026] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.

[0027] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the accompanying drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present application described here. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0028] As introduced in the background technology, there is a technical problem in the prior art that semiconductor devices have poor high voltage resistance. To solve this technical problem, an embodiment of the present application provides a semiconductor device and a method for manufacturing the same.

[0029] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0030] An embodiment of the present application provides a semiconductor device. Figure 1 A schematic cross-sectional view of a semiconductor device of the present invention is shown as an example. Figure 1 As shown, the semiconductor device comprises:

[0031] Substrate 10;

[0032] A first epitaxial layer, comprising an epitaxial layer body 12 and a first trench, wherein the epitaxial layer body 12 is located on a side surface of the substrate 10, and the first trench is located in the epitaxial layer body 12;

[0033] Specifically, the first trench extends from a surface of the epitaxial layer body 12 away from the substrate 10 into the epitaxial layer body 12 .

[0034] an oxide layer 15, located on the sidewalls of the first trench;

[0035] Specifically, Figure 1 The embodiment in which the oxide layer is located on both sidewalls of the first trench is exemplarily shown. Figure 1 In addition to the example shown, the oxide layer 15 may also be located only on one sidewall of the first trench; in addition, the oxide layer 15 may completely cover one sidewall of the first trench, or may only cover a portion of one sidewall of the first trench.

[0036] The second epitaxial layer 16 is located in the first trench. The second epitaxial layer 16 contacts the oxide layer 15 and the bottom surface of the first trench respectively. The conductivity type of the second epitaxial layer 16 is different from that of the first epitaxial layer.

[0037] Specifically, the oxide layer 15 located on the sidewall of the first trench serves to isolate the first epitaxial layer and the second epitaxial layer 16; the second epitaxial layer 16 contacts the epitaxial layer body 12 through the bottom surface of the first trench, and the second epitaxial layer 16 and the epitaxial layer body 12 have different conductivity types, so a PN junction is formed at the junction between the two. The surface of the second epitaxial layer 16 away from the substrate 10 can be flush with the surface of the epitaxial layer body 12 away from the substrate 10, that is, the second epitaxial layer 16 fills the first trench; of course, the surface of the second epitaxial layer away from the substrate 10 can also be higher or lower than the surface of the epitaxial layer body 12 away from the substrate 10. The conductivity type of the second epitaxial layer 16 can be P type or N type. When the conductivity type of the second epitaxial layer 16 is P type, the conductivity type of the epitaxial layer body 12 is N type; when the conductivity type of the second epitaxial layer 16 is N type, the conductivity type of the epitaxial layer body 12 is P type.

[0038] Through the embodiments, in the semiconductor device of the present application, the first epitaxial layer with the first trench is located on the substrate, the oxide layer is located on the sidewall of the first trench, the second epitaxial layer with a conductivity type different from that of the first epitaxial layer is located on the bottom surface of the first trench and in contact with the oxide layer, and a PN junction is formed at the junction of the first epitaxial layer and the second epitaxial layer. Compared with the solution of forming an ion implantation region in the first epitaxial layer in the prior art to form a PN junction, the present application fills the second epitaxial layer with a conductivity type different from that of the first epitaxial layer in the trench of the first epitaxial layer to form a PN junction. Since the depth of the trench has a large controllable range, the depth of the second epitaxial layer located in the trench can be made deeper, and compared with the ion implantation region, the doping concentration of the epitaxial layer is more uniform, so that the width of the depletion region formed by the PN junction of the present application is more uniform and controllable, and the resistivity of the device is higher, which ensures that the semiconductor device has a better high-voltage resistance capability, and solves the problem of poor high-voltage resistance capability of the semiconductor device in the prior art.

[0039] Specifically, the specific material of the substrate can be selected according to the actual needs of the semiconductor device, and may include a silicon substrate, a silicon carbide substrate, a silicon germanium substrate, an SOI substrate or a GOI substrate, etc. The conductivity type of the substrate may be P-type or N-type. The conductivity type of the epitaxial layer body may be the same as or different from that of the substrate. The materials of the first epitaxial layer and the second epitaxial layer may be the same or different, and the materials of the two may include but are not limited to silicon, silicon germanium, silicon carbide, and gallium nitride, etc. The material of the oxide layer may be any suitable isolation material, such as silicon oxide, high-k dielectric material, etc.

