Electrolyte, battery and electric device
By using cyclic fluoroether and ionic liquid in the electrolyte, the problem of failure of traditional electrolyte at high pressure is solved, the cycle stability and safety of lithium-ion batteries are improved, and the use temperature and Battery life.
Patent Information
- Application Number
- CN202411231175.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-26
AI Technical Summary
The carbonate in the existing electrolyte causes the metal lithium to react with the electrolyte, consumes the reversible capacity of the battery, and has unstable oxidation and decomposition problems under high cutoff voltage, resulting in battery failure and safety problems.
Using an electrolyte, including organic solvents, lithium salts and diluents, the stable negative electrode SEI is generated using cycloflurane with weak coordination ability, and combined with ionic liquid to regulate the solvation structure of lithium ions, forming a uniform interface layer to improve the battery's High pressure cycle stability and safety.
By optimizing the ratio of ionic liquid to cyclofluoroether, a local super-concentrated electrolyte system is formed, free solvents are reduced, the cycling stability of the battery is improved at high cutoff voltage, the use temperature is widened, the battery life is extended, and the energy and power density is improved. At the same time, the battery safety is enhanced.
Smart Images

Figure CN119029323A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery and electrochemical technology, and in particular to an electrolyte, a battery and an electrical device. Background Art
[0002] The metal lithium negative electrode of the battery has the highest specific capacity and the lowest redox potential, and is considered to be the ultimate choice for high energy density batteries. However, existing electrolytes often contain carbonates, and metal lithium will react with the electrolyte, consuming the reversible capacity of the battery. In addition, the lithium dendrites generated during its circulation process will accelerate the consumption of lithium and electrolyte. In addition, the current commercial battery electrolyte has the problem of unstable oxidative decomposition at high cut-off voltage, which ultimately leads to battery failure and safety problems. Therefore, how to overcome the above-mentioned technical problems and defects has become a key issue that needs to be solved. Summary of the invention
[0003] Aiming at the problem that conventional carbonate electrolytes are prone to failure under high pressure, the present invention provides an electrolyte, a battery and an electrical device.
[0004] The technical solution adopted by the present invention to solve the above technical problems is as follows:
[0005] A first aspect of the present invention provides an electrolyte comprising an organic solvent and a lithium salt, wherein the organic solvent comprises an ionic liquid, a co-solvent and a diluent, the co-solvent comprises an ether solvent, and the diluent comprises a cyclopentane diluent.
[0006] Optionally, the cyclofluoroether diluent includes one or more compounds represented by the following structural formula:
[0007]
[0008] Among them, in the structural formulas Ⅰ to Ⅲ, R1-R 18 Each is independently selected from H, F, C6-C26 fluorine-substituted phenoxy or C1-C20 fluorine-substituted alkyl; and R1-R8 are not H at the same time, R9-R14 are not H at the same time, and R15-R18 are not H at the same time.
[0009] Optionally, the cyclofluoroether diluent includes one or more of 3,3,4,4-tetrafluorotetrahydrofuran, perfluorobutyltetrahydrofuran, perfluorotetrahydrofuran, diperfluorobutyltetrahydrofuran, 2-(trifluoromethyl)dioxolane, 2,2-bis(trifluoromethyl)-1,3-dioxolane, 4,4-bis(trifluoromethyl)-1,2-epoxy-5,5,5-trifluoropentane, and hexafluoropropylene oxide.
[0010] Optionally, the ionic liquid includes cations and anions, and the cations include one or more of pyrrolidine cations, imidazolium cations, piperidine cations, and pyridine cations having groups shown in structural formula I' to structural formula V':
[0011]
[0012] Wherein, R1'-R10' in the structural formula I' to the structural formula V' are independently one or more of C1-C8 alkyl and C1-C8 alkyl isomers; and / or
[0013] The anion includes one or more of anions of bistrifluoromethanesulfonyl imide, bisfluoromethanesulfonyl imide, hexafluorophosphate, tetrafluoroborate and trifluoromethanesulfonate having groups represented by structural formula VI' to structural formula X':
[0014]
[0015] Optionally, the lithium salt includes one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium trifluoromethylsulfonate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium trifluoromethylsulfonyl-perfluorobutylsulfonyl imide, lithium fluorosulfonyl-perfluorobutylsulfonyl imide, lithium bis(oxalatoborate), and lithium difluorophosphate.
[0016] Optionally, based on the total mass of the electrolyte being 100%, the percentage of the organic solvent in the total mass of the electrolyte is 50wt% to 85wt%.
[0017] Optionally, the molar ratio of the diluent, the ionic liquid, the co-solvent and the lithium salt is (0.5-8): (0.65-3): (0.6-4): (0.8-2.5).
[0018] Optionally, the co-solvent includes one or more of linear ether compounds or cyclic ether compounds.
[0019] Optionally, the co-solvent includes one or more of ethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol dibutyl ether, dioxolane, and triethylene glycol dimethyl ether.
