EL device and method for manufacturing same
By adopting a combined sealing structure of a thin organic barrier layer and an inorganic protective layer in the OLED display device, the problems of limited bending and insufficient moisture resistance caused by the thick barrier layer are solved, and more efficient mass production and moisture resistance are achieved.
Patent Information
- Application Number
- CN202411363591.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2018-04-20
- Publication Date
- 2024-11-26
AI Technical Summary
In the thin film sealing structure of the existing OLED display device, the thick organic barrier layer causes limited bending. When printing techniques such as inkjet are formed, the mass production is low and the moisture resistance is insufficient, especially in the inorganic barrier layer and the organic one. Outside the contact area of the barrier layer, water vapor is easily inlet.
By adopting a thin film sealing structure with a thin organic barrier layer, an organic planarization layer is formed on the inorganic protective layer and an EL element layer is formed thereon, and a sealing structure is formed by using the joint portion between the inorganic barrier layer and the organic barrier layer to ensure that Water vapor does not enter, and an organic barrier layer is formed by a photocurable resin to improve moisture resistance.
The mass production and moisture resistance of the OLED display device are improved, ensuring that the thinner organic barrier layer does not affect the bending of the components, and at the same time, it effectively prevents water vapor from entering, improving the overall sealing performance.
Smart Images

Figure CN119031747A_ABST
Abstract
Description
This application is a divisional application with application number 201880092554.5, application date October 20, 2020, and invention name “Organic EL device and its manufacturing method”. Technical Field
[0001] The present invention relates to an EL device (eg, an organic EL display device and an organic EL lighting device) and a method for manufacturing the same. Background Art
[0002] Organic EL (Electro Luminescence) display devices have come into practical use. One of the characteristics of organic EL display devices is that they can be flexible displays. Organic EL display devices have at least one organic EL element (Organic Light Emitting Diode: OLED) and at least one TFT (Thin Film Transistor) for controlling the current supplied to each OLED for each pixel. Hereinafter, the organic EL display device will be referred to as an OLED display device. In this way, an OLED display device having a switching element such as a TFT for each OLED is called an active matrix OLED display device. In addition, a substrate on which TFTs and OLEDs are formed is referred to as an element substrate.
[0003] OLED (especially the organic light-emitting layer and cathode electrode materials) is easily degraded by moisture and prone to uneven display. As a technology to provide a sealing structure that protects OLED from moisture without damaging flexibility, thin film encapsulation (TFE) technology has been developed. Thin film encapsulation technology uses thin films to obtain sufficient water vapor barrier properties by alternately stacking inorganic barrier layers and organic barrier layers. From the perspective of moisture resistance reliability of OLED display devices, the WVTR (Water Vapor Transmission Rate) of thin film sealing structures is usually required to be 1×10 -4 g / m 2 / day or less.
[0004] The thin film sealing structure used in the currently commercially available OLED display device has an organic barrier layer (polymer barrier layer) with a thickness of about 5um to about 20um. In this way, the relatively thick organic barrier layer also plays a role in flattening the surface of the element substrate. However, when the organic barrier layer is thick, there is a problem that the bendability of the OLED display device is limited.
[0005] In addition, there is also a problem of low mass productivity. The relatively thick organic barrier layer mentioned above is formed using printing techniques such as inkjet method and microjet method. On the other hand, the inorganic barrier layer is formed in a vacuum atmosphere (for example, below 1 Pa) using thin film forming technology. Since the formation of the organic barrier layer using printing technology is carried out in the air or nitrogen atmosphere, and the formation of the inorganic barrier layer is carried out in a vacuum, in the process of forming the thin film sealing structure, the component substrate is taken out of the vacuum chamber and put in, and mass productivity is low.
[0006] Therefore, as disclosed in Patent Document 1, for example, a film forming apparatus has been developed that can continuously produce an inorganic barrier layer and an organic barrier layer.
[0007] In addition, a thin film sealing structure is disclosed in patent document 2, when the first inorganic material layer, the first resin material and the second inorganic material layer are formed in sequence from the element substrate side, the first resin material is unevenly distributed around the convex portion of the first inorganic material layer (the first inorganic material layer covering the convex portion). According to patent document 2, moisture and oxygen are inhibited from invading from the part by unevenly distributing the first resin material around a convex portion that may not be fully covered by the first inorganic material layer. In addition, by making the first resin material function as the base layer of the second inorganic material layer, the second inorganic material layer is appropriately film-formed, and the side of the first inorganic material layer can be appropriately covered with the desired film thickness. The first resin material is formed as follows. The heated and vaporized mist-like organic material is supplied to the element substrate maintained at a temperature below room temperature, and the organic material condenses on the substrate and drops. The drop-shaped organic material moves on the substrate through capillary phenomenon or surface tension, and is unevenly distributed on the side of the convex portion of the first inorganic material layer and the boundary portion of the substrate surface. Then, the first resin material is formed by solidifying the organic material at the boundary portion. Patent Document 3 discloses an OLED display device having a similar thin film sealing structure. Patent Document 4 discloses a film forming device for manufacturing an OLED display device. Prior art literature Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2013-186971 Patent Document 2: International Publication No. 2014 / 196137 Patent Document 3: Japanese Patent Application Publication No. 2016-39120 Patent Document 4: Japanese Patent Application Publication No. 2013-64187 Summary of the invention Technical Problems to be Solved by the Invention
[0009] It is considered that the thin film sealing structure described in Patent Document 2 or Patent Document 3 does not have a thick organic barrier layer, and therefore the bendability of the OLED display device is improved. In addition, since the inorganic barrier layer and the organic barrier layer can be formed continuously, mass productivity is also improved.
[0010] However, according to the research of the present inventors, when the organic barrier layer is formed by the method described in Patent Document 2 or Patent Document 3, there may be a problem that sufficient moisture resistance reliability cannot be obtained.
[0011] When the organic barrier layer is formed by a printing method such as an inkjet method, the organic barrier layer is formed only in the active area (sometimes also referred to as the "element formation area" or "display area") on the element substrate, and may not be formed in areas other than the active area. Therefore, around the active area (outside), there is an area where the first inorganic material layer and the second inorganic material layer are in direct contact, and the organic barrier layer is completely surrounded by the first inorganic material layer and the second inorganic material layer and isolated from the surroundings.
[0012] In contrast, in the method for forming an organic barrier layer described in Patent Document 2 or Patent Document 3, a resin (organic material) is supplied to the entire surface of the element substrate, and the surface tension of the liquid resin is used to unevenly distribute the resin on the side of the convex portion of the surface of the element substrate and the boundary portion of the substrate surface. Therefore, an organic barrier layer is also formed in the area outside the active area (sometimes also referred to as the "peripheral area"), that is, the terminal area where a plurality of terminals are arranged, and the lead wiring area where lead wiring from the active area to the terminal area is formed. Specifically, for example, the resin is unevenly distributed on the boundary portion between the side of the lead wiring and the terminal and the substrate surface. In this way, the end of the portion of the organic barrier layer formed along the lead wiring is not surrounded by the first inorganic barrier layer and the second inorganic barrier layer, and is exposed to the atmosphere (peripheral atmosphere).
[0013] The organic barrier layer has lower water vapor barrier properties than the inorganic barrier layer. Therefore, the organic barrier layer formed along the lead wiring serves as a path for introducing water vapor in the atmosphere into the active region.
[0014] Here, although the problem of the thin film sealing structure applicable to the flexible organic EL display device is described, the thin film sealing structure is not limited to the organic EL display device, and can also be used for other organic EL devices such as organic EL lighting devices.
[0015] The present invention is made to solve the above-mentioned problems, and its object is to provide an EL device having a thin film sealing structure with a thin organic barrier layer and improved mass productivity and moisture resistance reliability, and a manufacturing method thereof. Technical solutions for solving technical problems
[0016] An EL device according to one embodiment of the present invention comprises: a substrate; a driving circuit layer, the driving circuit layer comprising: a plurality of TFTs formed on the substrate, a plurality of gate buses and a plurality of source buses respectively connected to any one of the plurality of TFTs, a plurality of terminals, and a plurality of lead wirings connecting the plurality of terminals to any one of the plurality of gate buses or the plurality of source buses; a first inorganic protective layer formed on the driving circuit layer, exposing at least the plurality of terminals; an organic planarizing layer, which is an organic planarizing layer formed on the first inorganic protective layer, the organic planarizing layer having a surface with an arithmetic mean roughness Ra of less than 50 nm; an EL element layer, which is formed on the organic planarizing layer and has a plurality of EL elements respectively connected to any one of the plurality of TFTs; a thin film sealing structure, which is formed in a manner covering the EL element layer and has a first inorganic barrier layer, a plurality of EL elements respectively connected to any one of the plurality of TFTs; and a plurality of lead wirings connecting the plurality of terminals to any one of the plurality of gate buses or the plurality of source buses. an organic barrier layer in contact with the upper surface of the first inorganic barrier layer and a second inorganic barrier layer in contact with the upper surface of the organic barrier layer, the organic barrier layer being formed in an area surrounded by an inorganic barrier layer joint portion where the first inorganic barrier layer and the second inorganic barrier layer are in direct contact, the organic planarization layer being formed in the area where the first inorganic protective layer is formed when observed from the normal direction of the substrate, the plurality of EL elements being arranged in the area where the organic planarization layer is formed, the outer edge of the thin film sealing structure intersecting the plurality of lead wirings and existing between the outer edge of the organic planarization layer and the outer edge of the first inorganic protective layer, and in the portion where the first inorganic protective layer and the first inorganic barrier layer are in direct contact on the plurality of lead wirings, a taper angle of the side surface of the shape of the cross section of the first inorganic barrier layer parallel to the line width direction of the plurality of lead wirings is less than 90°.
[0017] In one embodiment, the EL device further includes a second inorganic protective layer formed on the organic planarization layer, and the EL element layer is formed on the second inorganic protective layer.
[0018] In one embodiment, the taper angle of the side surface of the first inorganic barrier layer is less than 70°.
[0019] In one embodiment, the organic planarization layer is formed of a photosensitive resin.