[0040] According to some exemplary embodiments of the present application, Figure 2In the semiconductor device shown, the conductivity type of the substrate is the same as the conductivity type of the first epitaxial layer, both are N-type; the doping concentration of the substrate is greater than the doping concentration of the first epitaxial layer, and the conductivity type of the second epitaxial layer is P-type.

[0041] In another embodiment of the present application, the oxide layer covers the two side walls of the first trench. That is, the second epitaxial layer contacts the first epitaxial layer only through the bottom surface of the first trench. The oxide layer on the two side walls of the first trench isolates the second epitaxial layer from the epitaxial layer body on both sides thereof, thereby ensuring that the area of ​​the PN junction is small, thereby ensuring that the leakage current of the device is small, and further ensuring that the device performance is good.

[0042] In actual application, the number of the first trench in the semiconductor device may be only one, or may be Figure 1 As shown, there are a plurality of first grooves, and the plurality of first grooves may be arranged at intervals.

[0043] Alternatively, if Figure 1 and Figure 2 As shown, the first epitaxial layer also includes a second groove, the second groove is located in the epitaxial layer body 12 and is spaced apart from the first groove, the second epitaxial layer 16 is also located on the sidewall and bottom surface of the second groove, and the semiconductor device also includes: a first metal layer 17, located in the second groove, in contact with the second epitaxial layer 16 located in the second groove, and the contact surface between the first metal layer 17 and the second epitaxial layer 16 is an ohmic contact surface. In this embodiment, the ohmic contact is formed by the groove structure, the contact area is large, so that the ohmic discharge area is large, and the surge resistance of the semiconductor device is ensured to be strong.

[0044] In actual application, the number of the second grooves in the semiconductor device may be only one or more, and the plurality of second grooves may be arranged at intervals. The material of the first metal layer may be any suitable metal monomer material or alloy material, etc. The first metal layer may be a single-layer metal layer or a multi-layer metal layer.

[0045] In a specific embodiment, Figure 4 As shown, the first grooves and the second grooves are arranged alternately and spaced apart. The material of the first metal layer is specifically nickel.

[0046] In order to further improve the device performance of the semiconductor device, according to some other optional solutions of the present application, Figure 4 FIG. 1 shows a schematic structural diagram of a first epitaxial layer 11 in which a first trench 13 and a second trench 14 are formed in an epitaxial layer body 12. Figure 4As shown, the depth D1 of the first trench 13 is equal to the depth D2 of the second trench 14, and the width W1 of the first trench 13 is equal to the width W2 of the second trench 14. In this embodiment, the depths of the first trench and the second trench are set to be the same, so that the reverse withstand voltage capability of the device can be strong, and the widths of the first trench and the second trench are set to be the same to ensure that the filling effect of the trench is relatively consistent and controllable, thereby simplifying the difficulty of the trench filling process.

[0047] In addition, if Figure 2 As shown, the semiconductor device further includes: a second metal layer 18, located on the surface of the first epitaxial layer away from the substrate 10, and the contact surface between the second metal layer 18 and the epitaxial layer body 12 is a Schottky contact surface; a third metal layer 19, located on the surface of the substrate 10 away from the first epitaxial layer, and the contact surface between the third metal layer 19 and the substrate 10 is an ohmic contact surface. This embodiment forms an ohmic contact and a Schottky contact, and under the premise of ensuring the withstand voltage performance of the device, the forward voltage drop of the device can be further reduced, thereby further improving the surge resistance of the device.

[0048] Those skilled in the art can flexibly set the specific structure and material of the second metal layer and the third metal layer according to actual needs. The second metal layer and the third metal layer can be a single metal layer or a multi-layer metal layer. The material of the second metal layer and the third metal layer can be a single metal material or an alloy material.

[0049] For example, Figure 2 As shown, the second metal layer 18 and the third metal layer 19 are both multi-layer structures. Specifically, the second metal layer 18 includes: a first metal sublayer 20, which is located on the surface of the first epitaxial layer away from the substrate 10, and is in contact with the second epitaxial layer 16 and the oxide layer 15 respectively; a second metal sublayer 21, which is located on the surface of the first metal sublayer 20 away from the first epitaxial layer; the third metal layer 19 includes: a third metal sublayer 22, which is located on the surface of the substrate 10 away from the first epitaxial layer; a fourth metal sublayer 23, which is located on the surface of the third metal sublayer 22 away from the substrate 10; and a fifth metal sublayer 24, which is located on the surface of the fourth metal sublayer 23 away from the third metal sublayer 22.