[0020] Optionally, based on the total mass of the electrolyte being 100%, the percentage of the co-solvent in the total mass of the electrolyte is 5% to 30%.
[0021] Optionally, the electrolyte further includes additives, and the additives include one or more of fluoroethylene carbonate, 1,3-propane sultone, vinylene carbonate, vinyl sulfate, lithium nitrate, lithium borate, lithium difluorooxalatoborate, triphenyl phosphate, triethyl phosphate, and trimethyl phosphate.
[0022] Optionally, based on the total mass of the electrolyte being 100%, the percentage of the additive in the total mass of the electrolyte is 0.05% to 5%.
[0023] A second aspect of the present invention provides a battery, comprising the electrolyte, separator, positive electrode sheet and negative electrode sheet as described above.
[0024] A third aspect of the present invention provides an electrical device, comprising the battery described above.
[0025] According to the electrolyte provided by the present invention, the present invention uses cyclofluoroether with weak coordination ability to generate a stable negative electrode SEI. Compared with linear fluoroether, the coordination ability between cyclofluoroether and lithium ions is weaker, which helps to reduce the impact on the inorganic SEI formation process. The solvation structure accurately regulates the distance between the anions around the lithium ions, and it is easy to form a uniform and stable SEI layer. The use of ionic liquids not only drives a large number of anions into the Li + The solvation sheath can also participate in regulating the solvation structure through a series of weak interactions. When the solvation structure is dominated by the fluorinated anion, it can complete multiple controls of the interface, thereby broadening the battery's operating temperature, long cycle life, high energy, and high power density while also improving the battery's high-voltage cycle stability and safety. DETAILED DESCRIPTION
[0026] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0027] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0028] A first aspect of the present invention provides an electrolyte comprising an organic solvent and a lithium salt, wherein the organic solvent comprises an ionic liquid, a co-solvent and a diluent, the co-solvent comprises an ether solvent, and the diluent comprises a cyclopentane diluent.
[0029] The present invention uses cyclofluoroether with weak coordination ability to generate a stable negative electrode SEI. Compared with linear fluoroether, the coordination ability between cyclofluoroether and lithium ions is weaker, which helps to reduce the impact on the inorganic SEI formation process. The solvation structure accurately regulates the distance between anions around lithium ions, and it is easy to form a uniform and stable SEI layer. The use of ionic liquids not only drives a large number of anions into Li + The solvation sheath can also participate in regulating the solvation structure through a series of weak interactions. When the solvation structure is dominated by fluorinated anions, it can complete multiple controls of the interface, thereby improving the battery's safety while broadening its operating temperature, long cycle life, and high energy / power density.
[0030] The present invention adopts the combination of cyclofluoroether and ionic liquid to solve the problem of high-voltage failure of traditional carbonate electrolyte. By optimizing the ratio of ionic liquid with high-voltage resistance and flame retardant properties to cyclofluoroether solvent, the Li + The solvation structure generates a SEI film on the negative electrode surface and a uniform and dense interface layer (CEI) is formed on the positive electrode side, which inhibits side reactions and structural damage of the high-voltage positive electrode, and effectively improves the high-voltage cycle stability and safety of lithium-ion batteries.
[0031] In one embodiment, the cyclofluoroether diluent includes one or more compounds represented by the following structural formulas:
[0032]
[0033] Among them, in the structural formulas Ⅰ to Ⅲ, R1-R 18 Each is independently selected from H, F, C6-C26 fluorine-substituted phenoxy or C1-C20 fluorine-substituted alkyl; and R1-R8 are not H at the same time, R9-R14 are not H at the same time, and R15-R18 are not H at the same time.
[0034] By using the above-mentioned cyclofluoroether diluent and ionic liquid in combination, the problem of high-voltage failure of traditional carbonate electrolytes is solved. By optimizing the ratio of ionic liquids with high-voltage resistance and flame retardant properties to cyclofluoroether solvents, the Li + The solvation structure generates a SEI film on the negative electrode surface and a uniform and dense interface layer (CEI) is formed on the positive electrode side, which inhibits side reactions and structural damage of the high-voltage positive electrode, and effectively improves the high-voltage cycle stability and safety of lithium-ion batteries.
[0035] In one embodiment, the cyclofluoroether diluent includes one or more of 3,3,4,4-tetrafluorotetrahydrofuran, perfluorobutyltetrahydrofuran, perfluorotetrahydrofuran, diperfluorobutyltetrahydrofuran, 2-(trifluoromethyl)dioxolane, 2,2-bis(trifluoromethyl)-1,3-dioxolane, 4,4-bis(trifluoromethyl)-1,2-epoxy-5,5,5-trifluoropentane, and hexafluoropropylene oxide.