[0020] In one embodiment, the organic planarization layer is formed of polyimide.
[0021] A method for manufacturing an EL device according to one embodiment of the present invention, the manufacturing method is the method for manufacturing an EL device described in any one of the above-mentioned descriptions, the manufacturing method comprising step A, forming the driving circuit layer on the substrate; step B, forming a first inorganic protective film on the driving circuit layer; step C, forming an organic planarizing film on the first inorganic protective film; step D, performing chemical mechanical polishing on the surface of the organic planarizing film; step E, obtaining the first inorganic protective layer and the organic planarizing layer by patterning the first inorganic protective film and the organic planarizing film; step F, heating the organic planarizing layer to a temperature above 100°C; and step G, after step F, forming a layer included in the EL element on the organic planarizing layer.
[0022] In one embodiment, after step D and before step E, the method further includes: forming a second inorganic protective film on the organic planarization film; and uniformly forming contact holes penetrating the first inorganic protective film, the organic planarization film, and the second inorganic protective film.
[0023] In one embodiment, after the process E and before the process F, it also includes: a process El, forming a positive photoresist film covering the organic planarization layer; and a process E2, removing the photoresist film by exposing the entire surface of the photoresist film and then developing it.
[0024] In one embodiment, a step of storing or transporting the substrate on which the photoresist film is formed is included between the step E1 and the step E2.
[0025] In one embodiment, the manufacturing method further includes: step H, after step G, selectively forming the first inorganic barrier layer in the active area where the multiple EL elements are formed; step I, after step H, disposing the substrate in a chamber and supplying vapor or mist of photocurable resin into the chamber; step J, which is a step of condensing the photocurable resin on the first inorganic barrier layer, condensing the photocurable resin so that the photocurable resin does not exist on the portion of the first inorganic barrier layer where the cone angle is less than 90°; and step K, after step J, forming the organic barrier layer composed of photocurable resin by irradiating the condensed photocurable resin with light.
[0026] In one embodiment, the manufacturing method further includes: step H, after step G, selectively forming the first inorganic barrier layer in the active area where the multiple EL elements are formed; step I, after step H, placing the substrate in a chamber and supplying vapor or mist of photocurable resin into the chamber; step J, condensing the photocurable resin on the first inorganic barrier layer to form a liquid film; step K, forming a photocurable resin layer by irradiating the liquid film of the photocurable resin with light; and step L, forming the organic barrier layer by partially ashing the photocurable resin layer. Beneficial Effects
[0027] According to an embodiment of the present invention, an EL display device having a thinner organic barrier layer with improved mass productivity and moisture resistance reliability and a method for manufacturing the same are provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 (a) is a schematic partial cross-sectional view of an active region of an OLED display device 100 according to an embodiment of the present invention, and (b) is a partial cross-sectional view of a TFE structure 10 formed on an OLED 3 . Figure 2 is a schematic top view of an OLED display device 100A according to an embodiment of the present invention. Figure 3 (a) and (b) are schematic cross-sectional views of the OLED display device 100A, (a) is a schematic cross-sectional view of the OLED display device 100A. Figure 2 The cross-sectional view along the line 3A-3A' in FIG. 1 and (b) along the line 3A-3A' in FIG. Figure 2 (c) is a cross-sectional view taken along line 3B-3B' of FIG. 1 , and (c) is a cross-sectional view showing a taper angle θ of the side surface of each layer. Figure 4 (a) to (d) are schematic cross-sectional views of the OLED display device 100A, (a) is a schematic cross-sectional view of the OLED display device 100A. Figure 2 The cross-sectional view along the line 4A-4A' in FIG. 4A-4A', (b) is a cross-sectional view along the line 4A-4A' in FIG. Figure 2 The cross-sectional view along the line 4B-4B' in FIG. 4B-4B', (c) is a cross-sectional view along the line 4B-4B' of FIG. Figure 2 The cross-sectional view along the 4C-4C' line in (d) is Figure 2 Cross-sectional view along line 4D-4D'. Figure 5 (a) and (b) are the OLED display devices 100B1 and 100B2 of the comparative example. Figure 4 (b) corresponds to a schematic cross-sectional view. Figure 6 is a schematic top view of an OLED display device 100C according to a comparative example. Figure 7(a) and (b) are schematic cross-sectional views of an OLED display device 100C, wherein (a) is a cross-sectional view of an OLED display device 100C. Figure 6 7A-7A' line cross-sectional view, (b) is a cross-sectional view along the line 7A-7A' Figure 6 Cross-sectional view along line 7B-7B'. Figure 8 (a) to (c) are schematic cross-sectional views of the OLED display device 100C, (a) is a schematic cross-sectional view of the OLED display device 100C. Figure 6 8A-8A' line, (b) is a cross-sectional view along Figure 6 8B-8B' line, (c) is a cross-sectional view along Figure 6 Cross-sectional view along line 8C-8C'. Fig. 9 (a) and (b) are schematic cross-sectional views each showing an example of a TFT that can be included in the OLED display device of the embodiment. Fig.10 (a) to (c) are schematic cross-sectional views of other OLED display devices according to the embodiments, respectively. Figure 4 (b) to (d) correspond to. Fig.11 (a) to (c) are schematic cross-sectional views of still another OLED display device according to an embodiment. Fig.12 (a) and (b) are diagrams schematically showing the structure of the film forming device 200, (a) shows the state of the film forming device 200 in the process of condensing the photocurable resin on the first inorganic barrier layer, and (b) shows the state of the film forming device 200 in the process of curing the photocurable resin. DETAILED DESCRIPTION
[0029] Hereinafter, an OLED display device and a manufacturing method thereof according to an embodiment of the present invention will be described with reference to the accompanying drawings. Hereinafter, an OLED display device having a flexible substrate is exemplified, but the embodiment of the present invention is not limited to an organic EL display device, and may also be other organic EL devices such as an organic EL lighting device, and is not limited to the embodiment exemplified below.
[0030] First, refer to Figure 1 (a) and (b) of the drawings illustrate the basic structure of the OLED display device 100 according to the embodiment of the present invention. Figure 1 (a) is a schematic partial cross-sectional view of an active region of an OLED display device 100 according to an embodiment of the present invention, Figure 1 (b) is a partial cross-sectional view of the TFE structure 10 formed on the OLED 3 .
[0031] The OLED display device 100 has a plurality of pixels, and each pixel has at least one organic EL element (OLED). Here, for simplicity, a structure corresponding to one OLED is described.
[0032] like Figure 1 As shown in (a), the OLED display device 100 is sometimes referred to as a flexible substrate (hereinafter, simply referred to as a "substrate") 1 and a circuit including TFTs formed on the substrate 1, sometimes referred to as a "driving circuit" or a "baseboard circuit") 2, an inorganic protective layer (first inorganic protective layer) 2Pa formed on the circuit 2, an organic planarization layer 2Pb formed on the inorganic protective layer 2Pa, an OLED 3 formed on the organic planarization layer 2Pb, and a TFE structure 10 formed on the OLED 3. Hereinafter, the substrate 1, the circuit 2 formed on the substrate 1, the inorganic protective layer 2Pa, the organic planarization layer 2Pb, and the OLED 3 are sometimes referred to as an element substrate 20. That is, the substrate 1 and the components arranged on the side closer to the substrate 1 than the TFE structure 10 on the substrate 1 are collectively referred to as an element substrate.
[0033] OLED 3 is, for example, a top-emitting type. The uppermost portion of OLED 3 is, for example, an upper electrode or a cap layer (refractive index adjustment layer). Sometimes a layer in which a plurality of OLEDs 3 are arranged is referred to as an OLED layer 3. An optional polarizing plate 4 is disposed on the TFE structure 10. In addition, the circuit 2 and the OLED layer 3 may also share some of the components. In addition, for example, a layer that performs a touch panel function may also be disposed between the TFE structure 10 and the polarizing plate 4. That is, the OLED display device 100 can be changed into an on-cell type display device with a touch panel.
[0034] The substrate 1 is a polyimide film with a thickness of 15 μm, for example. The circuit 2 including the TFT has a thickness of 4 μm, for example. The inorganic protective layer 2Pa is, for example, SiN x Layer (500 nm) / SiO2 layer (100 nm) (upper layer / lower layer). The inorganic protective layer 2Pa may also be, for example, SiO2 layer / SiN x The inorganic protective layer 2Pa may be a SiN layer or a SiO2 layer. x The organic planarization layer 2Pb is, for example, an acrylic resin layer, an epoxy resin layer, or a polyimide layer with a thickness of 4 μm. The organic planarization layer 2Pb is preferably formed using a resin that is not photosensitive, but can also be formed using a photosensitive resin. The thickness of the OLED 3 is, for example, 1 μm. The thickness of the TFE structure 10 is, for example, less than 2.5 μm.
[0035] Figure 1(b) is a partial cross-sectional view of the TFE structure 10 formed on the OLED 3. A first inorganic barrier layer (eg, SiN x An organic barrier layer (eg, an acrylic resin layer) 14 is formed on the first inorganic barrier layer 12, and a second inorganic barrier layer (eg, a SiN layer) is formed on the organic barrier layer 14. x Layer)16.
[0036] For example, the first inorganic barrier layer 12 is SiN with a thickness of 1.5 μm. x The second inorganic barrier layer 16 is, for example, SiN with a thickness of 800 nm. x The organic barrier layer 14 is, for example, an acrylic resin layer with a thickness of less than 100 nm. The thickness of the first inorganic barrier layer 12 and the second inorganic barrier layer 16 are independently 200 nm to 1500 nm, respectively, and the thickness of the organic barrier layer 14 is 50 nm to less than 200 nm. The thickness of the TFE structure 10 is preferably 400 nm to less than 3 μm, and more preferably 400 nm to 2.5 μm.
[0037] The TFE structure 10 is used to protect the active area of the OLED display device 100 (see Figure 2 The organic barrier layer 14 is formed in the active region R1 in the active region R1, and at least in the active region R1, as described above, the first inorganic barrier layer 12, the organic barrier layer 14, and the second inorganic barrier layer 16 are sequentially provided from the side close to the OLED 3. In addition, the organic barrier layer 14 does not exist as a film covering the entire surface of the active region R1, but has an opening. The portion of the organic barrier layer 14 where the organic film actually exists except the opening is referred to as a "solid portion". The organic barrier layer 14 can be formed using, for example, the method described in Patent Document 1 or Patent Document 2 or the film forming device 200 described later.
