18-valence electron Half-Heusler thermoelectric material and preparation method thereof

By preparing 18-valent electronic Half-Heusler thermoelectric materials, using ZrCoxNi1-xSn1-xSbx and NbFeyCo1-ySn1-ySby systems, the lattice thermal conductivity is reduced, the problem of low thermoelectric conversion efficiency of thermoelectric materials is solved, and the higher thermoelectricity is achieved Performance and wider application prospects.

CN119031813APending Publication Date: 2024-11-26SOUTHWEST JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411140903.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The high lattice thermal conductivity of existing thermoelectric materials limits the improvement of their thermoelectric conversion efficiency, resulting in limited application of thermoelectric devices.

Method used

Using the 18-valent electron Half-Heusler thermoelectric material system, the preparation methods of alloy compounds ZrCoxNi1-xSn1-xSbx and NbFeyCo1-ySn1-ySby, including magnetic levitation smelting, grinding, wet ball milling and discharge plasma sintering, reducing the lattice thermal conductivity .

Benefits of technology

It significantly reduces the thermal conductivity of the lattice, increases the ZT value of thermoelectric materials, improves its thermoelectric performance, and has a wider range of industrial application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031813A_ABST
    Figure CN119031813A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of thermoelectric materials, in particular to a 18-valence electron Half-Heusler thermoelectric material and a preparation method thereof. The 18-valence electron Half-Heusler thermoelectric material provided by the invention comprises ZrCo < x > Ni < 1-x > Sn < 1-x > Sb < x > and / or NbFe < y > Co < 1-y > Sn < 1-y > by, and x is greater than or equal to 0 and less than or equal to 1; y is greater than or equal to 0 and less than or equal to 1. The intrinsic lattice thermal conductivity of the thermoelectric material is closely related to the number N of atoms in an original unit cell, so that the lattice thermal conductivity is obviously reduced along with the increase of N. The ZrCo < x > Ni < 1-x > Sn < 1-x > Sb < x > and the NbFe < y > Co < 1-y > Sn < 1-y > Sby provided by the invention have larger N values compared with common three-principal-element and four-principal-element thermoelectric materials, so that the ZrCo < x > Ni < 1-x > Sn < 1-x > Sb < x > and the NbFe < y > Co <
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermoelectric materials, and in particular to an 18-valence electron Half-Heusler thermoelectric material and a preparation method thereof. Background Art

[0002] Thermoelectric devices can directly convert heat and electrical energy into each other based on the carrier transport characteristics, effectively recovering industrial waste heat and automobile exhaust waste heat. In addition, based on the thermoelectric effect, thermoelectric materials are widely used in thermocouple temperature measurement related fields, and also have certain applications in portable refrigerators, constant temperature water baths, deep space exploration and other fields. However, the conversion efficiency of thermoelectric devices is still far behind that of traditional heat engines. Therefore, the low thermoelectric conversion efficiency has become a key problem restricting the widespread application of thermoelectric devices.

[0003] Thermoelectric conversion efficiency depends largely on the thermoelectric figure of merit ZT. The larger the ZT value, the higher the thermoelectric conversion efficiency. Thermoelectric figure of merit is defined as ZT = α 2 σT / κ, where α is the Seebeck coefficient, σ is the conductivity, and α is the 2 σ can also be defined as the power factor PF, T is the absolute temperature, and κ is the total thermal conductivity, including the lattice (phonon) thermal conductivity κ l and the electronic thermal conductivity κ e (κ=κ l +κ e ). Therefore, in order to obtain a high ZT value, the material needs to have a high Seebeck coefficient and electrical conductivity, and low thermal conductivity, so as to improve the thermoelectric conversion efficiency of the material. However, due to these thermoelectric parameters (Seebeck coefficient α, electrical conductivity σ and electronic thermal conductivity κ e ) has a strong dependence on the carrier concentration n and is coupled to each other, that is, obtaining a high conductivity σ by adjusting the carrier concentration n often leads to a low Seebeck coefficient α and a high electronic thermal conductivity κ e Therefore, how to effectively improve the ZT value has always been a difficult problem that has troubled the academic community.