[0036] In one embodiment, the ionic liquid includes cations and anions, and the cations include one or more of pyrrolidine cations, imidazolium cations, piperidine cations, and pyridinium cations having groups represented by structural formula I' to structural formula V':
[0037]
[0038] Wherein, R1'-R10' in the structural formula I' to the structural formula V' are independently one or more of C1-C8 alkyl and C1-C8 alkyl isomers; and / or
[0039] The anion includes one or more of anions of bistrifluoromethanesulfonyl imide, bisfluoromethanesulfonyl imide, hexafluorophosphate, tetrafluoroborate and trifluoromethanesulfonate having groups represented by structural formula VI' to structural formula X':
[0040]
[0041] In a preferred embodiment, the ionic liquid comprises a mixture of one or more cations and one or more anions.
[0042] Specifically, the present invention uses an ionic liquid with a wide liquid phase range, high heat resistance, low vapor pressure, and a wide electrochemical window to form a local ultra-concentrated electrolyte system, which reduces the presence of free solvents and enables the battery system to have excellent cycle stability at a high cut-off voltage; the electrolyte system of the present invention is applied to a battery with a high cut-off voltage (>4.3V), and the introduction of the ionic liquid of the present invention not only drives a large number of anions into the Li + The solvation sheath can also regulate the solvation structure through a series of weak interactions. When the fluorinated anion dominates the solvation structure, multiple regulation of the interface can be completed, which can effectively regulate the Li + The solvation structure and derived interface can not only broaden the operating temperature of the battery, increase the long cycle life of the battery, increase the energy density and power density of the battery, but also improve the safety of the battery.
[0043] The present invention adopts cyclofluoroether and ionic liquid in combination to solve the problem of high-voltage failure of traditional carbonate electrolytes. By optimizing the ratio of ionic liquids with high-voltage resistance and flame retardant properties to cyclofluoroether solvents, the Li + The solvation structure generates a SEI film on the negative electrode surface and a uniform and dense interface layer (CEI) is formed on the positive electrode side, which inhibits side reactions and structural damage of the high-voltage positive electrode, and effectively improves the high-voltage cycle stability and safety of lithium-ion batteries.
[0044] In one embodiment, the lithium salt includes one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium trifluoromethylsulfonate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium trifluoromethylsulfonyl-perfluorobutylsulfonyl imide, lithium fluorosulfonyl-perfluorobutylsulfonyl imide, lithium bis(oxalatoborate), and lithium difluorophosphate.
[0045] Lithium salt is Li in the electrolyte + Lithium salts are the source of ions, providing the battery with free-moving ions and playing the role of transporting ions inside the battery. In addition, lithium salts can also form a protective layer on the surface of electrode materials, which has an important influence on the battery's capacity, cycle performance, power density, energy density and other properties.
[0046] In a preferred embodiment, based on the total mass of the electrolyte being 100%, the percentage of the organic solvent in the total mass of the electrolyte is 50 wt % to 85 wt %.
[0047] Specifically, the percentage of the organic solvent in the total mass of the electrolyte is any point value among 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, 80wt%, 85wt% or a range value consisting of any two point values; in a preferred embodiment, the percentage of the organic solvent in the total mass of the electrolyte is 60wt% to 80wt%.
[0048] When the percentage of the organic solvent in the total mass of the electrolyte is 50wt% to 85wt%, the cyclofluoroether and the ionic liquid are used in combination to solve the problem of high-voltage failure of traditional carbonate electrolytes. By optimizing the ratio of the ionic liquid with high-voltage resistance and flame retardant properties to the cyclofluoroether solvent, the solvation structure of Li+ can be effectively adjusted, a SEI film is generated on the surface of the negative electrode, and a uniform and dense interface layer (CEI) is formed on the positive electrode side, which inhibits side reactions and structural damage to the high-voltage positive electrode, and effectively improves the high-voltage cycle stability and safety of the lithium-ion battery.
[0049] In one embodiment, the molar ratio of the diluent, the ionic liquid, the co-solvent and the lithium salt is (0.5-8): (0.65-3): (0.6-4): (0.8-2.5).
[0050] Specifically, the molar ratio of the diluent, the ionic liquid and the lithium salt is 0.5:0.65:0.6:0.8, 1:0.65:0.6:0.8, 2:0.65:0.6:0.8, 3:0.65:0.6:0.8, 4:0.65:0.6:0.8, 5:0.65:0.6:0.8, 6:0.65:0.6:0.8, 7:0.65:0.6:0.8, 8:0.65:0.6:0.8, 8:1:0.6:0.8, 8:1 .5:0.6:0.8, 8:2:0.6:0.8, 8:2.5:0.6:0.8, 8:3:0.6:0.8, 8:3:1:0.8, 8:3:1.5:0.8, 8:3:2:0.8, 8:3:2.5:0.8, 8:3:3:0.8, 8:3:3.5:0.8, 8:3:4:0.8, 8:3:4:1, 8:3:4:1.5, 8:3:4:2, 8:3:4:2.5.