[0038] In addition, sometimes referred to as an "opening" (non-solid part), it is not necessary to be surrounded by a solid part, including a cutout, etc., and the first inorganic barrier layer 12 and the second inorganic barrier layer 16 are in direct contact at the opening. Hereinafter, the portion where the first inorganic barrier layer 12 and the second inorganic barrier layer 16 are in direct contact is referred to as an "inorganic barrier layer joint portion".
[0039] Next, refer to Figure 2 and Figure 3 , the structure and manufacturing method of the OLED display device 100A according to the embodiment of the present invention are described.
[0040] Figure 2 Schematic top view of an OLED display device 100A according to an embodiment of the present invention. Figure 3 (a) to (c) and Figure 4(a) to (d) of FIG. 1 illustrate the cross-sectional structure of the OLED display device 100A. Figure 3 (a) and (b) are schematic cross-sectional views of an OLED display device 100A. Figure 3 (a) is along Figure 2 The cross-sectional view of line 3A-3A' in FIG. Figure 3 (b) is along Figure 2 Cross-sectional view along line 3B-3B'. Figure 3 (c) is a cross-sectional view showing the taper angle θ of the side surface of each layer. Figure 4 (a) to (d) are schematic cross-sectional views of an OLED display device 100A. Figure 4 (a) is along Figure 2 The cross-sectional view of the line 4A-4A' in Figure 4 (b) is along Figure 2 The cross-sectional view of line 4B-4B' in Figure 4 (c) is along Figure 2 The cross-sectional view of the 4C-4C' line in Figure 4 (d) is along Figure 2 Cross-sectional view along line 4D-4D'.
[0041] First, refer to Figure 2 The circuit 2 formed on the substrate 1 has a plurality of TFTs (not shown) and a plurality of gate buses (not shown) and a plurality of source buses (not shown) respectively connected to any one of the plurality of TFTs (not shown). The circuit 2 may be a known circuit for driving a plurality of OLEDs 3. The plurality of OLEDs 3 are connected to any one of the plurality of TFTs of the circuit 2. The OLED 3 may also be a known OLED.
[0042] The circuit 2 further includes a plurality of terminals 34 and a plurality of lead wirings 32 connecting the plurality of terminals 34 and any one of the plurality of gate bus lines or the plurality of source bus lines. The plurality of terminals 34 are arranged in an active region ( Figure 2 The peripheral region R2 outside the active region R1 is sometimes referred to as the driving circuit layer 2. The circuit 2 including a plurality of TFTs, a plurality of gate bus lines, a plurality of source bus lines, a plurality of lead wirings 32, and a plurality of terminals 34 is sometimes referred to as the driving circuit layer 2. In addition, within the driving circuit layer 2, the portion formed within the active region R1 is referred to as the driving circuit layer 2A.
[0043] In addition, Figure 2In the drawings, as the components of the driving circuit layer 2, only the lead wiring 32 and / or the terminal 34 are sometimes shown in the figure, but the driving circuit layer 2 has not only a conductive layer including the lead wiring 32 and the terminal 34, but also one or more conductive layers, one or more insulating layers, and one or more semiconductor layers. The structure of the conductive layer, insulating layer, and semiconductor layer included in the driving circuit layer 2 can be described, for example, by Fig. 9 The configuration of the TFT illustrated in (a) and (b) is changed. In addition, an insulating film (primer layer) may be formed on the substrate 1 as a base film of the driving circuit layer 2.
[0044] When viewed from the normal direction of the substrate 1, the organic planarization layer 2Pb is formed in the region where the inorganic protective layer 2Pa is formed, and the active region R1 (2A, 3) is arranged in the region where the organic planarization layer 2Pb is formed. The outer edge of the TFE structure 10 intersects with the plurality of lead wires 32 and exists between the outer edge of the organic planarization layer 2Pb and the outer edge of the inorganic protective layer 2Pa. Therefore, the organic planarization layer 2Pb and the OLED layer 3 are surrounded by the joint portion where the inorganic protective layer 2Pa and the first inorganic barrier layer 12 are in direct contact (see FIG. 1 ). Figure 3 (b) and Figure 4 (b)). The inorganic protective layer 2Pa is formed, for example, by a plasma CVD method using a mask (e.g., a metal mask) in such a manner that at least a plurality of terminals 34 are exposed. Alternatively, the inorganic protective layer 2Pa may be obtained by forming an inorganic protective film by a plasma CVD method in such a manner as to cover the terminals 34, and then patterning the inorganic protective film by a photolithography process (including a dry etching process) to form an opening portion that exposes the terminals 34. In addition, as described later, when the second inorganic protective layer 2Pa2 is formed on the organic planarization layer 2Pb (see Fig.11 (b)), patterning including formation of contact holes is preferably performed uniformly on the inorganic protective film 2Pa (first inorganic protective film 2Pa1), the organic planarizing film 2Pb, and the second inorganic protective layer 2Pa2.
[0045] The inorganic protective layer 2Pa protects the driving circuit layer 2. The organic planarizing layer 2Pb planarizes the surface of the substrate on which the OLED layer 3 is formed. The organic planarizing layer 2Pb, like the organic barrier layer 14, has a lower water vapor barrier property than the inorganic protective layer 2Pa and the inorganic barrier layers 12 and 16. Figure 6 to Figure 8As shown in the comparative example, the organic planarization layer 2Pbc of the OLED display device 100C absorbs moisture from the organic planarization layer 2Pbc if part of it is exposed to the atmosphere (surrounding atmosphere). As a result, the organic planarization layer 2Pbc becomes a path for guiding water vapor in the atmosphere into the active region R1. As described above, in the OLED display device 100 of the embodiment, the organic planarization layer 2Pb is surrounded by the junction where the inorganic protective layer 2Pa and the first inorganic barrier layer 12 are in direct contact, so moisture is prevented from being introduced into the active region R1 from the organic planarization layer 2Pb.
[0046] The organic planarization layer 2Pb is formed of an organic resin. As the organic resin, acrylic resin, epoxy resin, and polyimide resin can be preferably used. The organic planarization layer 2Pb is obtained by patterning an organic resin film formed using various coating methods and printing methods. In one embodiment of the present invention, as described later, chemical mechanical polishing (CMP, hereinafter referred to as "CMP") is performed on the surface of the organic resin film. CMP is preferably performed before forming contact holes, etc. in the organic resin film. This is because if CMP is performed after forming contact holes on the organic resin film, it may not be possible to fully remove the abrasive in the contact holes.
[0047] The organic resin film is formed using, for example, a resin that is not photosensitive. However, a resin that is photosensitive may also be used. As the photosensitive resin, a positive photosensitive resin is preferably used. When a photosensitive resin is used, the organic resin film can be formed only in a predetermined area in the photolithography process. For example, after applying a photosensitive resin to substantially the entire surface of the element substrate, the photosensitive resin is exposed / developed, thereby forming a predetermined area (for example, a reference to FIG. 1 ) other than the peripheral portion of the element substrate. Fig.11 (c) After forming an organic resin film, CMP is performed, and contact holes and the like are formed separately after CMP. Alternatively, CMP may be performed after applying a photosensitive resin to substantially the entire surface of the element substrate, and then the photosensitive resin is exposed / developed to remove the photosensitive resin in the peripheral portion of the element substrate, for example, and to form contact holes and the like. Thus, when CMP is performed on the unexposed photosensitive resin, it is preferred that the photosensitive resin has high resistance to the chemical solution used in CMP, and from this point of view, a positive type is preferred. In addition, as described later, when a second inorganic protective layer 2Pa2 is formed on the organic planarizing layer 2Pb (see Fig.11 (b)), it is preferable to form contact holes in the inorganic protective film 2Pa (first inorganic protective film 2Pa1), the organic planarizing film 2Pb, and the second inorganic protective layer 2Pa2 at the same time.
[0048] An OLED layer 3 is formed on the organic planarization layer 2Pb. The lower electrode and the organic layer (also referred to as the organic EL layer. At least including the organic light-emitting layer) of the OLED 3 require high flatness. When the flatness is low, for example, the light-emitting efficiency of the OLED 3 is reduced. The organic planarization layer 2Pb is formed by a liquid organic resin material (which may contain a solvent) applied to the surface of the element substrate (referred to as the element substrate for simplicity during the manufacturing process), so that it can absorb the unevenness (height difference) of the base of the organic planarization layer 2Pb to form a flat surface. However, the surface of the organic resin film formed by the liquid resin material has a roughness (which may appear as "waviness") with an arithmetic mean roughness Ra exceeding 100nm to about 300nm (refer to Fig.11 (a)). If OLED 3 is formed on the organic planarization layer 2Pb having such surface roughness, the luminous efficiency cannot be sufficiently improved. For example, there is a problem that even if a micro-resonator structure is used, its effect cannot be fully demonstrated.
[0049] Therefore, in the embodiment of the present invention, by performing CMP on the surface of the organic resin film formed as described above, the arithmetic mean roughness Ra of the organic planarization layer 2Pb is controlled to be less than 50 nm, preferably less than 30 nm. The arithmetic mean roughness Ra is preferably smaller, and the lower limit is not limited, but considering the relationship between the cost, time and effect required for CMP, the arithmetic mean roughness Ra can be greater than 10 nm, or greater than 20 nm.
[0050] Specifically, CMP can be performed using a slurry containing a neutral cerium oxide (CeO2) abrasive, or a slurry containing a gas phase silica abrasive or a colloidal silica abrasive. Alternatively, a slurry containing aluminum oxide (Al2O3) powder, which is used for polishing the surface of a resin optical lens, can be used. The load of the polishing pad is preferably 50 g / cm 2 Above and 150g / cm 2 The rotation speed is preferably 20 rpm or more and 40 rpm or less. The time required for grinding is about 30 seconds to about 90 seconds.