[0050] Specifically, Figure 2 As shown, the first metal sublayer 20 not only covers the surface of the epitaxial layer body 12 away from the substrate 10, but also covers the oxide layer 15 located in the first trench, the second epitaxial layer 16 located in the first trench and the second trench, and the first metal layer 17 located in the second trench.

[0051] In an embodiment of the present application, the material of the first metal sublayer includes titanium, the material of the second metal sublayer includes aluminum, the material of the third metal sublayer includes titanium, the material of the fourth metal sublayer includes nickel, and the material of the fifth metal sublayer includes silver.

[0052] Furthermore, the first metal sublayer is a titanium layer, and the second metal sublayer is an aluminum layer. Since titanium has good corrosion resistance and electrical conductivity, and aluminum has high electrical conductivity and thermal conductivity, the two can be superimposed together to increase the electrode stability and electrical conductivity of the semiconductor device. In addition, the titanium layer can also provide protection and extend the service life of the semiconductor device, thereby improving the performance and reliability of the device. The third metal sublayer is a titanium layer, the fourth metal sublayer is a nickel layer, and the fifth metal sublayer is a silver layer. Since titanium, nickel, and silver each have different electrical conductivity and chemical properties, their laminated structure can effectively reduce the resistance of the electrode and improve the current transmission efficiency. In addition, the laminated structure of titanium, nickel, and silver can also improve the corrosion resistance of the electrode and extend the service life of the diode, thereby improving the performance and reliability of the device.

[0053] Of course, the constituent materials of the first metal sublayer to the fifth metal sublayer are not limited to the aforementioned materials, and those skilled in the art may flexibly select them according to actual needs, and the present application does not impose any specific restrictions on this.

[0054] In an optional embodiment, the materials of the substrate, the first epitaxial layer and the second epitaxial layer include silicon carbide respectively. The bandgap and thermal conductivity of SiC material are three times that of Si material, and the concentration of intrinsic carriers is only one tenth of that of silicon material. These excellent physical properties make semiconductor power devices made of SiC material have great advantages in high frequency, high temperature, high power and high radiation environments.

[0055] In a more specific embodiment, the materials of the substrate, the first epitaxial layer and the second epitaxial layer are all silicon carbide. The semiconductor device is specifically a silicon carbide power diode. Applying the semiconductor device structure of the present application to a silicon carbide power diode can obtain a power diode device with higher breakdown voltage and withstand voltage, which is suitable for application in high voltage circuits.

[0056] According to another aspect of the present application, a method for manufacturing the semiconductor device is provided, such as Figure 3 As shown, the method includes:

[0057] Step S201: providing a substrate 10;

[0058] Step S202: Figure 4As shown, an epitaxial layer body 12 is formed on one side surface of the substrate 10, and a portion of the epitaxial layer body 12 is removed to form a first trench 13 at least in the epitaxial layer body 12, thereby obtaining a first epitaxial layer 11;

[0059] Specifically, the first trench extends from a surface of the epitaxial layer body 12 away from the substrate 10 into the epitaxial layer body 12 .

[0060] Step S203: forming an oxide layer 15 on the sidewall of the first trench to obtain Figure 6 The structure shown;

[0061] Specifically, Figure 6 The embodiment in which the oxide layer is located on both sidewalls of the first trench is exemplarily shown. Figure 6 In addition to the example shown, the oxide layer 15 may also be located only on one sidewall of the first trench; in addition, the oxide layer 15 may completely cover one sidewall of the first trench, or may only cover a portion of one sidewall of the first trench.

[0062] Step S204: forming a second epitaxial layer 16 at least in the first trench where the oxide layer 15 is formed, the second epitaxial layer 16 contacts the oxide layer 15 and the bottom surface of the first trench respectively, and the conductivity type of the second epitaxial layer 16 is different from that of the first epitaxial layer.