[0051] The present invention optimizes the addition ratio of ionic liquid, diluent and lithium salt to effectively adjust Li + The solvation structure of the ionic liquid not only drives a large number of anions into the Li + The solvation sheath can also regulate the solvation structure by interacting with cyclopentadiene, and when the fluorinated anion dominates the solvation structure, multiple regulation of the interface can be achieved;
[0052] In a preferred embodiment, the molar ratio of the diluent, the ionic liquid, the co-solvent and the lithium salt is (2-4): (1-2): (2-3.5): (1-1.5).
[0053] The present invention forms a local super-concentrated electrolyte system by combining a cyclofluoroether diluent with a specific ratio, thereby reducing the presence of free solvents and enabling the battery system to have excellent cycle stability at a high cut-off voltage.
[0054] In one embodiment, the co-solvent includes one or more of linear ether compounds or cyclic ether compounds.
[0055] A co-solvent electrolyte is designed by using one or more linear ether compounds or cyclic ether compounds as a cyclofluoroether diluent, which inherits the advantages of a wide electrochemical stability window and avoids the disadvantage of high viscosity.
[0056] In one embodiment, the co-solvent includes one or more of ethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol dibutyl ether, dioxolane, and triethylene glycol dimethyl ether.
[0057] A co-solvent electrolyte is designed by using one or more of ethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol dibutyl ether, dioxolane, and triethylene glycol dimethyl ether as a cyclofluoroether diluent, which inherits the advantages of its wide electrochemical stability window and avoids the disadvantage of high viscosity.
[0058] In one embodiment, based on the total mass of the electrolyte being 100%, the percentage of the co-solvent in the total mass of the electrolyte is 5% to 30%.
[0059] Specifically, the percentage of the co-solvent in the total mass of the electrolyte is 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29% or 30%, or a range of any two points; in a preferred embodiment, the percentage of the co-solvent in the total mass of the electrolyte is 10%-20%.
[0060] In one embodiment, the electrolyte further includes additives, and the additives include one or more of fluoroethylene carbonate, 1,3-propane sultone, vinylene carbonate, vinyl sulfate, lithium nitrate, lithium borate, lithium difluorooxalatoborate, triphenyl phosphate, triethyl phosphate, and trimethyl phosphate.
[0061] Specifically, fluoroethylene carbonate (FEC) additives can enhance the stability of electrode materials; 1,3-propane sultone (1,3-PS) can inhibit the occurrence of side reactions on the electrode surface and the dissolution of metal ions, increase the initial capacity of the battery, improve the high and low temperature storage performance of the battery, increase the number of battery cycles and extend the service life; vinylene carbonate (VC) can form a solid electrolyte interface film (SEI film) by electrochemical reaction on the surface of the negative electrode during the initial charge and discharge of the battery. Vinyl sulfate can inhibit the decrease in the initial capacity of the battery, increase the initial discharge capacity, reduce the expansion of the battery after high temperature storage, and improve the charge and discharge performance and cycle number of the battery.
[0062] In one embodiment, based on the total mass of the electrolyte being 100%, the percentage of the additive in the total mass of the electrolyte is 0.05% to 5%.
[0063] Specifically, the percentage of the additive in the total mass of the electrolyte is 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, or a range of any two points; in a preferred embodiment, the percentage of the additive in the total mass of the electrolyte is 0.5%-2%.
[0064] In a preferred embodiment, monomers and initiators are added to the electrolyte, which is heated and cured to form a gel electrolyte.
[0065] Specifically, the monomer includes one or more of sulfonic acid group-containing vinyl monomers, acrylamide monomers, and acrylate monomers; specifically, the sulfonic acid group-containing vinyl monomers include one or more of 2-acrylamide-2-methylpropane sodium sulfonate, 2-acrylamide sodium dodecyl sulfonate, sodium dodecyl sulfonate, and 2-acrylamide sodium octane sulfonate; specifically, the acrylamide monomers include one or more of acrylamide, methacrylamide, isopropyl acrylamide, N,N-diethylacrylamide, isobutoxymethyl acrylamide, and diacetone acrylamide; specifically, the acrylate monomers include one or more of butyl acrylate, methyl acrylate, ethyl acrylate, 2-methyl methacrylate, and isooctyl acrylate.
[0066] Specifically, the initiator includes one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphosphonate, methyl o-benzoylbenzoate, benzophenone, 4-phenylbenzophenone, and ethyl 4-dimethylaminobenzoate; preferably, the lithium salt is selected from one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium perchlorate, lithium tetrafluoroborate, lithium dioxalatoborate, lithium difluorophosphate, lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium difluorooxalatoborate, and lithium hexafluoroarsenate.
[0067] In one embodiment, taking the total mass of the gel electrolyte as 100%, the percentage of the electrolyte in the total mass of the gel electrolyte is 0.5% to 50%; the percentage of the monomer in the total mass of the gel electrolyte is 49.9% to 99.49%; and the percentage of the initiator in the total mass of the gel electrolyte is 0.01% to 0.1%.
