Cerium-fluorine double-doped lithium-rich manganese-based positive electrode material, positive electrode, lithium battery and preparation method thereof

The short-range disordered structure is formed through cerium fluorine double-doping technology, which solves the problems of voltage attenuation and structural decay during the cycle process of lithium-rich manganese-based materials, and significantly improves the circulation performance and low-temperature performance of lithium batteries.

CN119029201AInactive Publication Date: 2024-11-26NANKAI UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411135126.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing lithium-rich manganese-based materials have voltage attenuation and structural decay problems during the circulation process, resulting in poor circulation performance of lithium batteries.

Method used

Through the cerium fluorine double-doping technology, a short-range disordered structure based on interlayers, within layers and their combinations is formed to inhibit transition metal ions migration, stabilize lattice oxygen, and adjust the oxygen band structure to improve the cycling performance of the material.

Benefits of technology

It significantly improves the circulation performance of lithium batteries, reduces voltage attenuation, improves the efficiency of the first circle of Coulomb, and shows good circulation performance under low temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119029201A_ABST
    Figure CN119029201A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium battery positive electrode materials, and discloses a cerium-fluorine double-doped lithium-rich manganese-based positive electrode material, a positive electrode, a lithium battery and a preparation method of the cerium-fluorine double-doped lithium-rich manganese-based positive electrode material. The chemical general formula of the cerium-fluorine double-doped lithium-rich manganese-based positive electrode material is xLi2MA3. (1-x) LiMA2, M is selected from at least one of Ni, Co, Mn and Ce, and x is more than or equal to 0.1 and less than or equal to 0.9; a is selected from at least one of O and F; the cerium-fluorine double-doped lithium-rich manganese-based positive electrode material has a short-distance disordered structure based on interlayer, intra-layer and combination thereof. Phase change from order to short-range partial disorder is formed in the lithium-rich phase of the positive electrode material, so that a short-range lithium-rich disorder structure and an integrated unit cell structure of doped atoms are formed, the short-range disorder structure is distributed among layers, in the layers and in the combination of the layers, lattice oxygen can be stabilized, transition metal ion migration can be inhibited, and the service life of the positive electrode material is prolonged. The capacity voltage attenuation in the cycle process is effectively inhibited, and the oxygen energy band structure can be adjusted, so that the positive electrode material has excellent cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium battery positive electrode materials, and specifically to a cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material, a positive electrode, a lithium battery, and a preparation method thereof. Background Art

[0002] With the development of various electrified equipment and devices, there is an urgent need to develop high energy density, low cost lithium-ion batteries. The energy density of lithium-ion batteries mainly depends on the energy density of the positive electrode material. High capacity and high energy density lithium-rich manganese-based materials have become the focus of current research on lithium battery positive electrode materials.

[0003] Lithium-rich manganese-based materials have a unique oxygen anion redox mechanism, which provides additional capacity and is the key to improving the energy density of lithium batteries. However, this unique anion redox is usually accompanied by irreversible oxygen release, which aggravates interface side reactions and structural decay, causing the average discharge voltage of lithium batteries to decay and affecting their cycle performance. In order to solve this problem, researchers usually adopt methods such as doping to modify the intrinsic lattice of the material to improve the electrochemical properties of the material. Among them, the doping source has a higher bond energy with oxygen anions, which inhibits the migration of transition metal ions after doping. However, although the traditional doping method has improved the electrochemical performance of lithium-rich manganese-based materials to a certain extent, it still cannot solve the problem of poor material cycle stability.

[0004] Based on this, the present application develops a new method to improve the cycle performance of lithium-rich manganese-based materials by doping to induce a disordered structure in the lithium-rich phase. Summary of the invention

[0005] The present application provides a cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material, a positive electrode, a lithium battery and a preparation method thereof, aiming to solve the problem of poor cycle stability of existing lithium-rich manganese-based materials.

[0006] In order to achieve the above objectives, the present application adopts the following technical solutions.

[0007] In a first aspect of the present application, a cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material is provided, the general chemical formula of which is xLi2MA3·(1-x)LiMA2, wherein M is selected from at least one of Ni, Co, Mn, and Ce, and 0.1≤x≤0.9; A is selected from at least one of O and F;

[0008] The cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material has a short-range disordered structure based on interlayer, intralayer and a combination thereof.