[0063] Specifically, the oxide layer 15 located on the sidewall of the first trench serves to isolate the first epitaxial layer and the second epitaxial layer 16; the second epitaxial layer 16 contacts the epitaxial layer body 12 through the bottom surface of the first trench, and the second epitaxial layer 16 and the epitaxial layer body 12 have different conductivity types, so a PN junction is formed at the junction between the two. The surface of the second epitaxial layer 16 away from the substrate 10 can be flush with the surface of the epitaxial layer body 12 away from the substrate 10, that is, the second epitaxial layer 16 fills the first trench; of course, the surface of the second epitaxial layer away from the substrate 10 can also be higher or lower than the surface of the epitaxial layer body 12 away from the substrate 10. The conductivity type of the second epitaxial layer 16 can be P type or N type. When the conductivity type of the second epitaxial layer 16 is P type, the conductivity type of the epitaxial layer body 12 is N type; when the conductivity type of the second epitaxial layer 16 is N type, the conductivity type of the epitaxial layer body 12 is P type.

[0064] Through the embodiment, the manufacturing method of the present application first forms a first epitaxial layer with a first groove on a side surface of the substrate; then forms an oxide layer on the side wall of the first groove; then, forms a second epitaxial layer at least in the remaining first groove, and the conductivity type of the second epitaxial layer is different from that of the first epitaxial layer, so that a PN junction is formed at the junction of the first epitaxial layer and the second epitaxial layer. The present application fills the second epitaxial layer with a conductivity type different from that of the first epitaxial layer into the groove of the first epitaxial layer to form a PN junction. Since the depth of the groove can be controlled in a large range, the depth of the second epitaxial layer located in the groove can be deeper, and compared with the ion implantation area, the doping concentration of the epitaxial layer is more uniform, so that the width of the depletion region formed by the PN junction of the present application is more uniform and controllable, and the resistivity of the device is higher, which ensures that the semiconductor device has a better high-voltage resistance capability, and solves the problem of poor high-voltage resistance capability of semiconductor devices in the prior art.

[0065] In actual application, the epitaxial layer body 12 can be formed on one side surface of the substrate 10 by epitaxial growth, for example, by using epitaxial methods such as vapor phase epitaxy, molecular beam epitaxy, liquid phase epitaxy or suspension epitaxy.

[0066] In a specific application, a portion of the epitaxial layer body is removed to form at least a first groove in the epitaxial layer body to obtain a first epitaxial layer, comprising: dry etching the epitaxial layer body 12 to form the first groove 13 and the second groove 14 spaced apart in the epitaxial layer body 12 to obtain Figure 4 The first epitaxial layer 11 shown includes the first trench 13, the second trench 14 and the epitaxial layer body 12. The first trench and the second trench are formed in the epitaxial layer body by dry etching, and the sizes of the first trench and the second trench can be precisely controlled, with strong controllability and high production efficiency.

[0067] In this embodiment, the first trench and the second trench having the same width and depth are obtained by dry etching. The first trench and the second trench are set to have the same depth, which can ensure that the reverse voltage withstand capability of the device is strong, and the first trench and the second trench are set to have the same width, which can ensure that the filling effect of the trench is relatively consistent and controllable, thereby simplifying the difficulty of the trench filling process.

[0068] On this basis, forming a second epitaxial layer 16 at least in the first trench 13 where the oxide layer 15 is formed includes: Figure 6 and Figure 7 As shown, an initial epitaxial layer 25 is formed in the first trench 13 and the second trench 14 where the oxide layer 15 is formed; a portion of the initial epitaxial layer 25 in the second trench 14 is removed to obtain a third trench 27, and the remaining initial epitaxial layer 25 forms a second epitaxial layer 16, referring to Figure 8 After at least forming the second epitaxial layer 16 in the first trench 13 where the oxide layer 15 is formed, the method further comprises: Figure 8 and Fig. 9 As shown, a metal material is filled in the third groove 27 to obtain a first metal layer 17, and the first metal layer 17 is in contact with the second epitaxial layer 16 located in the second groove; the structure formed with the first metal layer 17 is subjected to thermal annealing treatment to form an ohmic contact at the contact surface between the first metal layer 17 and the second epitaxial layer 16. In this embodiment, a third groove is formed by removing part of the initial epitaxial layer, and then a metal material is filled in the third groove to form a first metal layer in ohmic contact with the second epitaxial layer, thereby ensuring a larger contact area of ​​the ohmic contact, a larger ohmic discharge area, and a stronger surge resistance of the semiconductor device.