[0051] In the OLED display device of the embodiment of the present invention, the level of smoothing required to suppress the reduction in luminous efficiency is about one digit lower than the level of smoothing required for the optical process of ultra-LSI and the surface of an optical lens (the value of the arithmetic mean roughness Ra is about 10 times larger), and therefore known abrasives used in CMP of polymer materials (resin materials) can be widely used.
[0052] The surface roughness can be measured using, for example, a confocal laser microscope or an atomic force microscope (AFM). The measurement range preferably includes the vicinity of the center of the pixel, and the reference length is appropriately set according to the surface roughness.
[0053] In this specification, in order to distinguish between planarization by the organic planarization layer 2Pb and planarization by CMP, planarization by CMP may be referred to as “smoothing”.
[0054] By smoothing the surface of the organic planarization layer 2Pb, the lower electrode, the organic layer, and the upper electrode of the OLED 3 formed on the organic planarization layer 2Pb can be smoothed, thereby improving the light emission efficiency of the OLED display device.
[0055] Organic resins easily contain moisture. On the other hand, as mentioned above, OLEDs (especially organic light-emitting layers and cathode electrode materials) are easily affected by moisture and degraded. Therefore, it is preferred to heat (dry) the organic planarization layer 2Pb before forming the OLED layer 3 on the organic planarization layer 2Pb in order to remove the moisture contained in the organic planarization layer 2Pb. The heating temperature is preferably, for example, above 100°C (for example, for more than 1 hour), and more preferably above 250°C (for example, for more than 15 minutes). The atmosphere may be atmospheric pressure. If heating is performed under a reduced pressure atmosphere, the heating time can be shortened. In order to prevent thermal degradation during the heating (baking) process, a resin material with high heat resistance is preferred, such as polyimide.
[0056] In addition, after the organic planarization layer 2Pb is formed, before the OLED layer 3 is formed, the element substrate is sometimes stored or transported. That is, after the element substrate having the drive circuit layer 2, the inorganic protective layer 2Pa and the organic planarization layer 2Pb is produced, until the OLED layer 3 is formed, time is sometimes left (for example, stored for more than one day or several days), or moved to another factory. During this period, as a method to prevent the surface of the organic planarization layer 2Pb from being contaminated or dust from being attached during movement, for example, a positive photoresist film covering the organic planarization layer 2Pb is formed. The photoresist film is preferably formed by pre-baking (volatilization removal of the solvent: for example, heating for about 5 minutes to about 30 minutes in a temperature range of about 90°C to about 110°C) after applying a photoresist solution. After storage and movement, before the OLED layer 3 is formed, a clean surface of the organic planarization layer 2Pb can be obtained by removing the photoresist film. The removal of the photoresist film is preferably performed by exposing the entire surface of the photoresist film and then developing without performing a normal post-bake or by pre-bake and then stripping with a stripping solution without performing full-surface exposure. As a material for forming a positive photoresist film, for example, OFPR-800 manufactured by Tokyo Ohka Co., Ltd., which is a positive photoresist, can be appropriately used.
[0057] In addition, as referenced Fig.11 As described later in (b), in the process of forming the OLED element 3, a bank layer is sometimes formed. The bank layer is formed after the lower electrode is formed and before the organic layer (organic EL layer) is formed. Since the bank layer is formed of an organic resin (such as polyimide), it is easy to contain moisture and is in contact with the organic layer. Therefore, it is preferred to heat in order to remove the moisture from the bank layer. Therefore, after the organic planarization layer 2Pb is formed, the lower electrode is formed and the channel layer is formed, a positive photoresist film for protecting the surface of the element substrate may be formed as described above. After necessary storage and / or transportation, the photoresist film is removed as described above, and before the organic layer is formed, the moisture contained in the organic planarization layer 2Pb and the bank layer is removed by heating. In this way, it is also possible to have both a heating process for removing the moisture contained in the organic planarization layer 2Pb and a heating process for removing the moisture contained in the bank layer. Of course, as described above, the organic planarizing layer 2Pb can be protected by a positive photoresist film, and after removing the positive photoresist film, a heating process for removing moisture contained in the organic planarizing layer 2Pb can be performed. Then, after forming the lower electrode and the embankment layer and before forming the organic layer, a heating process for removing moisture contained in the embankment layer can be performed.
[0058] Next, refer to Figure 3 (a) to (c) and Figure 4 (a) to (d) of FIG. 1 further illustrate the cross-sectional structure of the OLED display device 100A in detail.
[0059] like Figure 3 (a), (b) and Figure 4 As shown in (a) and (b), the TFE structure 10A has a first inorganic barrier layer 12 formed on the OLED 3, an organic barrier layer 14 in contact with the first inorganic barrier layer 12, and a second inorganic barrier layer 16 in contact with the organic barrier layer 14. The first inorganic barrier layer 12 and the second inorganic barrier layer 16 are, for example, SiN x The layer is selectively formed only in a predetermined region by a plasma CVD method using a mask so as to cover the active region R1.
[0060] The organic barrier layer 14 can be formed by, for example, the method described in the above-mentioned Patent Document 2 or Patent Document 3. For example, in a chamber, vapor or mist of an organic material (e.g., an acrylic monomer) is supplied to an element substrate maintained at a temperature below room temperature, condensed on the element substrate, and the organic material in liquid form is distributed unevenly on the side of the convex portion and the boundary portion of the flat portion of the first inorganic barrier layer 12 by utilizing the capillary phenomenon or surface tension of the organic material. Thereafter, by irradiating the organic material with ultraviolet rays, for example, a solid portion of the organic barrier layer (e.g., an acrylic resin layer) 14 is formed on the boundary portion around the convex portion. The organic barrier layer 14 formed by this method has substantially no solid portion on the flat portion. The method for forming the organic barrier layer is cited in this specification for reference to the disclosures of Patent Documents 2 and 3.
[0061] The organic barrier layer 14 can also be formed by adjusting the initial thickness (e.g., less than 100 nm) of the resin layer formed using the film forming apparatus 200 and / or ashing the temporarily formed resin layer. The ashing process can be performed, for example, by plasma ashing using at least one gas selected from N2O, O2, and O3, as described later.
[0062] Figure 3 (a) is along Figure 2 The cross-sectional view along the line 3A-3A' in FIG. 1 shows a portion containing particles P. The particles P are fine waste generated in the manufacturing process of the OLED display device, such as fine glass fragments, metal particles, and organic particles. If a mask evaporation method is used, particles are particularly likely to be generated.
[0063] like Figure 3 As shown in (a), the organic barrier layer (solid portion) 14 may be formed only around the microparticles P. This is because the acrylic monomer applied after the first inorganic barrier layer 12 is formed condenses and is unevenly distributed around the surface (taper angle θ is 90° or more) of the first inorganic barrier layer 12a on the microparticles P. The flat portion of the first inorganic barrier layer 12 becomes the opening portion (non-solid portion) of the organic barrier layer 14.
[0064] If there are fine particles (for example, having a diameter of about 1 μm or more) P, cracks (defects) 12c may be formed in the first inorganic barrier layer 12. This is considered to be due to the SiN grown from the surface of the fine particles P. x The SiN layer 12a and the SiN layer 12a grown from the flat portion of the surface of the OLED 3 x The cracks 12c are generated by the impingement of the layer 12b. If such cracks 12c exist, the barrier property of the TFE structure 10A is reduced.
[0065] In the TFE structure 10A of the OLED display device 100A, as shown in FIG. Figure 3 As shown in (a), the organic barrier layer 14 is formed in a manner that fills the cracks 12c of the first inorganic barrier layer 12, and the surface of the organic barrier layer 14 continuously and smoothly connects the surface of the first inorganic barrier layer 12a on the particles P and the surface of the first inorganic barrier layer 12b on the flat portion of the OLED 3. Therefore, no defects are formed on the first inorganic barrier layer 12 on the particles P and the second inorganic barrier layer 16 formed on the organic barrier layer 14, but a dense film is formed. In this way, the barrier property of the TFE structure 10A can be maintained even if the particles P exist, by the organic barrier layer 14.
[0066] Next, refer to Figure 3 (b) and Figure 4 (a) to (d) illustrate the cross-sectional structure of the lead wiring 32 and the terminal 34.
[0067] like Figure 3 As shown in (b), a lead wiring 32 and a terminal 34 are integrally formed on the substrate 1, and an inorganic protective layer 2Pa is formed on the lead wiring 32 in a manner that exposes the terminal portion 34. An organic planarization layer 2Pb is formed on the inorganic protective layer 2Pa, and an OLED layer 3 is formed on the organic planarization layer 2Pb. The TFE structure 10A is formed in a manner that covers the OLED layer 3 and the organic planarization layer 2Pb, and the OLED layer 3 and the organic planarization layer 2Pb are surrounded by a junction where the inorganic protective layer 2Pa is in direct contact with the first inorganic barrier layer 12. In addition, the organic barrier layer (solid portion) 14 between the first inorganic barrier layer 12 and the second inorganic barrier layer 16 of the TFE structure 10A is formed only around the protrusions such as particles, and is therefore not shown here. The organic barrier layer (solid portion) 14 is surrounded by the inorganic barrier layer junction where the first inorganic barrier layer 12 and the second inorganic barrier layer 16 are in direct contact.
[0068] like Figure 4 As shown in (a), in the area close to the active area R1 (along Figure 2 In the cross section along the line 4A-4A′ in FIG. 1 , an inorganic protective layer 2Pa, an organic planarizing layer 2Pb, and a TFE structure 10A are formed on the lead wiring 32.
[0069] like Figure 4 As shown in (b), along Figure 2 In the cross section of the line 4B-4B' in FIG. 4B, the inorganic protective layer 2Pa is in direct contact with the first inorganic barrier layer 12, and the organic planarization layer 2Pb is surrounded by the junction where the inorganic protective layer 2Pa is in direct contact with the first inorganic barrier layer 12 (refer to FIG. 4B-4B'). Figure 2 , Figure 3 (b)).
[0070] like Figure 4As shown in (c) , in a region close to the terminal 34 , only the inorganic protective layer 2Pa is formed on the lead wiring 32 .