[0009] The second aspect of the present application provides a method for preparing the above-mentioned cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material, comprising:

[0010] S1, dispersing the cathode material precursor in an ethanol solution of a cerium salt, adding a fluoride salt, and stirring to obtain a mixed solution;

[0011] S2, drying the mixed solution, collecting the solid phase, grinding and mixing, and tableting to obtain a flaky intermediate product;

[0012] S3, pre-sintering the sheet-like intermediate product, and then heating it to calcine it to obtain a cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material.

[0013] In some embodiments, the cathode material precursor has a general structural formula of Li z N m (C2O4) z / 2+m , wherein z / m=1-2; N is selected from at least one of Ni, Co or Mn.

[0014] In some embodiments, the cathode material precursor is prepared by the following method:

[0015] Mixing lithium acetate and acetate of a transition metal and dissolving them in ethanol to obtain a metal ion solution; the transition metal is at least one of Ni, Co or Mn;

[0016] adding oxalic acid to the metal ion solution and stirring to obtain a suspension;

[0017] The suspension undergoes a solvent thermal reaction at 160-200° C., and the solid phase product is collected, washed, and dried to obtain a positive electrode material precursor.

[0018] In some embodiments, the drying temperature is 40-80°C; the pre-sintering temperature is 400-600°C; and the calcining temperature is 800-1000°C.

[0019] In some embodiments, the cerium salt includes at least one of cerium oxide, cerium nitrate, cerium chloride, cerium sulfate, and cerium fluoride;

[0020] and / or:

[0021] The fluoride salt includes at least one of lithium fluoride, nickel fluoride, manganese fluoride and cerium fluoride.

[0022] In some embodiments, the molar ratio of cerium ions to fluoride ions is 1:4;

[0023] The molar ratio of the cerium ion to the transition metal ion is 1:(100-1000);

[0024] The molar ratio of the fluoride ions to the oxygen atoms is 1:(60-500).

[0025] Another aspect of the present application provides the use of the above-mentioned cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material in the positive electrode of a lithium battery.

[0026] In another aspect of the present application, a lithium battery positive electrode is provided, which includes the above-mentioned cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material.

[0027] In another aspect of the present application, a lithium battery is provided, which includes the above-mentioned lithium battery positive electrode, a negative electrode that can insert and remove lithium ions or form alloys or undergo conversion reactions, and a liquid electrolyte, a semi-solid electrolyte, a quasi-solid electrolyte or a fully solid electrolyte.

[0028] Compared with the prior art, the beneficial effects of this application are:

[0029] The preparation method of the present application performs dual doping by calcining cerium and fluorine elements with a lithium-rich manganese-based material, forming a phase transition from order to short-range partial disorder in the monoclinic phase of the positive electrode material, thereby forming a short-range lithium-rich disordered structure and an integrated unit cell structure of doped atoms. The short-range disordered structure is distributed between layers, within layers, and in their combination, which can stabilize lattice oxygen, inhibit the migration of transition metal ions, effectively inhibit the capacity and voltage decay during the cycle process, and can adjust the oxygen energy band structure, so that the positive electrode material has excellent cycle performance.

[0030] The lithium battery using the cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material prepared in the present application has low voltage attenuation, high first-cycle coulombic efficiency and cycle performance, and good low-temperature cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments recorded in the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0032] Figure 1 XRD diagrams of positive electrode material 1 prepared in Example 1 and comparative material 1 prepared in Comparative Example 1;

[0033] Figure 2 is a scanning transmission electron microscope spectrum of comparative material 1;

[0034] Figure 3 is a scanning transmission electron microscope spectrum of positive electrode material 1;

[0035] Figure 4 TEM Mapping (transmission electron microscope energy spectrum scanning) diagram of positive electrode material 1;

[0036] Figure 5The first cycle charge and discharge performance diagram of the lithium battery prepared in the embodiment and the comparative battery of the comparative example;

[0037] Figure 6 The cycle performance diagram of the lithium battery prepared in the embodiment and the comparative battery of the comparative example;

[0038] Figure 7 This is a graph showing average voltage drop test results of lithium battery 1 and comparison battery 1;

[0039] Figure 8 This is a cycle performance test diagram of lithium battery 1 at 0°C;

[0040] Fig. 9 This is a test diagram of the cycle performance of lithium battery 1 at -15°C;

[0041] Fig.10 is a graph showing the full battery performance test results of lithium battery 5;

[0042] Fig.11 This is a physical picture of a lithium battery 6;

[0043] Fig.12 This is a graph showing the full battery performance test results of lithium battery 6;

[0044] Fig.13 is a graph showing the full battery performance test results of lithium battery 7;

[0045] Fig.14 This is a graph showing the full battery performance test results of lithium battery 8. DETAILED DESCRIPTION

[0046] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0047] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.