[0068] Specifically, the percentage of the electrolyte to the total mass of the gel electrolyte is 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, 100%, 101%, 102%, 103%, 104%, 105%, 106%, 107%, 108%, 109%, 110%, 0%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49% or 50%, or a range of any two points; in a preferred embodiment, the percentage of the electrolyte in the total mass of the gel electrolyte is 10%-40%.
[0069] Specifically, the percentage of the monomer in the total mass of the gel electrolyte is any point value of 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17% or 18%, or a range value consisting of any two point values; in a preferred embodiment, the percentage of the monomer in the total mass of the gel electrolyte is 12%-16%.
[0070] Specifically, the percentage of the electrolyte in the total mass of the gel electrolyte is any point value among 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09% or 0.1%, or a range value consisting of any two point values; in a preferred embodiment, the percentage of the initiator in the total mass of the gel electrolyte is 0.02%-0.08%.
[0071] Furthermore, in one embodiment, an electrolyte is added to the solid electrolyte to form a semi-solid electrolyte.
[0072] Specifically, the solid electrolyte includes an inorganic solid electrolyte, a polymer solid electrolyte and a composite solid electrolyte, the inorganic solid electrolyte includes one or more of an oxide solid electrolyte, a sulfide solid electrolyte and a halide solid electrolyte; the polymer solid electrolyte includes a polymer matrix, the polymer matrix is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer; the composite solid electrolyte includes an inorganic filler and a polymer matrix, the inorganic filler is selected from at least one of an inert filler and an active filler, the inert filler is one or more of silicon dioxide, titanium dioxide, aluminum oxide, metal organic framework (MOFs) and zeolite; the active filler is one or more of cubic garnet lithium lanthanum zirconium oxide (LLZO), lithium lanthanum zirconium tantalum oxide (LLZTO), NASICON type lithium aluminum titanium phosphate (LATP), perovskite type lithium lanthanum titanium oxide, sulfide electrolyte and halide electrolyte; the polymer matrix includes one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene and its derivatives, polyacrylonitrile, polymethyl methacrylate, or polyethyl methacrylate and its derivatives.
[0073] In one embodiment, taking the total mass of the solid electrolyte as 100%, the percentage of the electrolyte in the total mass of the solid electrolyte is 0.5%-50%.
[0074] Specifically, the percentage of the electrolyte to the total mass of the solid electrolyte is 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, 100%, 101%, 102%, 103%, 104%, 105%, 106%, 107%, 108%, 109%, 110 0%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49% or 50%, or a range of any two points; in a preferred embodiment, the percentage of the electrolyte in the total mass of the solid electrolyte is 10%-40%.
[0075] A second aspect of the present invention provides a battery, comprising the electrolyte, separator, positive electrode sheet and negative electrode sheet as described above.
[0076] Specifically, the diaphragm can be selected from one or more materials such as polypropylene (PP), polyethylene (PE), PP / PE / PP composite film, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ceramic diaphragm, ceramic polyamide (PI), aramid (AF), non-woven fabric, etc.
[0077] In a preferred embodiment, the production of the battery includes the following steps:
[0078] The positive electrode sheet, the separator and the negative electrode sheet are stacked in order, so that the separator is located between the positive and negative electrodes to play an isolating role. The electrode sheet and the separator are placed in an aluminum-plastic film bag formed by punching and shelling by stacking. The electrolyte, gel electrolyte or solid electrolyte prepared as above are respectively injected into the baked and dried battery cells. After vacuum packaging, standing, formation and other processes, a battery is obtained.
[0079] In one embodiment, the positive electrode sheet includes a positive electrode active material, and the positive electrode active material includes one or more of lithium iron phosphate (LFP), lithium iron manganese phosphate (LMFP), lithium cobalt oxide (LCO), lithium manganese oxide (LMO), lithium nickel oxide (LNO), ternary materials (NCM, NCA), lithium manganese-rich base (LMR), lithium nickel manganese oxide (LNMO), and lithium vanadium phosphate (Li3V2(PO4)3, LiVOPO4).
[0080] Specifically, when the electrolyte system is matched with a high-voltage positive electrode, including ternary materials and lithium-rich manganese-based materials, the high-voltage solvent system includes ionic liquids and cyclofluoroethers to form a local super-concentrated system with good flame retardant properties. The mixed solvent system generates stable SEI and CEI through solvation structure regulation, providing a stable circulation basis for the battery system under high voltage conditions and improving the safety characteristics of the battery.
[0081] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on one side or both sides of the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material, a conductive agent, and a binder.
[0082] In some embodiments, the positive electrode conductive agent includes one or more of graphite, superconducting carbon, acetylene black, carbon black, carbon nanotubes, graphene, carbon nanofibers, metal powder, metal fibers, and polyphenylene derivatives.
[0083] In some embodiments, the positive electrode binder includes one or more of polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.