[0071] like Figure 4 As shown in (d) , the terminal 34 is also exposed from the inorganic protective layer 2Pa and is used for electrical connection with an external circuit (for example, FPC (Flexible Printed Circuits)).
[0072] Due to the inclusion Figure 4 The area shown in (b) to (d) of FIG. 1 is not covered by the organic planarizing layer 2Pb, so that the organic barrier layer (solid portion) can be formed in the process of forming the organic barrier layer 14 of the TFE structure 10A. For example, if the side surface of the cross-sectional shape of the lead wiring 32 parallel to the line width direction has a taper angle θ of 90° or more, the organic barrier layer can be formed along the side surface of the lead wiring 32. However, if Figure 4 As shown in (b) to (d) of the embodiment, in the OLED display device 100A, at least in these regions, the taper angle θ of the side in the cross-sectional shape of the lead wiring 32 and the terminal 34 is set to be less than 90°, and the photocurable resin is not unevenly distributed. Therefore, the organic barrier layer (solid portion) is not formed along the side of the lead wiring 32 and the terminal 34.
[0073] Here, refer to Figure 3 (c) illustrates the taper angle θ of the side surface of each layer. Figure 3 (c) is a cross-sectional view showing the taper angle θ of the side surface of each layer, for example Figure 4 The cross-sectional view shown in (b) corresponds to the cross-sectional view shown in (b). Figure 3 As shown in (c), the taper angle θ of the side surface in the cross-sectional shape parallel to the width direction of the lead wiring 32 is represented by θ(32), and the taper angle θ of the side surface of other layers is similarly represented by θ (reference number of the component).
[0074] In this way, the taper angles θ of the inorganic protective layer 2Pa formed on the lead wiring 32, the side surface of the first inorganic barrier layer 12 formed on the TFE structure 10A on the inorganic protective layer 2Pa, and the side surface of the second inorganic barrier layer 16 satisfy the relationship of θ(32)≥θ(2Pa)≥θ(12)≥θ(16). Therefore, if the taper angle θ(32) of the side surface of the lead wiring 32 is less than 90°, the taper angle θ(2Pa) of the side surface of the inorganic protective layer 2Pa and the taper angle θ(12) of the side surface of the first inorganic barrier layer 12 are also less than 90°.
[0075] If the taper angle θ of the side surface is 90° or more, in the method for forming an organic barrier layer described in Patent Document 2 or Patent Document 3, vapor or mist of an organic material (e.g., an acrylic monomer) condenses along the boundary (forming an angle of 90° or less) between the side surface and the flat surface to form an organic barrier layer (solid portion). Thus, for example, the organic barrier layer (solid portion) formed along the lead wiring becomes a path for introducing water vapor in the atmosphere into the active region.
[0076] For example, Figure 5 The OLED display device 100B1 of the comparative example (a) is Figure 4 As shown in the schematic cross-sectional view corresponding to (b), if the taper angle θ(32B1) of the side of the lead wiring 32B1 and the taper angle θ(12B1) of the side of the first inorganic barrier layer 12B1 are greater than 90°, an organic barrier layer (solid portion) 14B1 is formed between the first inorganic barrier layer 12B1 and the second inorganic barrier layer 16B1 along the side of the first inorganic barrier layer 12B1 of the TFE structure 10B1. In addition, the OLED display device 100B1 may also omit the inorganic protective layer 2Pa in the OLED display device 100 of the embodiment, and change the taper angle θ(32) of the side of the lead wiring 32 and the taper angle θ(12) of the side of the first inorganic barrier layer 12 to greater than 90°.
[0077] In addition, if Figure 5 The OLED display device 100B2 of the comparative example (b) is Figure 4 As shown in the schematic cross-sectional view corresponding to (b), if the taper angles θ(32B2), θ(2PaB2) and θ(12B2) of the side surfaces of the lead wiring 32B2, the inorganic protective layer 2PaB2 and the first inorganic barrier layer 12B2 are 90° or more, an organic barrier layer (solid portion) 14B2 is formed between the first inorganic barrier layer 12B2 and the second inorganic barrier layer 16B2 along the side surface of the first inorganic barrier layer 12B2 of the TFE structure 10B2. In addition, the OLED display device 100B2 can change the side taper angle θ(32) of the lead wiring 32 and the side taper angle θ(12) of the first inorganic barrier layer 12 in the OLED display device 100A of the embodiment to 90° or more.
[0078] The OLED display device 100B2 is different from the OLED display device 100B1. Since the OLED display device 100B2 has the inorganic protective layer 2PaB2, the side taper angle θ(12B2) of the first inorganic barrier layer 12B2 is easily smaller than the side taper angle θ(12B1) of the first inorganic barrier layer 12B1 of the OLED display device 100B1.
[0079] Figure 4In the OLED display device 100A of the embodiment of the present invention shown in (b) to (d), the taper angles θ(32), θ(2Pa) and θ(12) of the side surfaces of the lead wiring 32, the inorganic protective layer 2Pa and the first inorganic barrier layer 12 are all less than 90°, and the organic barrier layer 14 is not formed along these sides. Therefore, moisture in the atmosphere does not reach the active region R1 through the organic barrier layer (solid portion) 14, so that excellent moisture resistance reliability can be achieved. Here, an example in which the taper angles θ(32), θ(2Pa) and θ(12) are all less than 90° is shown, but it is not limited to this. As long as the taper angle θ(12) of the side surface of at least the first inorganic barrier layer 12 constituting the surface directly below the organic barrier layer 14 is less than 90°, an organic barrier layer 14 is formed. Figure 4 The stacked structure shown in (b) (the portion where the inorganic protective layer 2Pa is in direct contact with the first inorganic barrier layer 12 (where the organic planarizing layer 2Pb is not present) and the portion where the first inorganic barrier layer 12 is in direct contact with the second inorganic barrier layer 16 (where the organic barrier layer 14 is not present)) can suppress / prevent moisture in the atmosphere from invading the active region R1 via the organic planarizing layer 2Pb or the organic barrier layer 14. In addition, by having the inorganic protective layer 2Pa, the taper angle θ(12) of the first inorganic barrier layer 12 can be reduced. Therefore, even if the taper angle θ(32) of the lead wiring 32 is made relatively large (for example, 90°), the taper angle θ(12) of the first inorganic barrier layer 12 can be made smaller than 90°. That is, the taper angle θ(32) of the lead wiring 32 can be made 90° or close to 90°, and therefore, the advantage of reducing the L / S of the lead wiring 32 can be obtained.
[0080] In addition, when the taper angle θ of the side surface is within the range of 70° or more and less than 90°, an organic barrier layer (solid portion) 14 is sometimes formed along the side surface. Of course, if an ashing treatment is performed, the resin unevenly distributed along the inclined side surface can be removed, but the time required for the ashing treatment becomes longer. For example, a long ashing treatment is required even after the resin formed on the flat surface is removed. Alternatively, the organic barrier layer (solid portion) formed around the particles P is excessively ashed (removed), and sometimes there is a problem that the effect of forming the organic barrier layer cannot be fully exerted. In order to suppress / prevent this problem, the taper angle θ(12) of the first inorganic barrier layer 12 is preferably set to less than 70°, and more preferably less than 60°.
[0081] Next, refer to Figures 6 to 8 , describing the structure of an OLED display device 100C of a comparative example. Figure 6 FIG. 1 is a schematic top view of an OLED display device 100C. Figure 7 (a) and (b) are schematic cross-sectional views of an OLED display device 100C. Figure 7 (a) is along Figure 6The cross-sectional view of line 7A-7A' in FIG. Figure 7 (b) is along Figure 6 Cross-sectional view along line 7B-7B'. Figure 8 (a) to (c) are schematic cross-sectional views of an OLED display device 100C. Figure 8 (a) is along Figure 6 The cross-sectional view of line 8A-8A' in FIG. Figure 8 (b) is along Figure 6 The cross-sectional view of line 8B-8B' in FIG. Figure 8 (c) is along Figure 6 Cross-sectional view along line 8C-8C'.
[0082] The OLED display device 100C is different from the OLED display device 100 of the embodiment in that it does not have an inorganic protective layer 2Pa and that an organic planarization layer 2Pbc is extended to a region not covered by the TFE structure 10C. In addition, components substantially the same as those of the OLED display device 100A are sometimes denoted by the same reference numerals and their description is omitted.
[0083] For example, by Figure 6 , Figure 7 (b) and Figure 8 As can be seen from (b), a portion of the organic planarization layer 2Pbc is exposed to the atmosphere (surrounding atmosphere). In this way, the organic planarization layer 2Pbc absorbs moisture from the portion exposed to the atmosphere and guides the water vapor in the atmosphere to the active region R1. Figure 3 (b) and Figure 4 As shown in (b), in the OLED display device 100A of the embodiment, the organic planarization layer 2Pb and the OLED layer 3 are surrounded by the junction where the inorganic protective layer 2Pa and the first inorganic barrier layer 12 are in direct contact. Therefore, the above-mentioned problem of the OLED display device 100C of the comparative example can be solved.
[0084] Next, refer to Fig. 9 as well as Fig.10 , an example of a TFT used in the OLED display device 100A and an example of a lead wiring and terminal formed using a gate metal layer and a source metal layer when manufacturing the TFT are described. The structures of the TFT, lead wiring and terminals described below can be used in the OLED display device 100A of the above embodiment.
[0085] In high-definition small and medium-sized OLED display devices, it is preferred to use a low-temperature polysilicon (abbreviated as "LTPS") TFT with high mobility or an oxide TFT (for example, a quaternary system (In-Ga-Zn-O system) oxide TFT containing In (indium), Ga (gallium), Zn (zinc), and O (oxygen)). The structure and manufacturing method of LTPS-TFT and In-Ga-Zn-O system TFT are widely known, so the following is limited to a simple description.
[0086] Fig. 9 (a) is LTPS-TFT2 P Schematic cross-sectional view of TFT2 P T may be included in the circuit 2 of the OLED display device 100A. LTPS-TFT2 P T is a top-gate TFT.