[0048] In the following description of this embodiment, the term "and / or" is used to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, B exists alone, and A and B exist at the same time. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.

[0049] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0050] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0051] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0052] Those skilled in the art will appreciate that the numerical ranges in the embodiments of the present application are to be construed as specifically disclosing each intermediate value between the upper and lower limits of the scope. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present application. The upper and lower limits of these smaller ranges may be independently included or excluded in the scope.

[0053] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which this application belongs. Although this application only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of this application. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0054] In the first aspect, the present application provides a cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material, whose general chemical formula is xLi2MA3·(1-x)LiMA2, wherein M is selected from at least one of Ni, Co, Mn, and Ce, and 0.1≤x≤0.9. In the present application, x can be 0.2, 0.3, 0.4, 0.5, 0.6, 0.7 or 0.8; A is selected from at least one of O and F.

[0055] The cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material has a short-range disordered structure based on interlayer, intralayer and a combination thereof.

[0056] In the present application, M is preferably a combination of Mn, Ni and Ce, a combination of Mn, Co and Ce, or a combination of Mn, Ni, Co and Ce, and more preferably M is a combination of Mn, Ni and Ce; A is preferably a combination of O and F.

[0057] The cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material of the present application has a crystal phase structure of a hexagonal layered structure and a monoclinic phase structure, an R-3m space group and a C / 2m space group, and a partially disordered structure based on interlayers, intralayers, and combinations thereof is formed in the monoclinic phase of the positive electrode material. The partially disordered structure, i.e., the short-range disordered structure, can stabilize the lattice oxygen and inhibit the migration of transition metal ions, thereby inhibiting the capacity and voltage decay during the cycle process.

[0058] In a second aspect, the present application provides a method for preparing the above-mentioned cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material, comprising:

[0059] S1, dispersing the cathode material precursor in an ethanol solution of a cerium salt, adding a fluoride salt, and stirring to obtain a mixed solution;

[0060] In the present application, the structural formula of the positive electrode material precursor is Li z N m (C2O4) z / 2+m , wherein z / m=1-2, preferably z=1.2, m=0.8; N is selected from at least one of Ni, Co or Mn, such as Mn and Ni, Mn and Co, Mn, Ni and Co, preferably N is Mn and Ni; preferably, the chemical formula of the positive electrode material precursor is Li 1.2 (NiMn) 0.8 (C2O4) 1.4 , more preferably Li 1.2 Ni 0.2 Mn 0.6 (C2O4) 1.4 .

[0061] In the present application, the cerium salt is used to introduce the cerium element, and the cerium salt includes at least one of cerium oxide, cerium nitrate, cerium chloride, cerium sulfate and cerium fluoride; the fluoride salt is used to introduce the fluorine element, and the fluoride salt includes at least one of lithium fluoride, nickel fluoride, manganese fluoride and cerium fluoride.

[0062] In the present application, the molar ratio of the cerium ion to the transition metal ion is 1:(100-1000), preferably 1:200; the concentration of the cerium ion in the mixed solution is 0.001mmol / L-1mol / L, preferably 0.1mmol / L. The molar ratio of the fluoride ion to the oxygen atom is 1:(60-500), preferably 1:125; the content of the fluoride ion in the mixed solution is 0.001mmol / L-1mol / L, preferably 0.4mmol / L.

[0063] In the present application, the molar ratio of cerium ions to fluoride ions in the mixed solution is preferably 1:4. The stirring time is 1-24 hours, preferably 4 hours.

[0064] S2, drying the mixed solution, collecting the solid phase, grinding and mixing, and tableting to obtain a flaky intermediate product;

[0065] The drying temperature of the mixed solution is 40 to 80°C, preferably 45°C.

[0066] S3, pre-sintering the sheet-like intermediate product, and then heating it to calcine it to obtain a cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material.

[0067] Wherein, the pre-sintering temperature is 400-600°C, the pre-sintering time is 2-8h, preferably 6h; the calcining temperature is 800-1000°C, the calcining time is 6-24h, preferably 15h.

[0068] The present application controls the reaction ratio of cerium and fluorine to effectively adjust the doping amount and the phase change structure formed in the positive electrode material, thereby achieving uniform co-doping of cerium and fluorine in the positive electrode material, and forming a phase transition from ordered to short-range partially disordered in the lithium-rich phase of the positive electrode material, thereby forming a short-range lithium-rich disordered structure and an integrated unit cell structure of doped atoms.