[0084] In some embodiments, the mass percentage of each component in the positive electrode active material layer is: 96-98 wt % of positive electrode active material, 0.5-2 wt % of conductive agent, and 1.0-2.0 wt % of binder.
[0085] When the mass ratio of the positive electrode active material in the positive electrode active material layer is within the above range, the positive electrode plate can have a higher lithium removal and lithium insertion capacity, and the battery can have a higher capacity.
[0086] The positive electrode current collector is selected from a metal material that can conduct electrons. Preferably, the positive electrode current collector includes one or more of copper, nickel, tin, copper, and stainless steel. In a more preferred embodiment, the positive electrode current collector is selected from aluminum foil.
[0087] The positive electrode sheet can be prepared according to conventional methods in the art. For example, the positive electrode active material layer is usually prepared by coating a positive electrode slurry made of a positive electrode active material, a positive electrode conductive agent, a positive electrode binder and any other components on a positive electrode current collector, followed by drying and cold pressing. The solvent can be N-methylpyrrolidone (NMP), but is not limited thereto.
[0088] In one embodiment, the negative electrode sheet includes a negative electrode active material, and the negative electrode active material includes one or more of a graphite negative electrode material, a silicon-oxygen negative electrode material, a silicon-carbon negative electrode material, a silicon negative electrode material, a tin negative electrode material, a tin oxide negative electrode material, a tin alloy negative electrode material (Sn-Fe, Sn-Co, Sn-Cu, etc.), a lithium metal negative electrode material, a lithium alloy negative electrode material (Li-Ag, Li-Al, Li-Sn, Li-Mg, Li-Zn, Li-In, Li-Ga, etc.), and a lithium-free negative electrode material.
[0089] The electrolyte of the present invention can be used in a high-voltage battery system, matched with a high-voltage ternary positive electrode and a lithium-manganese-rich positive electrode, a graphite negative electrode, a silicon-carbon negative electrode, a silicon-oxygen negative electrode, and a lithium metal negative electrode, and is used to make liquid, semi-solid laminated, wound or cylindrical batteries. The electrolyte of the present invention provides a stable circulation basis for the battery system under high voltage conditions, thereby improving the safety characteristics of the battery.
[0090] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on one or both sides of the negative electrode current collector, and the negative electrode active material layer includes a negative electrode active material, a conductive agent, a binder, and a thickener.
[0091] In some embodiments, the negative electrode conductive agent includes one or more of graphite, superconducting carbon, acetylene black, carbon black, carbon nanotubes, graphene, carbon nanofibers, metal powders, metal fibers, and polyphenylene derivatives.
[0092] In some embodiments, the negative electrode binder includes one or more of styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, and polymethacrylic acid.
[0093] In some embodiments, the thickener includes one or more of sodium alginate, sodium carboxymethyl cellulose, and carboxymethyl chitosan.
[0094] In some embodiments, the mass percentage of each component in the negative electrode active material layer is: 96%-97% of negative electrode active material, 0.5%-1.5% of conductive agent, 1%-2% of binder and 0.5%-1.5% of thickener.
[0095] The mass ratio of the negative electrode active material and the mesoporous material in the negative electrode film layer is within the above range, which allows the mesoporous material to be in full contact with the active material, and enables the electrolyte stored in the mesopores to be directly transported to the active material. At the same time, lithium reaches the active material interface faster through the mesopores, and the improvement effects on kinetics, circulation, etc. are better.
[0096] The negative electrode current collector is selected from metal materials that can conduct electrons. Preferably, the negative electrode current collector includes one or more of Al, Ni, tin, copper, and stainless steel. In a more preferred embodiment, the negative electrode current collector is selected from copper foil.
[0097] The negative electrode sheet can be prepared according to conventional methods in the art. For example, the negative electrode active material layer is usually prepared by coating a negative electrode slurry made of a negative electrode active material, a negative electrode conductive agent, a negative electrode binder and any other components on a negative electrode current collector, followed by drying and cold pressing. The solvent can be an aqueous solvent, but is not limited thereto.
[0098] A third aspect of the present invention provides an electrical device, comprising the battery described above.
[0099] The third aspect of the present invention provides an electric device, which includes the battery described in the second aspect of the present invention. The battery is used as a power source for the device. The number of batteries in the electric device can be adjusted according to the application and capacity of the electric device.
[0100] Preferably, the electrical device may be, but is not limited to, electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0101] The beneficial effects of the present invention are further illustrated below in conjunction with embodiments.
[0102] In order to make the invention purpose, technical scheme and beneficial technical effect of the present invention clearer, the present invention is further described in detail below in conjunction with examples. However, it should be understood that the examples of the present invention are only for explaining the present invention, not for limiting the present invention, and the examples of the present invention are not limited to the examples given in the specification. The specific experimental conditions or operating conditions not specified in the examples are made under conventional conditions, or are made under the conditions recommended by the material supplier.