[0069] It should be noted that the third trench 27 obtained by etching will not expose the epitaxial layer body 12 .

[0070] Specifically, dry etching may be used to remove part of the initial epitaxial layer 25 in the second trench 14. The initial epitaxial layer 25 is also grown epitaxially, such as by vapor phase epitaxy, molecular beam epitaxy, liquid phase epitaxy or suspension epitaxy.

[0071] Wherein, the annealing temperature of the thermal annealing treatment is greater than 900°C.

[0072] In order to further simplify the manufacturing process, specifically, Figures 4 to 6 As shown, an oxide layer 15 is formed on the sidewall of the first trench 13, including: Figure 4 The first epitaxial layer 11 formed with the first trench 13 and the second trench 14 is thermally oxidized to form an initial oxide layer 26 on the surface of the first epitaxial layer 11 away from the substrate 10, that is, the initial oxide layer 26 covers the exposed surface of the epitaxial layer body 12, the exposed surface of the first trench 13 and the exposed surface of the second trench 14, and obtains Figure 5 The structure shown in FIG. 1 is as follows; the initial oxide layer 26 located on the bottom surface of the first trench 13, the initial oxide layer 26 located in the second trench 14, and the initial oxide layer 26 located on the surface of the epitaxial layer body 12 away from the substrate 10 are removed, so that the initial oxide layer 26 located on the two side walls of the first trench 13 is retained, and the remaining initial oxide layer 26 constitutes the oxide layer 15, and the structure shown in FIG. Figure 6 The structure shown.

[0073] In addition to the thermal oxidation process, other deposition methods may be used to form the initial oxide layer 26 on the surface of the first epitaxial layer 11 away from the substrate 10, including but not limited to atomic layer deposition, chemical vapor deposition, physical vapor deposition, molecular beam epitaxy, etc.

[0074] Optionally, after forming the second epitaxial layer at least in the first trench having the oxide layer formed therein, the method further comprises: Fig.11 As shown, a second metal layer 18 is formed on the surface of the first epitaxial layer away from the substrate 10 and a thermal annealing process is performed to form a Schottky contact at the contact surface between the second metal layer 18 and the epitaxial layer body 12; Figure 2 As shown, a third metal layer 19 is formed on the surface of the substrate 10 away from the first epitaxial layer and a thermal annealing process is performed to form an ohmic contact between the contact surface of the third metal layer 19 and the substrate 10 .

[0075] Optionally, forming a second metal layer on a surface of the first epitaxial layer away from the substrate and performing a thermal annealing process to form a Schottky contact at a contact surface between the second metal layer and the epitaxial layer body comprises: Fig.10 and Fig.11 As shown, a first metal sublayer 20 is formed on the surface of the first epitaxial layer away from the substrate 10, and the first metal sublayer 20 is in contact with the second epitaxial layer 16 and the oxide layer 15 respectively; a second metal sublayer 21 is formed on the surface of the first metal sublayer 20 away from the first epitaxial layer, and the thermal annealing process is performed during the formation of the second metal sublayer 21, so that the contact surface of the first metal sublayer 20 and the epitaxial layer body 12 forms a Schottky contact, and the first metal sublayer 20 and the second metal sublayer 21 constitute the second metal layer 18. By forming ohmic contacts and Schottky contacts, the forward voltage drop of the device can be further reduced while ensuring the withstand voltage performance of the device, thereby further improving the surge resistance of the device.

[0076] Specifically, the second metal sub-layer is prepared at high temperature, and a thermal annealing operation is performed simultaneously during the preparation of the second metal sub-layer.

[0077] Forming a third metal layer on a surface of the substrate away from the first epitaxial layer and performing a thermal annealing process, including: Fig.11 and Figure 2As shown, a third metal sublayer 22, a fourth metal sublayer 23 and a fifth metal sublayer 24 are stacked in sequence on the surface of the substrate 10 away from the first epitaxial layer, and the thermal annealing process is performed so that the third metal sublayer 22 forms an ohmic contact with the contact surface of the substrate 10, and the third metal sublayer 22, the fourth metal sublayer 23 and the fifth metal sublayer 24 constitute the third metal layer 19.