[0069] In the present application, the structural formula of the positive electrode material precursor is Li z N m (C2O4) z / 2+m , wherein z / m=1-2; N is selected from at least one of Ni, Co or Mn. The positive electrode material precursor is prepared by the following method:

[0070] Lithium acetate and acetate of transition metal are mixed and dissolved in ethanol to obtain a metal ion solution; the transition metal is selected from at least one of Ni, Co or Mn, such as Ni and Mn, Co and Mn, or Ni, Co and Mn.

[0071] adding oxalic acid to the metal ion solution and stirring to obtain a suspension;

[0072] The suspension is subjected to a solvent thermal reaction at 160-200° C., and the solid phase product is collected, washed, and dried to obtain a positive electrode material precursor.

[0073] The cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material prepared in the present application can be used to prepare the positive electrode of a lithium battery. Specifically, the cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material of the present application is ground and evenly dispersed with a conductive additive and an adhesive in a solvent to form a slurry, the slurry is coated on the surface of an aluminum foil current collector, and then vacuum-heated and dried to form a positive electrode film, which is cut to form a corresponding lithium battery positive electrode sheet. Among them, the mass ratio of the cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material, the conductive additive and the adhesive is preferably (70-98):(20-1):(20-1).

[0074] It should be noted that the present application does not specifically limit the types of conductive additives and adhesives. For example, the conductive additive may be one or more of graphite, acetylene black, carbon black, Ketjen black, carbon nanotubes or graphite; the adhesive may be one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer (EVA) and polyvinyl alcohol (PVA). The solvent may be N-methylpyrrolidone.

[0075] The present application also provides a lithium battery, which includes the above-mentioned lithium battery positive electrode, a negative electrode capable of inserting and removing lithium ions or forming an alloy or undergoing a conversion reaction, and a liquid electrolyte, a semi-solid electrolyte, a quasi-solid electrolyte or a fully solid electrolyte. Specifically, the positive electrode sheet and the negative electrode sheet of the lithium battery of the present application are separated by a diaphragm, and an appropriate amount of electrolyte is added to assemble a button-type lithium battery.

[0076] The lithium battery of the present application can be made of any one of graphite, lithium titanate, silicon-carbon material, lithium foil or copper foil for the negative electrode. The electrolyte is a solution obtained by dissolving different lithium salts in different organic solvents, and the concentration of the electrolyte is 0.5-4.0 mol / L, preferably about 1.0 mol / L; wherein the lithium salt can be made of a mixture of one or more of lithium perchlorate, lithium bis(trifluoromethanesulfonyl)imide or lithium hexafluorophosphate salt in any proportion; the organic solvent can be made of one or more of ethylene glycol dimethyl ether (DME), ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), fluoroethylene carbonate (FEC), fluoroethyl methyl carbonate (FEMC), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (HFE) in any proportion.

[0077] The present application is further described below by way of examples. In the examples of the present application, all reagents used can be purchased from the market, and all instruments used to perform the operations are commonly used laboratory equipment, and unless otherwise specified, all operations are performed at room temperature, normal pressure, and ventilation conditions.

[0078] Example

[0079] This embodiment provides a method for preparing a positive electrode material precursor, comprising:

[0080] Lithium acetate, nickel acetate and manganese acetate were added to ethanol in a molar ratio of 1.32:0.2:0.6 to fully dissolve to obtain a mixed metal ion solution, in which the total molar concentration of metal ions was 0.237 mol / L. Oxalic acid with a molar concentration of 0.95 mol / L was slowly added to the mixed metal ion solution in a molar ratio of oxalic acid to metal ions of 1.05:1, and stirred thoroughly to form a suspension. After stirring for 30 minutes, it was poured into a hydrothermal autoclave and subjected to a solvent thermal reaction at 180°C for 10 hours. The reaction product was filtered, washed and dried to obtain a positive electrode material precursor powder, whose chemical formula is Li 1.2 Mn 0.6 Ni 0.2 (C2O4) 1.4 .

[0081] Example 1

[0082] This embodiment provides a method for preparing a cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material, comprising:

[0083] Take 0.161 mol of the above cathode material precursor Li 1.2 Mn 0.6 Ni 0.2 (C2O4) 1.4 , added to 200ml of anhydrous ethanol solution of Ce(NO3)3 with a concentration of 3.225mmol / L, and then added 2.58mmol of lithium fluoride, stirred at a speed of 700rpm for 4h to obtain a mixed solution. The mixed solution was dried at 50℃, the solid phase was collected and fully ground, and then pressed into sheets by a tablet press at a pressure of 10MPa. The sheet material was placed in a muffle furnace and pretreated at 450℃ for 6h, and then heated to 850℃ and calcined for 15h to obtain a cerium-fluoride dual-doped lithium-rich manganese-based positive electrode material, whose chemical formula is Li 1.2 Ni 0.2 Mn 0.6 Ce 0.004 O2F 0.016 , recorded as positive electrode material 1.