[0103] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0104] In the following examples, the reagents, materials and instruments used, unless otherwise specified, can be purchased commercially or obtained by synthetic methods known in the art.
[0105] Table 1 Design of electrolytes of Examples 1-7 and Comparative Examples 1-3;
[0106]
[0107] Example 1
[0108] This embodiment is used to illustrate the electrolyte and battery disclosed in the present invention; it includes the following operating steps:
[0109] Preparation of electrolyte: In a glove box filled with argon (O2 <1ppm, H2O <1ppm), the ionic liquid Pyr13FSI, the co-solvent DME, and the cyclofluoroether solvent TFF are mixed in a mass ratio of 4:4:7, stirred evenly to obtain a mixed solvent, 25% lithium salt LiFSI is slowly added to the mixed solvent, and finally 0.05% LiNO3 is added to obtain the electrolyte.
[0110] Preparation of positive electrode sheet: Mix the positive electrode active material lithium nickel cobalt manganese oxide (NCM), the conductive agent CNT, and the adhesive PVDF in a mass ratio of 97:1.5:1.5. Stir and mix thoroughly in NMP solvent to form a uniform positive electrode slurry. Apply this slurry on at least one side of the positive electrode current collector aluminum foil, and after drying, rolling, die-cutting and other processes, a positive electrode sheet that meets the requirements is obtained.
[0111] Production of negative electrode sheet: The negative electrode uses a copper-lithium composite strip with a metal lithium thickness of 20um.
[0112] Preparation of diaphragm: PE porous polymer film is used as the diaphragm substrate;
[0113] Battery production:
[0114] The positive electrode sheet, the separator and the negative electrode sheet are stacked in order, and the separator is placed between the positive and negative electrodes to play an isolating role. Then the stacked electrode sheets and the separator are placed in the aluminum-plastic film bag formed by punching and forming. The non-aqueous electrolyte prepared above is respectively injected into the baked and dried battery cells. After vacuum packaging, standing, formation and other processes, a battery with a capacity of 1Ah is obtained.
[0115] Embodiment 2-7
[0116] Examples 2-7 are used to illustrate the electrolyte and battery disclosed in the present invention, and include most of the operating steps in Example 1, except that:
[0117] The components and contents of the organic solvent in the electrolyte shown in Table 1 were used.
[0118] Comparative Examples 1-3
[0119] Comparative Examples 1-3 are used to illustrate the electrolyte and battery disclosed in the present invention, and include most of the operating steps in Example 1, except that:
[0120] The components and contents of the organic solvent in the electrolyte shown in Table 1 were used.
[0121] Performance Testing
[0122] The following performance tests were performed on the batteries prepared in Examples 1 to 7 and Comparative Examples 1 to 3:
[0123] (1) Electrolyte oxidation potential test: The linear scanning potential method was used to test the oxidation potential of the electrolyte membrane using the EC-Lab electrochemical workstation. The test voltage range was 2.5 to 6 V and the scanning rate was 1 mV·s-1. This method used a "stainless steel sheet | membrane | lithium sheet" device structure for testing, with the stainless steel sheet as the working electrode and the lithium sheet as the reference electrode.
[0124] (2) Battery cell cycle performance test: In the voltage range of 3.0V ~ 4.3V, temperature 25℃, 0.2C / 0.5D cycle charge and discharge test, record the capacity retention rate of the battery after 100 cycles, and the average efficiency of battery charge and discharge.
[0125] The test results are shown in Table 2.
[0126] Table 2 Electrochemical performance of lithium battery
[0127] Electrochemical window / V Average charge and discharge efficiency Capacity retention rate Example 1 5.20 99.85% 94% Example 2 5.15 99.70% 93% Example 3 5.15 99.75% 92% Example 4 5.05 99.68% 93% Example 5 5.10 99.71% 92% Example 6 5.00 99.56% 91% Example 7 5.18 99.63% 90% Comparative Example 1 4.65 98.70% 82% Comparative Example 2 4.78 98.81% 80% Comparative Example 3 5.00 98.79% 79%
[0128] As shown in Table 2, when the electrolyte lacks cyclopentadiene or ionic liquid, the electrochemical window is reduced, the average charge and discharge efficiency of the battery is reduced, the battery capacity retention rate is reduced, and the battery performance is poor. By adding cyclopentadiene with weak coordination ability to the electrolyte to generate a stable negative electrode SEI,
[0129] Comparative Example 3 uses linear fluoroether. Compared with Comparative Example 3, when cyclofluoroether is used in the electrolyte, Examples 1-7 have weaker coordination ability between cyclofluoroether and lithium ions, which helps to reduce the impact on the inorganic SEI formation process, and the solvation structure accurately regulates the distance between the anions around the lithium ions, and it is easy to form a uniform and stable SEI layer. The combination of ionic liquids not only drives a large number of anions into the Li+ solvation sheath, but also participates in regulating the solvation structure through a series of weak interactions. When the fluorinated anions dominate the solvation structure, multiple interfaces are regulated, which improves the battery's safety while broadening its operating temperature, long cycle life, and high energy / power density.