[0087] TFT2 P A primer layer 2 is formed on a substrate (eg, a polyimide film) 1. P Although omitted in the above description, it is preferred that a primer layer made of an inorganic insulator is formed on the substrate 1.
[0088] TFT2 P T has: formed on the base layer 2 P Polysilicon layer 2 on p P se, formed on the polysilicon layer 2 P Gate insulation layer 2 on se P gi, formed on the gate insulating layer 2 P Gate 2 on gi P g. Formed on gate 2 P Interlayer insulation layer 2 on g P i, and forming an interlayer insulating layer 2 P Source 2 on i P ss and drain 2 P sd. source 2 P ss and drain 2 P sd is formed on the interlayer insulating layer 2 P i and gate insulating layer 2 P The contact holes of gi are respectively connected to the polysilicon layer 2 P The source region and drain region of se are connected.
[0089] Gate 2 P g is included in the same gate metal layer as the gate bus, source 2 P ss and drain 2 P sd is included in the same source metal layer as the source bus. The gate metal layer and source metal layer are used to form the lead wiring and terminals (refer to Fig.10 to be described later).
[0090] TFT2 P T is produced, for example, in the following manner.
[0091] As the substrate 1 , for example, a polyimide film having a thickness of 15 μm is prepared.
[0092] Formation of primer layer 2 by plasma CVD method P p(SiO2 film: 250nm / SiN x Film: 50nm / SiO2 film: 500nm (upper layer / middle layer / lower layer)) and a-Si film (40nm).
[0093] The a-Si film is subjected to a dehydrogenation treatment (eg, annealing at 450° C. for 180 minutes).
[0094] The a-Si film is converted into polysilicon by an excimer laser annealing (ELA) method.
[0095] The active layer (semiconductor island) is formed by patterning the a-Si film in a photolithography process.
[0096] A gate insulating film (SiO2 film: 50 nm) was formed by plasma CVD.
[0097] Doping is performed in the channel region of the active layer (B + ).
[0098] A gate metal (Mo: 250 nm) is formed into a film by sputtering, and patterned by a photolithography process (including a dry etching process) (forming a gate 2 P g and gate bus, etc.).
[0099] Doping is performed in the source and drain regions of the active layer (P + ).
[0100] Activation annealing (for example, annealing at 450° C. for 45 minutes) is performed. P se.
[0101] The interlayer insulating film (e.g. SiO2 film: 300nm / SiN) is formed by plasma CVD method. x Membrane: 300nm (upper layer / lower layer)).
[0102] Contact holes are formed on the gate insulating film and the interlayer insulating film by dry etching. In this way, the interlayer insulating layer 2 can be obtained. P i and gate insulating layer 2 P gi.
[0103] The source metal (Ti film: 100 nm / Al film: 300 nm / Ti film: 30 nm) was formed by sputtering and patterned by photolithography (including dry etching) (forming source 2 P ss, drain 2 P sd and source bus, etc.).
[0104] Then, the inorganic protective layer 2Pa described above is formed by, for example, a plasma CVD method (see Figure 2 and Figure 3 ).
[0105] Fig. 9 (b) is an In-Ga-Zn-O TFT2 O Schematic cross-sectional view of TFT2 O TFT2 may be included in the circuit 2 of the OLED display device 100A. O T is a bottom-gate TFT.
[0106] TFT20T is formed on a substrate (eg, a polyimide film) 1 and a primer layer 2 O p. TFT2 O T has: formed on the base layer 2 O Gate 2 on p O g; a gate insulating layer 2 formed on the gate 20g O gi; formed on the gate insulating layer 2 O Oxide semiconductor layer 2 on gi O se; and are respectively connected to the oxide semiconductor layer 2 O The source region of se and the source 2 on the drain region O ss and drain 2 O sd. source 2 O ss and drain 2 O sd is interlayer insulating layer 2 O i Cover.
[0107] Gate 2 O g is included in the same gate metal layer as the gate bus, source 2 O ss and drain 2 O sd is included in the same source metal layer as the source bus. The gate metal layer and the source metal layer are used to form the lead wiring and terminals, which can have a reference Fig.10 The structure described below.
[0108] TFT2 O T is produced, for example, as follows.
[0109] As the substrate 1 , for example, a polyimide film having a thickness of 15 μm is prepared.
[0110] Plasma CVD method for forming a primer layer 2 O p(SiO2 film: 250nm / SiN x Film: 50nm / SiO2 film: 500nm (upper layer / middle layer / lower layer)).
[0111] A gate metal (Cu film: 300 nm / Ti film: 30 nm (upper layer / lower layer)) is formed by sputtering and patterned (forming the gate 20g and gate bus lines, etc.) by a photolithography process (including a dry etching process).
[0112] The gate insulating film (SiO2 film: 30nm / SiN) is formed by plasma CVD method x Membrane: 350nm (upper layer / lower layer)).
[0113] An oxide semiconductor film (In—Ga—Zn—O-based semiconductor film: 100 nm) was deposited by sputtering and patterned by a photolithography process (including a wet etching process) to form an active layer (semiconductor island).
[0114] The source metal (Ti film: 100 nm / Al film: 300 nm / Ti film: 30 nm (upper layer / middle layer / lower layer)) was formed by sputtering and patterned by photolithography (including dry etching) (forming source 2 O ss, drain 2 O sd and source bus, etc.).
[0115] Activation annealing (for example, annealing at 300° C. for 120 minutes) is performed. In this way, the oxide semiconductor layer 2 can be obtained. O se.
[0116] Then, an interlayer insulating layer 2 is formed as a protective film by a plasma CVD method. O i (e.g. SiN x film: 300nm / SiO2 film: 300nm (upper layer / lower layer)). The interlayer insulating layer 2 O i can also serve as the above-mentioned inorganic protective layer 2Pa (refer to Figure 2 as well as Figure 3 ). Of course, it is also possible to O An inorganic protective layer 2Pa is further formed on i.
[0117] Next, refer to Fig.10 (a) to (c) illustrate the structure of another OLED display device according to the embodiment. The circuit (backplane) 2 of the OLED display device has Fig. 9 TFT2 shown in (a) P T or Fig. 9 TFT2 shown in (b)O T, use to make TFT2 P T or TFT2 O The gate metal layer and the source metal layer at T form the lead wiring 32A and the terminal 34A. Fig.10 (a)~(c) are respectively Figure 4 The reference numerals for the corresponding components are marked with "A". Fig.10 The base layer 2p and Fig. 9 (a) Primer 2 P p and Fig. 9 (b) Primer 2 O p corresponds to, Fig.10 The gate insulating layer 2gi and Fig. 9 (a) The gate insulating layer 2 P gi and Fig. 9 (b) The gate insulating layer 2 O gi corresponds to, Fig.10 The interlayer insulating layer 2i and Fig. 9 (a) The interlayer insulating layer 2 P i and Fig. 9 (b) The interlayer insulating layer 2 O i correspond respectively.
[0118] like Fig.10 As shown in (a) to (c) of FIG. 1 , the gate metal layer 2g and the source metal layer 2s are formed on the base layer 2p formed on the substrate 1. Figure 3 and Figure 4 Although omitted in the figure, it is preferred that a primer layer 2p formed of an inorganic insulator is formed on the substrate 1.
[0119] like Fig.10 As shown in (a) to (c), the lead wiring 32A and the terminal 34A are formed as a stack of the gate metal layer 2g and the source metal layer 2s. The portion of the lead wiring 32A and the terminal 34A formed by the gate metal layer 2g has, for example, the same cross-sectional shape as the gate bus, and the portion of the lead wiring 32A and the terminal 34A formed by the source metal layer 2s has, for example, the same cross-sectional shape as the source bus. For example, in the case of a 5.7-inch display device with a 500ppi, the line width of the portion formed by the gate metal layer 2g is, for example, 10um, and the adjacent spacing is 16um (L / S=10 / 16), and the line width of the portion formed by the source metal layer 2s is, for example, 16um, and the adjacent spacing is 10um (L / S=16 / 10). The cone angle θ is less than 90°, preferably less than 70°, and more preferably less than 60°. In addition, the cone angle of the portion formed under the organic planarization layer Pb may also be greater than 90°.
[0120] Next, refer to Fig.11 , describing the structure and manufacturing method of other OLED display devices according to other embodiments of the present invention. Fig.11 The OLED display device shown has Fig. 9 (a) shows the LTPS-TFT2 P T. Of course, you can also use Fig. 9 In-Ga-Zn-O TFT2 shown in (b) O T replaces LTPS-TFT2 P T, other well-known TFTs may also be used. Fig.11 In (a) and (b), the common wiring 2 electrically connected to the upper electrode (common electrode) 46 of the OLED is also shown. P c and contact part 2 P cV.
[0121] Fig.11 (a) schematically shows the state after the first inorganic protective film 2Pa1, which becomes the first inorganic protective layer 2Pa1, is formed on the driving circuit layer 2, and the organic planarizing film 2Pb, which becomes the organic planarizing layer 2Pb, is formed. The first inorganic protective film 2Pa1 is selectively formed in the desired area by a metal mask. In addition, the organic planarizing film 2Pb is selectively coated and formed in the desired area of the element substrate 20, or is temporarily formed on the entire surface, and then the unnecessary part is removed. The first inorganic protective film 2Pa1 is different from the first inorganic protective layer 2Pa1 in that it does not have openings such as contact holes, but for simplicity, it is represented by the same reference symbol. Similarly, the organic planarizing film 2Pb is different from the organic planarizing layer 2Pb in that it does not have openings such as contact holes, but for simplicity, it is represented by the same reference symbol. In addition, the first inorganic protective layer 2Pa1 is formed in the same way as the above-mentioned inorganic protective layer 2Pa.
[0122] The surface 2Pb_Sa of the organic planarization film 2Pb immediately after formation, i.e., before CMP is performed, has a roughness of about 300 nm with an arithmetic mean roughness Ra exceeding 100 nm. If an OLED 3 is formed on the organic planarization layer 2Pb having such a surface roughness, the luminous efficiency cannot be sufficiently improved. For example, there is a problem that even if a micro-resonator structure is used, its effect cannot be fully achieved.
