Low volatile radiation curable composition for coating optical fibers
By using fiber primary coating compositions with oligomer and urethane components on the fiber, the microbending and volatile problems of fiber coating during thermal aging and hydrolysis are solved, and stability and fiber adhesion are achieved. Improvement of sex.
Patent Information
- Application Number
- CN202380034724.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-21
- Filing Date
- 2023-04-19
- Publication Date
- 2024-11-26
AI Technical Summary
Existing optical fiber coatings are prone to microbending during thermal aging and hydrolysis, resulting in signal transmission attenuation, and high content of volatile monomers and diluents, affecting fiber adhesion and curing speed.
An optical fiber primary coating composition is adopted, including oligomers, isocyanate compounds, hydroxy functional blocking agents and carbamate oligomers, to form a solid coating by ultraviolet curing, reducing volatility and improving adhesion.
It is achieved to reduce the volatility and micro-bending resistance of the optical fiber coating while maintaining acceptable curing speed and fiber properties, and improve the stability and fiber adhesion of the coating.
Smart Images

Figure BDA0005089509280000271 
Figure BDA0005089509280000281 
Figure BDA0005089509280000311
Abstract
Description
Technical Field
[0001] The present invention relates generally to radiation curable formulations, particularly suitable as primary coating compositions for optical fibers, methods of coating optical fibers with the radiation curable formulations as primary coating compositions, and coated optical fibers produced thereby.
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] none
[0004] background
[0005] Optical fiber is composed of glass fiber obtained by hot melt spinning of glass and one or more coatings provided on the glass fiber for protection and reinforcement. For example, optical fiber is produced by first forming a flexible primary coating on the surface of the glass fiber and then forming a more rigid secondary covering layer (called secondary coating) on the primary coating. Also known are ribbon optical fibers or optical fiber cables, which have a plurality of coated optical fibers bonded with a bonding material.
[0006] Radiation-curable thermosetting compositions have long been used to form primary and secondary coatings because they cure particularly quickly and impart desirable properties to optical fibers. Typically, radiation-curable optical fiber coatings are the cured product of a composition containing a mixture of one or more components having one or more ethylenically unsaturated (C=C) bonds that crosslink by free radical polymerization under the influence of radiation. Such compositions also typically include a photoinitiator to facilitate radiation curing, particularly when curing is achieved by irradiation at ultraviolet (UV) wavelengths.
[0007] The relatively soft inner primary coating provides resistance to microbending, which is undesirable due to increased signal transmission attenuation (i.e., signal loss) in the coated optical fiber. Microbending is a microscopic curvature in an optical fiber involving local axial displacements of a few microns and spatial wavelengths of a few millimeters. Microbending can be caused by thermal stresses and / or mechanical lateral forces. The coating can provide lateral force protection to prevent microbending of the optical fiber, but the amount of protection provided decreases as the coating thickness decreases.
[0008] The primary coating preferably has a higher refractive index than the cladding of the associated optical fiber to allow them to strip errant optical signals from the optical fiber core. The primary coating should maintain adequate adhesion to the glass fiber during thermal and hydrolytic aging and (if necessary) be capable of being stripped therefrom for splicing purposes. The primary coating typically has a thickness in the range of 20 to 50 μm (e.g., about 25 or 32.5 μm), with a thinner thickness in the range of 15 to 25 μm for 200 μm fiber.
[0009] The harder secondary coating provides resistance to processing forces, such as those encountered when the coated optical fiber is formed into ribbons and / or cables. The radiation-curable optical fiber secondary coating composition also typically comprises a mixture of ethylenically unsaturated compounds, including one or more acrylate-functional oligomers dissolved or dispersed in a liquid ethylenically unsaturated diluent and a photoinitiator. The coating composition is typically applied to the optical fiber in liquid form and then exposed to actinic radiation to achieve cure.