[0084] Example 2

[0085] This embodiment provides a method for preparing a cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material, comprising:

[0086] Take 0.161 mol of the above cathode material precursor Li 1.2 Mn 0.6 Ni 0.2 (C2O4) 1.4 , added to 200ml of anhydrous ethanol solution of Ce(NO3)3 with a concentration of 1.66mmol / L, and then added 1.29mmol of lithium fluoride, stirred at a speed of 700rpm for 4h to obtain a mixed solution. The mixed solution was dried at 50℃, the solid phase was collected and fully ground, and then pressed into sheets by a tablet press at a pressure of 10MPa. The sheet material was placed in a muffle furnace and pretreated at 450℃ for 6h, and then heated to 850℃ and calcined for 15h to obtain a cerium-fluoride dual-doped lithium-rich manganese-based positive electrode material, whose chemical formula is Li 1.2 Ni 0.2 Mn 0.6 Ce 0.002 O2F 0.008 , recorded as positive electrode material 2.

[0087] Example 3

[0088] This embodiment provides a method for preparing a cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material, comprising:

[0089] Take 0.161 mol of the above cathode material precursor Li 1.2 Mn 0.6 Ni 0.2 (C2O4) 1.4 , added to 200ml of anhydrous ethanol solution of Ce(NO3)3 with a concentration of 4.98mmol / L, and then added 3.87mmol of lithium fluoride, stirred at a speed of 700rpm for 4h to obtain a mixed solution. The mixed solution was dried at 50℃, the solid phase was collected and fully ground, and then pressed into sheets by a tablet press at a pressure of 10MPa. The sheet material was placed in a muffle furnace and pretreated at 450℃ for 6h, and then heated to 850℃ and calcined for 15h to obtain a cerium-fluoride dual-doped lithium-rich manganese-based positive electrode material, whose chemical formula is Li 1.2 Ni 0.2 Mn 0.6 Ce 0.006 O2F 0.024 , recorded as positive electrode material 3.

[0090] Example 4

[0091] This embodiment provides a method for preparing a cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material, comprising:

[0092] Take 0.161 mol of the above cathode material precursor Li 1.2 Mn 0.6 Ni 0.2 (C2O4) 1.4 , added to 200ml of anhydrous ethanol solution of Ce(NO3)3 with a concentration of 6.45mmol / L, and then added 5.16mmol of lithium fluoride, stirred at a speed of 700rpm for 4h to obtain a mixed solution. The mixed solution was dried at 50℃, the solid phase was collected and fully ground, and then pressed into sheets by a tablet press at a pressure of 10MPa. The sheet material was placed in a muffle furnace and pretreated at 450℃ for 6h, and then heated to 850℃ and calcined for 15h to obtain a cerium-fluoride dual-doped lithium-rich manganese-based positive electrode material, whose chemical formula is Li 1.2 Ni 0.2 Mn 0.6 Ce 0.008 O2F 0.032 , recorded as positive electrode material 4.

[0093] Comparative Example 1

[0094] Comparative Example 1 provides a method for preparing an undoped lithium-rich manganese-based positive electrode material, comprising:

[0095] Take 0.161 mol of the above cathode material precursor Li 1.2 Mn 0.6 Ni 0.2 (C2O4) 1.4 The sheet material was pressed into a sheet under a pressure of 10 MPa by a sheet press, and the sheet material was placed in a muffle furnace for pretreatment at 450 ° C for 6 hours, and then heated to 850 ° C for calcination for 15 hours to obtain a lithium-rich manganese-based positive electrode material with a chemical formula of Li 1.2 Ni 0.2 Mn 0.6 O2, recorded as comparative material 1.

[0096] The cerium-fluorine dual-doped lithium-manganese-rich positive electrode material (positive electrode material 1) prepared in Examples 1-4 and the lithium-manganese-rich positive electrode material (comparative material 1) prepared in Comparative Example 1 were characterized. The results showed that the positive electrode materials prepared in Examples 1-4 all had lithium-manganese-rich R-3m and C / 2m structures.

[0097] Figure 1 XRD diagrams of positive electrode material 1 and comparative material 1. Figure 1 It can be seen that the comparative material 1 presents a lithium-manganese-rich R-3m and C / 2m structure, and the modified positive electrode material also maintains a similar structure, and no impurity phase is generated.