[0004] Half-Heusler (HH) alloy is a thermoelectric material with excellent thermoelectric and mechanical properties. Since its operating temperature range is in the medium and high temperature region, it can be used as a potential thermoelectric material in the fields of waste heat recovery and deep space exploration, and has a very broad prospect for industrial application. At present, the ZT value of some HH thermoelectric alloys has exceeded 1, mainly including ZrNiSn, ZrCoSb, ZrCoBi, NbFeSb and TaFeSb systems. However, the intrinsic lattice thermal conductivity of the above common three-principal HH thermoelectric alloy systems is generally high, which limits the substantial improvement of their ZT value. In the early stage, researchers mainly introduced point defects, grain boundaries and nano-precipitation phases into the HH thermoelectric alloy matrix to regulate the multi-scale hierarchical structure, thereby scattering phonons of different frequencies to reduce the lattice thermal conductivity and increase the ZT value. However, the optimized lattice thermal conductivity is still higher than that of other typical thermoelectric material systems. Therefore, the development of new HH thermoelectric alloys is expected to fundamentally solve the problem of high lattice thermal conductivity and bring more possibilities for the subsequent regulation of other thermoelectric parameters, thereby greatly improving the thermoelectric performance of the system and giving it a broader prospect for industrial application. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides an 18-valence electron Half-Heusler thermoelectric material and a preparation method and application thereof. The 18-valence electron Half-Heusler thermoelectric material provided by the present invention has low lattice thermal conductivity and is more widely used.

[0006] The present invention provides an 18-valence electron Half-Heusler thermoelectric material, comprising ZrCo x Ni 1-x Sn 1-x Sb x and / or NbFe y Co 1-y Sn 1-y Sb y , where the value range of x is 0≤x≤1; the value range of y is 0≤y≤1.

[0007] The present invention also provides a method for preparing the ZrNiSn-based Half-Heusler alloy thermoelectric material described in the above technical solution, comprising the following steps:

[0008] Corresponding to ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb yThe chemical element composition of ZrNiSn and ZrCoSb alloy raw material group, NbFeSb and NbCoSb alloy raw material group were smelted under protective atmosphere conditions to obtain ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y Alloy ingots;

[0009] ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y The alloy ingots were ground and dried in turn to obtain ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y Alloy powder;

[0010] The ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y The alloy powders are respectively subjected to spark plasma sintering to obtain the 18-valence electron Half-Heusler thermoelectric material.

[0011] Preferably, the protective atmosphere is argon; the smelting is magnetic suspension smelting; the smelting temperature is 1600-1800°C, the holding time is 1-5 minutes, and the argon pressure is 10 4 ~10 5 Pa; the number of smelting is 3 to 6 times.

[0012] Preferably, the heating rate to the smelting temperature is 1000-3000° C. / min.

[0013] Preferably, the grinding process is performed until the particle size of the material is 0.5-2 μm.

[0014] Preferably, the grinding comprises firstly grinding the ingot into powder with a particle size of 0.1 to 1 mm using a mortar; and then performing wet ball milling in an argon atmosphere.

[0015] Preferably, the medium for wet ball milling is anhydrous ethanol, the ball-to-material ratio is 10 to 20:1, the rotation speed is 200 to 600 r / min, and the wet ball milling time is 5 to 20 h.

[0016] Preferably, the temperature of the spark plasma sintering is 800-1000° C., the pressure of the spark plasma sintering is 80-100 MPa, and the holding time is 5-20 min.

[0017] Preferably, the heating rate to the spark plasma sintering temperature is 100-300° C. / min.

[0018] The present invention provides an 18-valence electron Half-Heusler thermoelectric material, comprising ZrCo x Ni 1-x Sn 1-x Sb x and / or NbFe y Co 1-y Sn 1-y Sb y , where x is in the range of 0≤x≤1; y is in the range of 0≤y≤1. Since the intrinsic lattice thermal conductivity of thermoelectric materials is closely related to the number of atoms N in the original unit cell, the lattice thermal conductivity decreases significantly with the increase of the number of atoms N in the unit cell. x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y Compared with the common three-principal element and four-principal element HH thermoelectric materials, it has a higher N value and thus has a lower lattice thermal conductivity. x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y The lattice thermal conductivity of the thermoelectric material is significantly lower than that of the traditional three-principal HH thermoelectric material, and it has a higher ZT value. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 (a) is the five main elements ZrCo in Example 1 0.5 Ni0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 XRD pattern of HH thermoelectric alloy sample; (b) XRD pattern of bulk four principal element sample;