[0123] Therefore, in the OLED display device 100D according to the embodiment of the present invention, Fig.11 As shown in (b), the surface 2Pb_Sb of the organic planarization layer 2Pb is smoothed, and the arithmetic mean roughness Ra is controlled to be less than 50 nm.
[0124] Through Fig.11By subjecting the surface 2Pb_Sa (Ra>50nm) of the organic planarization film 2Pb shown in (a) to CMP, a surface 2Pb_Sb with an arithmetic mean roughness Ra≤50nm can be obtained. The arithmetic mean roughness Ra of the surface 2Pb_Sb is preferably less than 30nm. The arithmetic mean roughness Ra is preferably smaller, and the lower limit is not limited, but considering the relationship between the cost, time and effect required for CMP, the arithmetic mean roughness Ra can be more than 10nm, or more than 20nm. The specific conditions of CMP are as described above.
[0125] Then, if Fig.11 As shown in (b), a second inorganic protective film 2Pa2 is formed on the organic planarizing film 2Pb having a smoothed surface 2Pb_Sb. The second inorganic protective film 2Pa2 is also selectively formed in a desired area using a mask in the same manner as the first inorganic protective film 2Pa1. The second inorganic protective film 2Pa2 is formed on the surface 2Pb_Sb of the organic planarizing film 2Pb, and thus has the same degree of smoothness as the surface 2Pb_Sb of the organic planarizing film 2Pb. For example, in the case of using SiN x When the second inorganic protective film 2Pa2 is formed by a plasma CVD method, for example, a SiN film having a thickness of 150 nm or more is formed at a film forming rate of not more than 10 nm / s. x film, thereby obtaining a second inorganic protective film 2Pa2 that reflects the smoothness of the substrate.
[0126] Next, the first inorganic protective film 2Pa1, the organic planarization film 2Pb, and the second inorganic protective film 2Pa2 formed in the desired area of the element substrate 20 are patterned together to form openings such as the contact holes CH1 and CH2. This patterning can be performed, for example, by dry etching using a mixed gas of O2 and CF4. Therefore, the resin forming the organic planarization film 2Pb2 does not need to be photosensitive. In addition, as Fig.11 As shown in (c), in order to form a portion where the first inorganic protective layer 2Pa1 is in direct contact with the first inorganic barrier layer (not shown) constituting the TFE structure 10D, only the portion where the first inorganic protective layer 2Pa1 remains can be formed by using a multi-tone mask, for example.
[0127] Next, the lower electrode 42 and the upper electrode contact portion 43 are formed. The lower electrode 42 is connected to the drain electrode 2 in the contact hole CH1. P sd electrical connection.
[0128] Next, a bank layer 48 is formed, which is used to define each of the multiple pixels Pix. The bank layer 48 has an opening corresponding to the pixel Pix, and the side of the opening includes an inclined surface having a positive tapered side portion. The inclined surface of the bank layer 48 surrounds each pixel. The bank layer 48 is formed using, for example, a photosensitive resin (such as polyimide or acrylic resin). The thickness of the bank layer 48 is, for example, greater than 1um and less than 2um. The inclination angle of the inclined surface of the bank layer 48 is less than 60°. When the inclination angle θb of the inclined surface of the bank layer 48 exceeds 60°, there is a case where defects occur in the layer located on the bank layer 48.
[0129] As described above, in order to remove the moisture contained in the bank layer 48 and the moisture contained in the organic planarization layer 2Pb, heating (drying) is preferred. The heating temperature is preferably, for example, above 100°C (for example, for more than 1 hour), and more preferably above 250°C (for example, for more than 15 minutes). The atmosphere may also be atmospheric pressure. If heating is performed under a reduced pressure atmosphere, the heating time can be shortened. In order to prevent thermal degradation during the heating (baking) process, the bank layer 48 and the organic planarization layer 2Pb are preferably formed of a resin material with high heat resistance, such as preferably formed of polyimide.
[0130] After that, the manufacturing of the element substrate may be interrupted to store or transport the element substrate. In this case, as described above, a positive photoresist film covering the surface of the element substrate formed to the bank layer 48 may be formed. After storage or transportation, before forming the organic layer 44, a clean surface can be obtained by removing the photoresist film. In addition, before forming the organic layer 44, the moisture contained in the organic planarization layer 2Pb and the body layer 48 is removed by heating.
[0131] Next, an organic layer 44 is formed on the lower electrode 42. The organic layer 44 is formed by, for example, vapor deposition. An upper electrode 46 is formed on the organic layer 44. The upper electrode 46 is in contact with the upper electrode contact portion 43 via the contact portion 2 P cV and common wiring 2 P cElectrical connection.
[0132] The lower electrode 42 and the upper electrode 46 constitute, for example, an anode and a cathode, respectively. The upper electrode 46 is a common electrode formed throughout the pixel in the active region, and the lower electrode (pixel electrode) 42 is formed for each pixel. If a bank layer 48 is present between the lower electrode 42 and the organic layer 44, holes will not be injected from the lower electrode 42 into the organic layer 44. Therefore, the region where the bank layer 48 is present does not function as a pixel Pix, and the bank layer 48 defines the outer edge of the pixel Pix. The bank layer 48 is sometimes referred to as a PDL (Pixel Defining Layer: physical layer).
[0133] After the OLED 3 is formed in this way, a TFE structure 10D is formed. The TFE structure 10D has the same structure as the TFE structure 10A. That is, the TFE structure 10D has a first inorganic barrier layer (e.g., SiN) from the side close to the OLED 3. x layer) 12, an organic barrier layer 14, and a second inorganic barrier layer (eg, SiN x Layer) 16. Fig.11 As shown in (c), the first inorganic barrier layer 12 is in contact with the upper surface and the inclined side surface of the second inorganic protective layer 2Pa2, the inclined side surface of the organic planarization layer 2Pb, and the upper surface of the first inorganic protective layer 2Pa1. That is, the OLED display device 100D has a Figure 3 The OLED display device 100A shown in (b) has the same structure and has excellent moisture resistance reliability.
[0134] Next, refer to Fig.12 (a) and (b) illustrate a film forming apparatus 200 for forming an organic barrier layer and a film forming method using the film forming apparatus 200. Fig.12 (a) and (b) are diagrams schematically showing the structure of the film forming apparatus 200. Fig.12 (a) shows the state of the film forming apparatus 200 in the process of condensing the photocurable resin on the first inorganic barrier layer in a chamber containing the vapor or mist of the photocurable resin. Fig.12 (b) shows the state of the film forming apparatus 200 in the step of irradiating the photocurable resin with light to which the photocurable resin is exposed to light and curing the photocurable resin.
[0135] The film forming device 200 has a chamber 210 and a partition wall 234 that divides the interior of the chamber 210 into two spaces. In one space of the chamber 210 separated by the partition wall 234, a workbench 212 and a shower plate 220 are arranged. In the other space separated by the partition wall 234, an ultraviolet irradiation device 230 is arranged. The chamber 210 controls the space inside it to a specified pressure (vacuum degree) and temperature. The workbench 212 has an upper surface for receiving an element substrate 20, and the upper surface can be cooled to, for example, -20°C. The element substrate 20 has a plurality of OLEDs 3 formed with a first inorganic barrier layer.
[0136] The shower plate 220 is configured to form a gap 224 between the shower plate 220 and the partition wall 234, and has a plurality of through holes 222. The vertical dimension of the gap 224 may be, for example, not less than 100 mm and not more than 1000 mm. The acrylic monomer (in the form of vapor or mist) supplied to the gap 224 is supplied from the plurality of through holes 222 of the shower plate 220 to the space on the side of the workbench 212 in the chamber 210. The acrylic monomer is heated as required. The vapor or mist of the acrylic monomer 26p of the acrylic monomer adheres to or contacts the first inorganic barrier layer of the element substrate 20. The acrylic monomer 26 is supplied from the container 202 to the chamber 210 at a predetermined flow rate. The acrylic monomer 26 is supplied to the container 202 via the pipe 206, and nitrogen is supplied to the container 202 from the pipe 204. The flow rate of the acrylic monomer to the container 202 is controlled by the flow controller 208. The shower plate 220 , the container 202 , the pipes 204 , 206 , the flow controller 208 and the like constitute a raw material supply device.
[0137] The ultraviolet irradiation device 230 has an ultraviolet light source and an optional optical element. The ultraviolet light source may be, for example, an ultraviolet lamp (such as a mercury lamp (including high pressure, ultra-high pressure), a mercury xenon lamp or a metal halide lamp). The optical element may be, for example, a reflector, a prism, a lens and a diffraction element.
[0138] When the ultraviolet irradiation device 230 is arranged at a predetermined position, it emits light having a predetermined wavelength and intensity toward the upper surface of the stage 212. The partition wall 234 and the shower plate 220 are preferably formed of a material having a high transmittance of ultraviolet rays, such as quartz.
[0139] The organic barrier layer 14 can be formed, for example, in the following manner using the film forming apparatus 200. Here, an example using an acrylic monomer as the photocurable resin is described.
[0140] The acrylic monomer 26p is supplied into the chamber 210. The element substrate 20 is cooled to, for example, -15°C on the workbench 212. The acrylic monomer 26p is condensed on the first inorganic barrier layer 12 of the element substrate 20. By controlling the conditions at this time, the liquid acrylic monomer can be unevenly distributed only around the convex portion of the first inorganic barrier layer 12. Alternatively, the conditions are controlled so that the acrylic monomer condensed on the first inorganic barrier layer 12 forms a liquid film.
[0141] By adjusting the viscosity and / or surface tension of the liquid photocurable resin, the thickness of the liquid film and the shape (concave shape) of the portion of the first inorganic barrier layer 12 in contact with the convex portion can be controlled. For example, the viscosity and surface tension depend on the temperature, and therefore can be controlled by adjusting the temperature of the element substrate. For example, the size of the solid portion existing on the flat portion can be controlled by the shape (concave shape) of the portion of the liquid film in contact with the convex portion of the first inorganic barrier layer 12 and the conditions of the subsequent ashing process.