[0098] Figure 2 is a scanning transmission electron microscope (STEM) image of comparative material 1, Figure 3This is a scanning transmission electron microscope (STEM) image of positive electrode material 1. Figure 3 and Figure 2 Compared with the above, a disordered structure is obviously present. Figure 2 It can be seen that the lithium-rich phase of comparative material 1 exhibits an ordered structure of lithium (invisible) layers and transition metal (visible) layers, and the arrangement of the transition metal layers is a dumbbell-shaped structure of "lithium-transition metal-transition metal" without interlayer mixing. Figure 3 and Figure 2 By comparison, it can be seen that the lithium-rich phase in the positive electrode material 1 has interlayer mixing, transition metal atoms appear in the lithium layer, and the dumbbell-shaped structure of the transition metal layer also has a contrast difference, that is, some transition metal atoms in the dumbbell-shaped structure are mixed to the lithium layer.

[0099] Figure 4 TEM Mapping / Transmission Electron Microscope Energy Spectrum Scanning of the Positive Electrode Material 1. Figure 4 It can be seen that the co-doped elements Ce and F are uniformly distributed in the electrode material 1.

[0100] Through first-principles calculations, the electron state density of oxygen atoms in the structures of comparative material 1 and positive electrode material 1 was calculated, and the lone pair electron center of the O2p energy band of comparative material 1 was -0.96eV, while the lone pair electron center of the O2p energy band of positive electrode material 1 was -1.42eV, which was lower in energy. That is, the O in the modified structure is more stable.

[0101] Using first-principles calculations, the potential barriers of the transition metal ion migration paths of the comparison material 1 and the positive electrode material 1 in the deep delithiation state were calculated. From the calculation results, it can be obtained that the migration barrier after modification is 3.22eV, which is 1.93eV higher than the migration barrier of the unmodified material, that is, the modification inhibits the migration side reaction of the transition metal during the cycle.

[0102] The positive electrode materials prepared in Examples 1-4 were respectively used as active positive electrode materials to prepare positive electrodes for lithium batteries and assemble lithium batteries, and their electrochemical properties were tested.

[0103] Example 5 Preparation of lithium battery 1

[0104] This embodiment provides a method for preparing a lithium battery in which the positive electrode and the negative electrode of the lithium battery are lithium metal, comprising:

[0105] The positive electrode material 1 prepared in Example 1 was used as the active positive electrode material. The positive electrode material 1, the conductive additive SuperP, and the binder PVDF were added to the N-methylpyrrolidone solvent at a mass ratio of 8:1:1, and ground to form a uniform slurry. The slurry was applied to the surface of the aluminum foil current collector with a scraper, and dried overnight at 80°C under vacuum to obtain a positive electrode film, which was cut to obtain a positive electrode sheet. The positive electrode sheet was used as the positive electrode, lithium metal was used as the negative electrode, a solution of LiPF6 salt in a mixed solvent of EC:DMC (volume ratio of 3:7) (concentration 1M) was used as the electrolyte, a Gelgard2400 diaphragm was used as the diaphragm, and a CR2032 battery shell was used to assemble a button cell in a glove box filled with argon gas, which was recorded as lithium battery 1.

[0106] Example 6 Preparation of lithium battery 2

[0107] The difference between Example 6 and Example 5 is that the active positive electrode material is the positive electrode material 2 prepared in Example 2, which is the same as Example 5. The lithium battery prepared in Example 6 is recorded as lithium battery 2.

[0108] Example 7 Preparation of lithium battery 3

[0109] The difference between Example 7 and Example 5 is that the active positive electrode material is positive electrode material 3 prepared in Example 3, which is the same as Example 5. The lithium battery prepared in Example 7 is recorded as lithium battery 3.

[0110] Example 8 Preparation of lithium battery 4

[0111] The difference between Example 7 and Example 5 is that the active positive electrode material is positive electrode material 4 prepared in Example 4, which is the same as Example 5. The lithium battery prepared in Example 8 is recorded as lithium battery 4.

[0112] Example 9 Preparation of a lithium battery with a graphite negative electrode

[0113] The difference between Example 9 and Example 5 is that the negative electrode is replaced with graphite, and the rest is the same as Example 5.

[0114] The lithium battery prepared in Example 9 is recorded as lithium battery 5.

[0115] Example 10 Preparation of a soft-packaged lithium battery with a graphite negative electrode

[0116] The difference between Example 10 and Example 9 is that the CR2032 battery shell is replaced with an aluminum-plastic film to assemble into a soft-pack battery. The lithium battery prepared in Example 10 is recorded as lithium battery 6.