[0020] Figure 2 ZrCo in Example 1 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 Comparison chart of lattice thermal conductivity of HH thermoelectric alloy sample and common three-principal element, four-principal element and five-principal element lattice thermal conductivity prepared in this project;

[0021] Figure 3 ZrCo in Example 1 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 (a) Electrical conductivity; (b) Seebeck coefficient; (c) Power factor diagram of HH thermoelectric alloy sample;

[0022] Figure 4 ZrCo in Example 1 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 ZT value diagram of HH thermoelectric alloy specimens. DETAILED DESCRIPTION

[0023] The present invention provides an 18-valence electron Half-Heusler thermoelectric material, comprising ZrCo x Ni 1-x Sn 1-x Sb x and / or NbFe y Co 1-y Sn 1-y Sb y , where the value range of x is 0≤x≤1; the value range of y is 0≤y≤1.

[0024] In the present invention, the 18-valence electron Half-Heusler thermoelectric material is preferably ZrCo x Ni 1-x Sn 1-x Sb x and / or NbFe y Co 1-y Sn 1-y Sb.

[0025] The present invention also provides a method for preparing the 18-valence electron Half-Heusler thermoelectric material described in the above technical solution, comprising the following steps:

[0026] Corresponding to ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y The chemical element composition of ZrNiSn and ZrCoSb alloy raw material group, NbFeSb and NbCoSb alloy raw material group were smelted under protective atmosphere conditions to obtain ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y Alloy ingots;

[0027] ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y The alloy ingots were ground and dried in turn to obtain ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y Alloy powder;

[0028] The ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn1-y Sb y The alloy powders are respectively subjected to spark plasma sintering to obtain the 18-valence electron Half-Heusler thermoelectric material.

[0029] The present invention corresponds to ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y The chemical element composition of ZrNiSn and ZrCoSb alloy raw material group, NbFeSb and NbCoSb alloy raw material group were smelted under protective atmosphere conditions to obtain ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y Alloy ingot.

[0030] In the present invention, the protective atmosphere is argon; the smelting is preferably magnetic suspension smelting; the smelting temperature is preferably 1600-1800°C, more preferably 1650-1750°C; the heating rate to the smelting temperature is preferably 1000-3000°C / min, more preferably 1500-2500°C / min; the holding time is preferably 1-5min, more preferably 3-5min; during the smelting, the argon pressure is preferably 10 4 ~10 5 Pa, more preferably 5×10 4 Pa; the number of smelting is preferably 3 to 6 times, more preferably 4 to 5 times.

[0031] After obtaining the alloy ingot, the present invention respectively x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y The alloy ingots were ground and dried in turn to obtain ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y Alloy powder.

[0032] In the present invention, the grinding is preferably performed until the material particle size is 0.5 to 2 μm. In the present invention, the grinding is preferably performed by first using a mortar to coarsely grind the ingot into a powder with a particle size of 0.1 to 1 mm, and then wet ball milling is performed under an argon atmosphere; the medium for wet ball milling is preferably anhydrous ethanol, the ball-to-material ratio is preferably 10 to 20:1, more preferably 15:1, the rotation speed is preferably 200 to 600 r / min, more preferably 300 to 500 r / min; the time for wet ball milling is preferably 5 to 20 h, more preferably 10 to 15 h.

[0033] In the present invention, after the grinding, it is preferred to further include suction filtration.

[0034] In the present invention, the drying is preferably natural drying, and the natural drying step is preferably to dry the filtered powder naturally in a glove box for 12 to 48 hours, more preferably to dry it naturally for 12 to 24 hours.

[0035] After obtaining the alloy powder, the present invention further comprises: x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y The alloy powders are respectively subjected to spark plasma sintering to obtain the 18-valence electron Half-Heusler thermoelectric material.

[0036] In the present invention, the temperature of the spark plasma sintering is preferably 800-1000°C, more preferably 900-1000°C; the heating rate to the temperature of the spark plasma sintering is preferably 100-300°C / min, more preferably 150-250°C / min; the pressure of the spark plasma sintering is preferably 80-100MPa, more preferably 100MPa, and the holding time is preferably 5-20min, more preferably 10-15min.