[0078] Those skilled in the art may choose any suitable method to grow the metal sub-layers, including but not limited to chemical vapor deposition (CVD), physical vapor deposition (PVD), sputtering, and evaporation to produce the metal sub-layers.

[0079] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the process, method, commodity or device including the elements.

[0080] From the above description, it can be seen that the embodiments described in this application achieve the following technical effects:

[0081] 1) In the semiconductor device of the present application, the first epitaxial layer with the first trench is located on the substrate, the oxide layer is located on the sidewall of the first trench, the second epitaxial layer with a conductivity type different from that of the first epitaxial layer is located on the bottom surface of the first trench and in contact with the oxide layer, and a PN junction is formed at the junction of the first epitaxial layer and the second epitaxial layer. Compared with the solution of forming an ion implantation region in the first epitaxial layer to form a PN junction in the prior art, the second epitaxial layer with a conductivity type different from that of the first epitaxial layer is filled in the trench of the first epitaxial layer in the present application to form a PN junction. Since the depth of the trench can be controlled in a large range, the depth of the second epitaxial layer located in the trench can be deeper, and compared with the ion implantation region, the doping concentration of the epitaxial layer is more uniform, so that the width of the depletion region formed by the PN junction of the present application is more uniform and controllable, and the resistivity of the device is higher, which ensures that the semiconductor device has a better high-voltage resistance capability, and solves the problem of poor high-voltage resistance capability of the semiconductor device in the prior art.

[0082] 2) The manufacturing method of the present application first forms a first epitaxial layer with a first groove on a side surface of the substrate; then forms an oxide layer on the side wall of the first groove; then, forms a second epitaxial layer at least in the remaining first groove, and the conductivity type of the second epitaxial layer is different from that of the first epitaxial layer, so that a PN junction is formed at the junction of the first epitaxial layer and the second epitaxial layer. The present application fills the second epitaxial layer with a conductivity type different from that of the first epitaxial layer into the groove of the first epitaxial layer to form a PN junction. Since the depth of the groove can be controlled in a large range, the depth of the second epitaxial layer located in the groove can be deeper, and compared with the ion implantation area, the doping concentration of the epitaxial layer is more uniform, so that the width of the depletion region formed by the PN junction of the present application is more uniform and controllable, and the resistivity of the device is higher, which ensures that the semiconductor device has better high-voltage resistance and solves the problem of poor high-voltage resistance of semiconductor devices in the prior art.

[0083] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A semiconductor device, characterized in that: include: substrate; A first epitaxial layer, comprising an epitaxial layer body and a first trench, wherein the epitaxial layer body is located on a side surface of the substrate, and the first trench is located in the epitaxial layer body; an oxide layer, located on the sidewalls of the first trench; A second epitaxial layer is located in the first trench, the second epitaxial layer is in contact with the oxide layer and a bottom surface of the first trench respectively, and the conductivity type of the second epitaxial layer is different from that of the first epitaxial layer.

2. The semiconductor device according to claim 1, wherein: The first epitaxial layer further includes a second trench, the second trench is located in the epitaxial layer body and is spaced apart from the first trench, the second epitaxial layer is also located on the sidewall and bottom surface of the second trench, and the semiconductor device further includes: The first metal layer is located in the second trench and contacts the second epitaxial layer in the second trench. The contact surface between the first metal layer and the second epitaxial layer is an ohmic contact surface.

3. The semiconductor device according to claim 2, characterized in that The depth of the first groove is equal to the depth of the second groove, and the width of the first groove is equal to the width of the second groove.

4. The semiconductor device according to claim 1, wherein: The semiconductor device further comprises: A second metal layer is located on a surface of the first epitaxial layer away from the substrate, and a contact surface between the second metal layer and the epitaxial layer body is a Schottky contact surface; The third metal layer is located on a surface of the substrate away from the first epitaxial layer, and a contact surface between the third metal layer and the substrate is an ohmic contact surface.

5. The semiconductor device according to claim 4, characterized in that The second metal layer comprises: A first metal sublayer is located on a surface of the first epitaxial layer away from the substrate and is in contact with the second epitaxial layer and the oxide layer respectively; The second metal sub-layer is located on a surface of the first metal sub-layer away from the first epitaxial layer, and the third metal layer includes: A third metal sublayer is located on a surface of the substrate away from the first epitaxial layer; a fourth metal sublayer, located on a surface of the third metal sublayer away from the substrate; The fifth metal sub-layer is located on a surface of the fourth metal sub-layer away from the third metal sub-layer.