[0010] Methods commonly used to form a covering on a glass fiber are, for example, coating the glass fiber with a liquid curable resin composition and curing it with heat or light (and especially ultraviolet radiation). Optical fiber coatings (including primary and secondary layers) are typically applied using one of two processes: wet-on-wet (WOW) and wet-on-dry (WOD). In the WOD process, the fiber first undergoes a primary coating application and is then cured by exposure to ultraviolet radiation. The fiber then undergoes a secondary coating application, which is then cured in a similar manner. In the WOW process, the fiber undergoes primary and secondary coating applications and then the fiber undergoes a curing step. In the wet-on-wet process, the curing lamp between the primary and secondary coating applications is omitted.
[0011] There is a continuing quest for more sustainable and effective optical fiber coatings. Known optical fiber coatings that cure quickly enough and provide adequate on-fiber performance, and yet are able to adequately adhere to their associated optical fiber substrates, still have room for improvement. Specifically, it would be desirable to provide an optical fiber primary coating that maintains acceptable cure speeds and on-fiber performance, as desired by the industry, but still has lower volatility, as evidenced by reduced levels of monomers and / or diluent compounds contained therein. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] none
[0014] Brief description
[0015] Several aspects and embodiments of the invention are described herein. The first aspect is an optical fiber primary coating composition comprising, relative to the weight of the entire primary coating composition: (a) at least 0.01 wt. % of one or more oligomers, the oligomers being the reaction product of (i) a hydroxyl or thiol functional backbone compound, (ii) an isocyanate compound, and (iii) a hydroxyl functional endcapping agent further comprising an ethylenically unsaturated moiety; wherein the molar ratio of the number of isocyanate groups in (ii) to the number of hydroxyl and thiol groups in (i) is less than or equal to 1.0; (b) optionally, one or more urethane (meth)acrylate oligomers other than (a); (c) optionally, a reactive diluent monomer; (d) a photoinitiator; (e) optionally, one or more additives; wherein the total amount of (a) + (b) is between 70 wt. % and 99 wt. %. If (b) is not present, the one or more oligomers according to (a) preferably have at least two ethylenically unsaturated groups. More preferably, if (b) is absent, the one or more oligomers according to (a) have two ethylenically unsaturated groups.
[0016] In another embodiment according to the first aspect, the one or more oligomers according to (a) are present in an amount greater than 0.1 wt%, preferably greater than 1 wt%, preferably greater than 5 wt%, preferably greater than 10 wt%, preferably greater than 40 wt%, and preferably less than or equal to 96 wt%, more preferably less than or equal to 95 wt%, more preferably less than or equal to 90 wt%, more preferably less than or equal to 80 wt%, more preferably less than or equal to 70 wt%. In still other embodiments, the molar ratio of the number of isocyanate groups in (ii) to the number of hydroxyl and thiol groups in (i) is greater than or equal to 2 / 3, such that the ratio is between 2 / 3 (about 0.67) and 1.0. In various other embodiments of the first aspect, the one or more oligomers according to (a) have a variety of urethane bonds, block structures, theoretical molecular weight values, termination moieties, backbone types, isocyanate types, and hydroxyl functional end cap types. In still other embodiments, more specific types are described for elements (b)-(e).
[0017] The second aspect of the present invention is a method for coating an optical fiber, comprising providing a glass optical fiber, preferably drawing the glass optical fiber by a drawing tower; applying a primary coating composition to the surface of the glass optical fiber; optionally, applying a dose of ultraviolet light sufficient to at least partially cure the primary coating composition; applying a secondary coating composition to the primary coating composition; exposing the primary coating composition and the secondary coating composition to at least one radiation source capable of emitting ultraviolet radiation to affect the curing of the primary coating composition and the secondary coating composition to form a cured primary coating on the surface of the optical fiber and a cured secondary coating on the surface of the cured primary coating; wherein the primary coating composition is a composition according to any embodiment of the first aspect of the present invention.