[0037] The present invention adopts the double 18-valence electron principle (i.e., mixing two adjacent 18-valence electron HH system compounds) and mixes the currently common three-principal HH thermoelectric alloys of ZrNiSn and ZrCoSb, NbFeSb and NbCoSn to prepare a new single-phase ZrCo with low lattice thermal conductivity. 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5HH thermoelectric alloy.

[0038] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0039] Example 1

[0040] Material selection: According to the master alloy ZrCo 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 The chemical formula elements are proportioned and smelted to prepare ZrCo 0.5 Ni 0.5 Sn 0.5 Sb 0.5 ZrNiSn and ZrCoSb alloys were selected as raw materials and mixed in a molar ratio of 1:1. 0.5 Co 0.5 Sn 0.5 Sb 0.5 NbFeSb and NbCoSn alloys are selected as raw materials and mixed in a molar ratio of 1:1; the atomic percentage of each element is: Zr: 33.2%; Co: 16.7%; Ni: 16.7%; Sn: 16.7%; Sb 16.7%; Nb: 33.2%; Fe: 16.7%.

[0041] Melting: A magnetic levitation melting furnace was used. In an argon protective atmosphere (pressure of 0.07 MPa), the temperature was raised to 1700°C and then kept warm for 3 minutes. The melting was repeated 4 times to obtain an alloy ingot.

[0042] Ball milling and filtration: First, the alloy ingot was coarsely ground into powder with a particle size of 0.5 mm using a mortar, and then wet ball milled in an argon atmosphere. The wet ball milling medium was anhydrous ethanol, the ball-to-material ratio was 15:1, the rotation speed was 500 r / min, and the ball milling time was 10 h.

[0043] After wet ball milling, the alloy powder with a particle size of ~1μm was obtained by filtration.

[0044] Drying treatment: The filtered powder was naturally dried in a glove box for 24 hours.

[0045] Sintering: The dried alloy powder was subjected to spark plasma sintering at a sintering temperature of 950°C, a sintering pressure of 100 MPa, and a holding time of 15 min to obtain ZrCo 0.5 Ni 0.5 Sn 0.5 Sb0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 HH thermoelectric alloy specimen.

[0046] Example 2

[0047] Material selection: According to the master alloy ZrCo 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 The chemical formula elements are proportioned and smelted to prepare ZrCo 0.5 Ni 0.5 Sn 0.5 Sb 0.5 ZrNiSn and ZrCoSb alloys were selected as raw materials and mixed in a molar ratio of 1:1. 0.5 Co 0.5 Sn 0.5 Sb 0.5 NbFeSb and NbCoSn alloys are selected as raw materials and mixed in a molar ratio of 1:1; the atomic percentage of each element is: Zr: 33.2%; Co: 16.7%; Ni: 16.7%; Sn: 16.7%; Sb 16.7%; Nb: 33.2%; Fe: 16.7%.

[0048] Melting: A magnetic levitation melting furnace was used. In an argon protective atmosphere (pressure of 0.07 MPa), the temperature was raised to 1700°C and then kept warm for 4 minutes. The melting was repeated 5 times to obtain an alloy ingot.

[0049] Ball milling and filtration: First, the alloy ingot was coarsely ground into powder with a particle size of 0.1-1 mm using a mortar, and then wet ball milled in an argon atmosphere. The wet ball milling medium was anhydrous ethanol, the ball-to-material ratio was 20:1, the rotation speed was 600 r / min, and the ball milling time was 8 h.

[0050] After wet ball milling, the alloy powder with a particle size of ~1μm was obtained by filtration.

[0051] Drying treatment: The filtered powder was naturally dried in a glove box for 24 hours.

[0052] Sintering: The dried alloy powder was subjected to spark plasma sintering at a sintering temperature of 850°C, a sintering pressure of 90 MPa, and a holding time of 20 min to obtain a ZrNiSn-based Half-Heusler alloy thermoelectric material.

[0053] ZrCo prepared in Example 1 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 The XRD patterns of HH thermoelectric alloy samples and four principal element samples are shown in Figure 1 As shown, from Figure 1 It can be seen that the prepared ZrCo 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 HH thermoelectric alloys are all single-phase, while a large number of impurity phases are generated in quaternary HH alloys without 18 valence electrons.