[0142] Next, the ultraviolet irradiation device 230 is used to irradiate the entire upper surface of the element substrate 20 with ultraviolet rays 232 to cure the acrylic monomer on the first inorganic barrier layer 12. As the ultraviolet light source, for example, a high-pressure mercury lamp having a main peak at 365 nm is used, and as the ultraviolet intensity, for example, 12 mW / cm 2 , irradiate for about 10 seconds.
[0143] In this way, the organic barrier layer 14 made of acrylic resin is formed. The tact time of the process for forming the organic barrier layer 14 is, for example, less than about 30 seconds, and mass productivity is very high.
[0144] After curing the photocurable resin in the form of a liquid film, the organic barrier layer 14 may be formed only around the convex portion by ashing. In addition, when the organic barrier layer 14 is formed by curing the photocurable resin that is unevenly distributed, ashing may be performed. The ashing can improve the adhesion between the organic barrier layer 14 and the second inorganic barrier layer 16. That is, the ashing is not only used to remove the excess portion of the temporarily formed organic barrier layer, but also to modify (hydrophilize) the surface of the organic barrier layer 14.
[0145] Ashing can be performed using a known plasma ashing device, a light-excited ashing device, or a UV ozone ashing device. For example, it can be achieved by plasma ashing using at least one of N2O, O2, and O3, or by combining these with ultraviolet irradiation. x When the films are formed as the first inorganic barrier layer 12 and the second inorganic barrier layer 16, N2O is used as the raw material gas. Therefore, when N2O is used for ashing, there is an advantage that the device can be simplified.
[0146] When ashing is performed, the surface of the organic barrier layer 14 is oxidized and modified to be hydrophilic. In addition, the surface of the organic barrier layer 14 is roughly uniformly cut and extremely finely concavoconvex is formed, and the surface area is increased. The surface area increase effect when ashing is performed has a greater effect on the surface of the organic barrier layer 14 than on the first inorganic barrier layer 12 which is an inorganic material. Therefore, when the surface of the organic barrier layer 14 is modified to be hydrophilic, the surface area is increased, and thus the adhesion with the second inorganic barrier layer 16 is improved.
[0147] Then, the organic barrier layer 14 is transported to a CVD chamber for forming the second inorganic barrier layer 16, and the second inorganic barrier layer 16 is formed under the same conditions as the first inorganic barrier layer 12. The second inorganic barrier layer 16 is formed in the region where the first inorganic barrier layer 12 is formed, so an inorganic barrier layer joint portion for directly contacting the first inorganic barrier layer 12 and the second inorganic barrier layer 16 is formed in the non-solid portion of the organic barrier layer 14. Therefore, as described above, water vapor in the atmosphere is suppressed / prevented from reaching the active region via the organic barrier layer.
[0148] In addition, the first inorganic barrier layer 12 and the second inorganic barrier layer 16 are formed, for example, in the following manner. By using a plasma CVD method using SiH4 and N2O gases, for example, an inorganic barrier layer having a thickness of 400 nm can be formed at a film forming rate of 400 nm / min while the temperature of the substrate (OLED 3) to be film-formed is controlled to be below 80°C. The inorganic barrier layer thus obtained has a refractive index of 1.84 and a transmittance of visible light of 400 nm of 90% (thickness of 400 nm). In addition, the absolute value of the film stress is 50 MPa.
[0149] In addition, as an inorganic barrier layer, in addition to SiN x In addition to the SiO2 layer, SiO x N y (x>y) layer, SiN x O y (x>y) layer, Al2O3 layer, etc. The photocurable resin includes, for example, monomers containing vinyl groups. Among them, acrylic monomers are preferably used. Acrylic monomers can be mixed with photopolymerization initiators as needed. Various well-known acrylic monomers can be used. Multiple acrylic monomers can also be mixed. For example, bifunctional monomers and trifunctional or higher multifunctional monomers can also be mixed. In addition, oligomers can also be mixed. The viscosity of the photocurable resin at room temperature (for example, 25°C) before curing is preferably not more than 10Pa·s, and particularly preferably 1 to 100mPa·s. When the viscosity is high, it is sometimes difficult to form a thin liquid film with a thickness of less than 500nm.
[0150] In the above, although an OLED display device having a flexible substrate and a method for manufacturing the same are described, the embodiments of the present invention are not limited to the exemplified embodiments and can be widely applied to an organic EL device (e.g., an organic EL lighting device) having an organic EL element formed on a substrate that is not flexible (e.g., a glass substrate) and a thin film sealing structure formed on the organic EL element. Industrial Applicability
[0151] The embodiments of the present invention are used in an organic EL device and a method for manufacturing the same. The embodiments of the present invention are particularly suitable for use in a flexible organic EL display device and a method for manufacturing the same. Description of Reference Numerals
[0152] 1: Flexible substrate; 2: Backplane (circuit) 2Pa: Inorganic protective layer (first inorganic protective layer), inorganic protective film (first inorganic protective Protective film) 2Pa1: first inorganic protective layer, first inorganic protective film 2Pa2: Second inorganic protective layer, second inorganic protective film 2Pb: organic planarization layer, organic planarization film 3: Organic EL components 4: Polarizing plate 10: Thin film sealing structure (TFE structure) 12: The first inorganic barrier layer (SiN x layer) 14: Organic barrier layer (acrylic resin layer) 16: Second inorganic barrier layer (SiN x layer) 20: Component substrate 26: Acrylic monomer 26p: Vapor or mist of acrylic monomers 100, 100A, 100D: Organic EL display device 200: Film forming device
Claims
1. An EL device, characterized in that: The EL device comprises: substrate; A driving circuit layer, the driving circuit layer comprising: a plurality of TFTs formed on the substrate, a plurality of gate buses and a plurality of source buses respectively connected to any one of the plurality of TFTs, a plurality of terminals, and a plurality of lead-out wirings connecting the plurality of terminals to any one of the plurality of gate buses or the plurality of source buses; A first inorganic protective layer, formed on the driving circuit layer, exposing at least the plurality of terminals; an organic planarization layer formed on the first inorganic protective layer, the organic planarization layer having a surface with an arithmetic average roughness Ra of 50 nm or less; an EL element layer formed on the organic planarization layer and having a plurality of EL elements respectively connected to any one of the plurality of TFTs; a thin film sealing structure formed in a manner covering the EL element layer, comprising a first inorganic barrier layer, an organic barrier layer in contact with an upper surface of the first inorganic barrier layer, and a second inorganic barrier layer in contact with an upper surface of the organic barrier layer, wherein the organic barrier layer is formed in a region surrounded by an inorganic barrier layer junction portion where the first inorganic barrier layer and the second inorganic barrier layer are in direct contact with each other, When observed from the normal direction of the substrate, the organic planarization layer is formed in the region where the first inorganic protective layer is formed, the plurality of EL elements are arranged in the region where the organic planarization layer is formed, the outer edge of the thin film sealing structure intersects the plurality of lead wirings and exists between the outer edge of the organic planarization layer and the outer edge of the first inorganic protective layer, In a portion where the first inorganic protective layer and the first inorganic barrier layer are in direct contact with each other on the lead wirings, a taper angle of a side surface of a cross-section of the first inorganic barrier layer parallel to a line width direction of the lead wirings is less than 90°.
2. The EL device according to claim 1, characterized in that The EL device further has a second inorganic protective layer formed on the organic planarization layer, The EL element layer is formed on the second inorganic protective layer.
3. The EL device according to claim 1 or 2, characterized in that The taper angle of the side surface of the first inorganic barrier layer is less than 70°.
4. The EL device according to claim 1 or 2, characterized in that: The organic planarization layer is formed of a photosensitive resin.
5. The EL device according to claim 1 or 2, characterized in that: The organic planarization layer is formed of polyimide.
6. A method for manufacturing an EL device, which is the method for manufacturing an EL device according to any one of claims 1 to 5, characterized in that: The manufacturing method comprises: Step A, forming the driving circuit layer on the substrate; Step B, forming a first inorganic protective film on the driving circuit layer; Step C, forming an organic planarization film on the first inorganic protective film; Step D, performing chemical mechanical polishing on the surface of the organic planarization film; Step E, obtaining the first inorganic protective layer and the organic planarization layer by patterning the first inorganic protective film and the organic planarization film; Step F, heating the organic planarization layer to a temperature above 100° C.; and Step G: after step F, forming a layer included in the EL element on the organic planarizing layer.
7. The manufacturing method according to claim 6, characterized in that: After step D and before step E, the method further includes: forming a second inorganic protective film on the organic planarization film; and The step of forming a contact hole penetrating the first inorganic protective film, the organic planarization film, and the second inorganic protective film is performed simultaneously.
8. The manufacturing method according to claim 6 or 7, characterized in that: After step E and before step F, the method further includes: Step E1, forming a positive photoresist film covering the organic planarization layer; and In step E2, the photoresist film is removed by exposing the entire surface of the photoresist film and then developing the film.
9. The manufacturing method according to claim 8, characterized in that: A step of storing or transporting the substrate on which the photoresist film is formed is included between the step E1 and the step E2.
10. The manufacturing method according to claim 6 or 7, characterized in that: The manufacturing method further comprises: Step H, after step G, selectively forming the first inorganic barrier layer in the active region where the plurality of EL elements are formed; Step I, after step H, placing the substrate in a chamber and supplying vapor or mist of a photocurable resin into the chamber; Step J is a step of condensing a photocurable resin on the first inorganic barrier layer, wherein the photocurable resin is condensed so that the photocurable resin does not exist on a portion of the first inorganic barrier layer where the taper angle is less than 90°; and Step K, after step J, irradiating the condensed photocurable resin with light to form the organic barrier layer made of photocurable resin.
11. The manufacturing method according to claim 6 or 7, characterized in that: The manufacturing method further comprises: Step H, after step G, selectively forming the first inorganic barrier layer in the active area where the plurality of EL elements are formed; Step I, after step H, placing the substrate in a chamber and supplying vapor or mist of a photocurable resin into the chamber; Step J, condensing the photocurable resin on the first inorganic barrier layer to form a liquid film; Step K, forming a photocurable resin layer by irradiating the liquid film of the photocurable resin with light; and Step L: forming the organic barrier layer by partially ashing the photocurable resin layer.