[0117] Example 11 Preparation of a lithium battery with a negative electrode made of silicon-carbon

[0118] The difference between Example 11 and Example 5 is that the negative electrode is replaced with silicon carbon, and the other parts are the same as Example 5. The lithium battery prepared in Example 9 is recorded as lithium battery 7.

[0119] Example 12 Preparation of gel lithium battery

[0120] The method for preparing the positive electrode sheet in Example 12 is the same as that in Example 5.

[0121] The positive electrode sheet was used as the positive electrode and graphite as the negative electrode. LiPF6 salt was dissolved in EC:DMC mixed solvent (volume ratio of 3:7) to prepare a 1M solution. 4wt% of triethylene glycol dimethacrylate and 20wt% of acrylate were added to the solution and polymerized to obtain a gel electrolyte. Gelgard2400 diaphragm was used as the diaphragm and CR2032 battery shell was used to assemble into a button cell in an argon-filled glove box, recorded as lithium battery 8.

[0122] Comparative Example 2

[0123] Comparative material 1 prepared in comparative example 1 was used as an active positive electrode material to prepare a positive electrode of a lithium battery and a lithium battery. The difference between comparative example 2 and example 5 is that positive electrode material 1 was replaced by comparative material 1, which is the same as example 5. The battery prepared in comparative example 1 is recorded as comparative battery 1.

[0124] The electrochemical performance of lithium batteries 1-4 prepared in Examples 5-8 and the comparative battery 1 prepared in Comparative Example 2 was tested. The test temperature was room temperature, the test voltage range was 2.0-4.8V, 1C = 200mAh g -1 , the test results are as follows Figure 5 and Figure 6 shown.

[0125] in Figure 5 The first cycle charge and discharge performance diagram of lithium batteries 1-4 and comparison battery 1. Figure 5 It can be seen that compared with the comparison battery 1, the lithium batteries 1-3 assembled with the modified materials all showed higher specific capacity and higher coulombic efficiency, that is, the side reactions of the lithium batteries 1-3, including oxygen release, were significantly alleviated.

[0126] Figure 6 The cycle performance diagram of lithium batteries 1-4 and comparative battery 1 at room temperature is shown in FIG. Figure 6 It can be seen that during the cycle process, compared with the control battery 1, the lithium batteries 1-4 assembled with the modified materials all showed higher capacity retention rates, among which the capacity retention rate of lithium battery 1 was the highest, with a capacity retention rate of 70% after 400 cycles at 1C.

[0127] Figure 7The average voltage drop test diagram of the lithium battery 1 prepared in Example 5 and the comparative battery 1 prepared in Comparative Example 2 during the cycle process is shown in FIG. Figure 7 It can be seen that compared with the average voltage drop of the comparative battery 1, the modified lithium battery 1 exhibits a higher average discharge voltage, and the attenuation during the cycle process is significantly alleviated.

[0128] Figure 8 and Fig. 9 The low temperature cycle performance test results of the lithium battery 1 prepared in Example 5, wherein the test voltage range is 2.0-4.8V, 1C=200mAh g -1 , Figure 8 This is the test result diagram at 0℃. Fig. 9 The test results at -15℃ are shown in the figure. Figure 8 and Fig. 9 It can be seen that the lithium battery 1 assembled with the modified material exhibits good cycle performance at 0°C and -15°C, that is, the material has good low-temperature performance.

[0129] The electrochemical performance of lithium batteries 5-8 prepared in Examples 9-12 was tested. The test temperature was room temperature, the test voltage range of lithium batteries 5, 6, and 8 was 2.0-4.7V, the test voltage range of lithium battery 7 was 2.0-4.55V, 1C = 200mAhg -1 .

[0130] Fig.10 The full battery performance test result diagram of lithium battery 5 with graphite as negative electrode is shown in FIG. Fig.10 It can be seen that the lithium battery assembled with the modified material and graphite has excellent cycle performance, with a capacity retention rate of 70.1% after 800 cycles.

[0131] Fig.11 This is a physical picture of a soft-pack lithium battery 6 with a graphite negative electrode. Fig.12 The following is the battery performance test result chart. Fig.12 It can be seen that the soft-pack battery assembled with the modified material and graphite has excellent cycle performance, with a capacity retention rate of 71.5% after 400 cycles.