[0054] The present invention uses a laser thermal conductivity meter and a transient laser flash method to directly measure the thermal diffusion coefficient of the material, and then calculates the lattice thermal conductivity. The ZrCo prepared in Example 1 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 The lattice thermal conductivity of the HH thermoelectric alloy sample is compared with the lattice thermal conductivity of the common three-principal element, four-principal element and the five-principal element prepared in this project. Figure 2 As shown. Figure 2 It can be seen that ZrCo 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 The intrinsic lattice thermal conductivity of the HH thermoelectric alloy sample is significantly lower than that of the common three-principal element and four-principal element systems.

[0055] The present invention uses an electrical comprehensive test system and a laser thermal conductivity meter to measure the ZrCo prepared in Example 1. 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5The thermoelectric properties of HH thermoelectric alloy samples above room temperature, including conductivity, Seebeck coefficient and power factor, are shown in Figure 2. Figure 3 As shown, from Figure 3 It can be seen that ZrCo 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 HH thermoelectric alloy samples have excellent electrical properties.

[0056] ZrCo prepared in Example 1 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 The ZT value of HH thermoelectric alloy sample is as follows Figure 4 As shown. Figure 4 It can be seen that: NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 The ZT value of the HH sample is as high as 0.25 at 1073K, while the five main elements ZrCo 0.5 Ni 0.5 Sn 0.4 Sb 0.6 The ZT value of the HH sample is as high as 0.58 at 1123K.

[0057] This embodiment firstly introduces the dual 18-valence electron design concept into the preparation of Half-Heusler alloy, thereby preparing a new type of five principal elements with low lattice thermal conductivity and high ZT value, providing more possibilities for the industrial application of medium and high temperature Half-Heusler thermoelectric materials. 0.5 Ni 0.5 Sn 0.5 Sb 0.5 and NbFe 0.5 Co 0.5 Sn 0.5 Sb 0.5 The lattice thermal conductivity of Half-Heusler thermoelectric materials is significantly lower than that of common three-principal element and four-principal element HH thermoelectric materials, thus successfully solving the problem of high lattice thermal conductivity of HH thermoelectric material system.

[0058] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. An 18-valence electron Half-Heusler thermoelectric material, characterized in that: Including ZrCo x Ni 1-x Sn 1-x Sb x and / or NbFe y Co 1-y Sn 1-y Sb y , where the value range of x is 0≤x≤1; the value range of y is 0≤y≤1.

2. The method for preparing the 18-valence electron Half-Heusler thermoelectric material according to claim 1, characterized in that: The following steps are involved: Corresponding to ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y The chemical element composition of ZrNiSn and ZrCoSb alloy raw material group, NbFeSb and NbCoSb alloy raw material group were smelted under protective atmosphere conditions to obtain ZrCo x Ni 1- x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y Alloy ingots; ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y The alloy ingots were ground and dried in turn to obtain ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y Alloy powder; The ZrCo x Ni 1-x Sn 1-x Sb x and NbFe y Co 1-y Sn 1-y Sb y The alloy powders are respectively subjected to spark plasma sintering to obtain the 18-valence electron Half-Heusler thermoelectric material.

3. The preparation method according to claim 2, characterized in that: The protective atmosphere is argon; the smelting is magnetic suspension smelting; the smelting temperature is 1600-1800°C, the holding time is 1-5 minutes, and the argon pressure is 10 4 ~10 5 Pa; the number of smelting is 3 to 6 times.

4. The preparation method according to claim 3, characterized in that: The heating rate to the smelting temperature is 1000-3000°C / min.

5. The preparation method according to claim 2, characterized in that: The grinding step is performed until the particle size of the material is 0.5 to 2 μm.

6. The preparation method according to claim 5, characterized in that: The grinding is to firstly grind the ingot into powder with a particle size of 0.1 to 1 mm using a mortar, and then perform wet ball milling in an argon atmosphere.

7. The preparation method according to claim 6, characterized in that: The medium of the wet ball milling is anhydrous ethanol, the ball-to-material ratio is 10-20:1, the rotation speed is 200-600 r / min, and the wet ball milling time is 5-20 hours.

8. The preparation method according to claim 2, characterized in that: The temperature of the spark plasma sintering is 800-1000° C., the pressure of the spark plasma sintering is 80-100 MPa, and the heat preservation time is 5-20 minutes.

9. The preparation method according to claim 8, characterized in that: The heating rate to the spark plasma sintering temperature is 100 to 300° C. / min.