6. The semiconductor device according to claim 5, characterized in that The material of the first metal sublayer includes titanium, the material of the second metal sublayer includes aluminum, the material of the third metal sublayer includes titanium, the material of the fourth metal sublayer includes nickel, and the material of the fifth metal sublayer includes silver.

7. The semiconductor device according to any one of claims 1 to 6, characterized in that Materials of the substrate, the first epitaxial layer, and the second epitaxial layer respectively include silicon carbide.

8. A method for manufacturing a semiconductor device, characterized in that: The semiconductor device is a semiconductor device according to any one of claims 1 to 7, and the method comprises: providing a substrate; Forming an epitaxial layer body on one side surface of the substrate, and removing part of the epitaxial layer body to form a first trench at least in the epitaxial layer body to obtain a first epitaxial layer; forming an oxide layer on the sidewalls of the first trench; A second epitaxial layer is formed at least in the first trench where the oxide layer is formed, the second epitaxial layer is in contact with the oxide layer and the bottom surface of the first trench respectively, and the conductivity type of the second epitaxial layer is different from that of the first epitaxial layer.

9. The method according to claim 8, characterized in that Removing part of the epitaxial layer body to form a first trench at least in the epitaxial layer body to obtain a first epitaxial layer, comprising: dry etching the epitaxial layer body to form the first trench and the second trench spaced apart in the epitaxial layer body to obtain the first epitaxial layer including the first trench, the second trench and the epitaxial layer body; Forming a second epitaxial layer at least in the first trench where the oxide layer is formed, comprising: forming an initial epitaxial layer in the first trench where the oxide layer is formed and in the second trench; removing a portion of the initial epitaxial layer in the second trench to obtain a third trench, and forming the remaining initial epitaxial layer into a second epitaxial layer; At least after forming the second epitaxial layer in the first trench in which the oxide layer is formed, the method further includes: filling metal material in the third trench to obtain a first metal layer, wherein the first metal layer contacts the second epitaxial layer located in the second trench; and performing thermal annealing on the structure in which the first metal layer is formed to form an ohmic contact at the contact surface between the first metal layer and the second epitaxial layer.

10. The method according to claim 9, characterized in that An oxide layer is formed on the sidewall of the first trench, comprising: thermally oxidizing the first epitaxial layer formed with the first trench and the second trench to form an initial oxide layer on the surface of the first epitaxial layer away from the substrate; removing the initial oxide layer on the bottom surface of the first trench, the initial oxide layer in the second trench, and the initial oxide layer on the surface of the epitaxial layer body away from the substrate, and the remaining initial oxide layer constitutes the oxide layer.

11. The method according to claim 8, characterized in that After forming a second epitaxial layer at least in the first trench having the oxide layer formed therein, the method further comprises: Forming a second metal layer on a surface of the first epitaxial layer away from the substrate and performing a thermal annealing process to form a Schottky contact at a contact surface between the second metal layer and the epitaxial layer body; A third metal layer is formed on a surface of the substrate away from the first epitaxial layer and a thermal annealing process is performed to form an ohmic contact between the contact surface of the third metal layer and the substrate.

12. The method according to claim 11, characterized in that A second metal layer is formed on a surface of the first epitaxial layer away from the substrate and a thermal annealing process is performed to form a Schottky contact at a contact surface between the second metal layer and the epitaxial layer body, comprising: forming a first metal sublayer on a surface of the first epitaxial layer away from the substrate, the first metal sublayer being in contact with the second epitaxial layer and the oxide layer respectively; forming a second metal sublayer on a surface of the first metal sublayer away from the first epitaxial layer, and performing the thermal annealing process during the formation of the second metal sublayer, so that a Schottky contact is formed at a contact surface between the first metal sublayer and the epitaxial layer body; A third metal layer is formed on the surface of the substrate away from the first epitaxial layer and a thermal annealing process is performed, including: stacking a third metal sublayer, a fourth metal sublayer and a fifth metal sublayer in sequence on the surface of the substrate away from the first epitaxial layer, and performing the thermal annealing process so that the third metal sublayer forms an ohmic contact with the contact surface of the substrate.