[0132] Fig.13 This is a full battery performance test diagram of a lithium battery 7 with silicon-carbon as the negative electrode. Fig.13 It can be seen that the lithium battery assembled with the modified material and silicon-carbon has excellent cycle performance, with a capacity retention rate of 67.8% after 400 cycles.

[0133] Fig.14 This is a full battery cycle performance test diagram of the gel lithium battery 8. Fig.14It can be seen that when using gel electrolyte, the lithium battery assembled with the modified material and graphite has excellent cycle performance, with a capacity retention rate of 66.7% after 500 cycles.

[0134] The above test data show that the lithium battery using the cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material prepared in this application has low voltage attenuation, high first-cycle coulombic efficiency and cycle performance, and good low-temperature cycle performance.

[0135] Although the present application has been described in detail in general terms and in specific embodiments in this specification, it is obvious to those skilled in the art that some modifications or improvements may be made to the present application. Therefore, these modifications or improvements made without departing from the spirit of the present application are within the scope of protection claimed in the present application.

Claims

1. A cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material, It is characterized in that Its chemical formula is xLi 2 MA 3 (1-x)LiMA 2 , wherein M is selected from at least one of Ni, Co, Mn, and Ce, and 0.1≤x≤0.9; A is selected from at least one of O and F; The cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material has a short-range disordered structure based on interlayer, intralayer and a combination thereof.

2. The method for preparing the cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material according to claim 1, It is characterized in that include: S1, dispersing the cathode material precursor in an ethanol solution of a cerium salt, adding a fluoride salt, and stirring to obtain a mixed solution; S2, drying the mixed solution, collecting the solid phase, grinding and mixing, and tableting to obtain a flaky intermediate product; S3, pre-sintering the sheet-like intermediate product, and then heating it to calcine it to obtain a cerium-fluorine dual-doped lithium-rich manganese-based positive electrode material.

3. The preparation method according to claim 2, It is characterized in that The structural formula of the positive electrode material precursor is Li z N m (C 2 O 4 ) z / 2+m , wherein z / m=1-2; N is selected from at least one of Ni, Co or Mn.

4. The preparation method according to claim 3, It is characterized in that The positive electrode material precursor is prepared by the following method: Mixing lithium acetate and acetate of a transition metal and dissolving them in ethanol to obtain a metal ion solution; the transition metal is at least one of Ni, Co or Mn; adding oxalic acid to the metal ion solution and stirring to obtain a suspension; The suspension undergoes a solvent thermal reaction at 160-200° C., and the solid phase product is collected, washed, and dried to obtain a positive electrode material precursor.

5. The preparation method according to claim 2, It is characterized in that The drying temperature is 40-80°C; the pre-sintering temperature is 400-600°C; and the calcining temperature is 800-1000°C.

6. The preparation method according to claim 2, It is characterized in that The cerium salt includes at least one of cerium oxide, cerium nitrate, cerium chloride, cerium sulfate and cerium fluoride; and / or: The fluoride salt includes at least one of lithium fluoride, nickel fluoride, manganese fluoride and cerium fluoride.

7. The preparation method according to claim 2, It is characterized in that The molar ratio of the cerium ion to the fluoride ion is 1:4; The molar ratio of the cerium ion to the transition metal ion is 1:(100-1000); The molar ratio of the fluoride ions to the oxygen atoms is 1:(60-500).

8. Use of the cerium-fluorine dual-doped lithium-manganese-rich positive electrode material according to claim 1 or the cerium-fluorine dual-doped lithium-manganese-rich positive electrode material prepared by the preparation method according to any one of claims 2 to 7 in the positive electrode of a lithium battery.

9. A lithium battery positive electrode, It is characterized in that It includes the cerium-fluorine dual-doped lithium-manganese-rich positive electrode material according to claim 1, or the cerium-fluorine dual-doped lithium-manganese-rich positive electrode material prepared by the preparation method according to any one of claims 2-7.

10. A lithium battery, It is characterized in that It includes the lithium battery positive electrode as described in claim 9, a negative electrode that can insert and remove lithium ions or form an alloy or undergo a conversion reaction, and a liquid electrolyte, a semi-solid electrolyte, a quasi-solid electrolyte or a fully solid electrolyte.

Citation Information

Patent Citations

  • Preparation method of layered lithium-rich positive electrode material

    CN106169566A

  • Lithium ion battery layered positive electrode material doped with metal ions, and preparation method thereof

    CN107017402A

  • Linkage modified lithium-rich manganese-based positive electrode material and preparation method thereof

    CN111509224A

  • High-energy-efficiency lithium-manganese-rich positive electrode material as well as preparation method and application thereof

    CN117954605A