[0130] In summary, the present invention adopts the combination of cyclofluoroether and ionic liquid to solve the problem of high-voltage failure of traditional carbonate electrolyte. By optimizing the ratio of ionic liquid with high-voltage resistance and flame retardant properties to cyclofluoroether solvent, the Li + The solvation structure generates a SEI film on the negative electrode surface and a uniform and dense interface layer (CEI) is formed on the positive electrode side, which inhibits side reactions and structural damage of the high-voltage positive electrode, and effectively improves the high-voltage cycle stability and safety of lithium-ion batteries.
[0131] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An electrolyte, characterized in that: The invention comprises an organic solvent and a lithium salt. The organic solvent comprises an ionic liquid, a co-solvent and a diluent. The co-solvent comprises an ether solvent. The diluent comprises a cyclofluoroether diluent.
2. The electrolyte according to claim 1, characterized in that: The cyclofluoroether diluent includes one or more compounds shown in the following structural formula: Among them, in the structural formulas Ⅰ to Ⅲ, R1-R 18 Each is independently selected from H, F, C6-C26 fluorine-substituted phenoxy or C1-C20 fluorine-substituted alkyl; and R1-R8 are not H at the same time, R9-R14 are not H at the same time, and R15-R18 are not H at the same time.
3. The electrolyte according to claim 2, characterized in that: The cyclofluoroether diluent includes one or more of 3,3,4,4-tetrafluorotetrahydrofuran, perfluorobutyltetrahydrofuran, perfluorotetrahydrofuran, diperfluorobutyltetrahydrofuran, 2-(trifluoromethyl)dioxolane, 2,2-bis(trifluoromethyl)-1,3-dioxolane, 4,4-bis(trifluoromethyl)-1,2-epoxy-5,5,5-trifluoropentane, and hexafluoropropylene oxide.
4. The electrolyte according to claim 1, characterized in that: The ionic liquid includes cations and anions, wherein the cations include one or more of pyrrolidine cations, imidazolium cations, piperidine cations, and pyridine cations having groups shown in structural formula I' to structural formula V': Wherein, R1'-R10' in the structural formula I' to the structural formula V' are independently one or more of C1-C8 alkyl and C1-C8 alkyl isomers; and / or The anion includes one or more of anions of bistrifluoromethanesulfonyl imide, bisfluoromethanesulfonyl imide, hexafluorophosphate, tetrafluoroborate and trifluoromethanesulfonate having groups represented by structural formula VI' to structural formula X':
5. The electrolyte according to claim 1, characterized in that: The lithium salt includes one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium trifluoromethylsulfonate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium trifluoromethylsulfonyl-perfluorobutylsulfonylimide, lithium fluorosulfonyl-perfluorobutylsulfonylimide, lithium bis(oxalatoborate), and lithium difluorophosphate.
6. The electrolyte according to claim 1, characterized in that: Taking the total mass of the electrolyte as 100%, the percentage of the organic solvent in the total mass of the electrolyte is 50wt% to 85wt%.
7. The electrolyte according to claim 1, characterized in that: The molar ratio of the diluent, the ionic liquid, the co-solvent and the lithium salt is (0.5-8): (0.65-3): (0.6-4): (0.8-2.5).
8. The electrolyte according to claim 1, characterized in that: The co-solvent includes one or more of linear ether compounds or cyclic ether compounds.
9. The electrolyte according to claim 8, characterized in that: The co-solvent includes one or more of ethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol dibutyl ether, dioxolane, and triethylene glycol dimethyl ether.
10. The electrolyte according to claim 8, characterized in that: Taking the total mass of the electrolyte as 100%, the percentage of the co-solvent in the total mass of the electrolyte is 5% to 30%.
11. The electrolyte according to claim 1, characterized in that: The electrolyte also includes additives, which include one or more of fluoroethylene carbonate, 1,3-propane sultone, vinylene carbonate, vinyl sulfate, lithium nitrate, lithium borate, lithium difluorooxalatoborate, triphenyl phosphate, triethyl phosphate, and trimethyl phosphate.
12. The electrolyte according to claim 11, characterized in that: Taking the total mass of the electrolyte as 100%, the percentage of the additive in the total mass of the electrolyte is 0.05% to 5%.
13. A battery, characterized in that: The invention comprises an electrolyte, a separator, a positive electrode sheet and a negative electrode sheet as described in any one of claims 1 to 12.
14. An electrical device, characterized in that: Comprising a battery according to claim 13.
Citation Information
Patent Citations
Low-temperature battery electrolytic solution based on ionic liquid, preparation method and application thereof
CN112952194A
Electrolyte and lithium ion battery
CN113889671A
Composition
CN114556660A
Lithium metal secondary electrolyte and lithium metal secondary battery
CN114792806A
Lithium battery electrolyte and secondary battery
CN114976251A