[0018] The third aspect of the present invention is a coated optical fiber, which includes a glass core and a cladding in contact with and surrounding the glass core; and a coating portion, the coating portion further including a primary coating in contact with and surrounding the cladding; and a secondary coating in contact with and surrounding the primary coating. According to the third aspect, the primary coating is a cured product of a radiation-curable composition according to any embodiment of the first aspect, and the primary coating and the secondary coating are applied and cured according to any embodiment of the second aspect.
[0019] Detailed Description
[0020] The first aspect of the present invention is an optical fiber primary coating composition, which comprises, consists essentially of, or consists of the following components, measured by weight relative to the entire primary coating composition:
[0021] (a) at least 0.01 wt. % of one or more oligomers which are the reaction product of (i) a hydroxy or thiol functional backbone compound, (ii) an isocyanate compound, and (iii) a hydroxyl functional end-capping agent further comprising an ethylenically unsaturated moiety; wherein the molar ratio of the number of isocyanate groups in (ii) to the number of hydroxyl and thiol groups in (i) is less than or equal to 1.0;
[0022] (b) optionally, one or more urethane (meth)acrylate oligomers other than (a);
[0023] (c) optionally, a reactive diluent monomer;
[0024] (d) a photoinitiator;
[0025] (e) optionally, one or more additives;
[0026] The total amount of (a) + (b) is 70 wt % to 99 wt %.
[0027] If (b) is not present, the one or more oligomers according to (a) preferably have at least two ethylenically unsaturated groups. More preferably, if (b) is not present, the one or more oligomers according to (a) have two ethylenically unsaturated groups.
[0028] Thus, the radiation curable composition for coating an optical fiber according to the first aspect of the present invention may contain an oligomer (a), a second oligomer (b), a reactive diluent component (c), a photoinitiator component (d) and an additive component (e). Such components described below may be used in a composition or formulation according to any aspect of the present invention, including an optical fiber primary coating composition according to the first aspect, a primary coating composition used in a method for coating an optical fiber according to the second aspect, and a composition applied to and cured on an optical fiber as described in relation to the third aspect.
[0029] It has surprisingly been found that oligomers (a) tend to have lower viscosity values. It has surprisingly been found that the presence of such oligomers in an optical fiber primary coating composition can advantageously contribute to the ability to reduce the volatile content of the optical fiber primary coating composition while still being suitable for optical fiber coating application, particularly maintaining acceptable viscosity and cure speed and on-fiber performance, as desired by the industry.
[0030] Oligomer components
[0031] The radiation curable composition according to the present invention comprises an oligomer component; that is, a collection of one or more individual oligomers having one or more specific structures or types. As used herein, an oligomer refers to a molecule of medium relative molecular mass, the structure of which comprises a plurality of units that are actually or conceptually derived from molecules of lower relative molecular mass. As used herein, a component is considered an oligomer if it also has a number average molecular weight (Mn) greater than about 1 kilodalton (kDa), preferably measured by size exclusion chromatography (SEC) as described elsewhere herein. It will be appreciated by those skilled in the art that oligomers having Mn values within this range are generally less volatile than their low molecular weight analogs and are therefore - advantageously - less likely to migrate from the primary coating composition to the glass tube surrounding the optical fiber during the drawing process.
[0032] In one embodiment, the oligomer component comprises, consists of, or consists essentially of one or more oligomers having an Mn of at least 1 kiloDalton (kDa), or at least 2 kDa, or at least 3 kDa, or at least 5 kDa, or at least 10 kDa, or at least 20 kDa, or at least 30 kDa, or at least 40 kDa, or from 20 to 150 kDa, or from 20 to 130 kDa, or from 20 to 100 kDa, or from 30 to 80 kDa, or from 35 to 55 kDa. According to other embodiments, the oligomer component comprises, consists of, or consists essentially of one or more oligomers having a theoretical molecular weight (Mn,theo) of at least 1 kDa, or at least 5 kDa, or at least 10 kilodaltons (kDa), more preferably greater than 12 kDa, more preferably greater than 15 kDa, more preferably greater than 17 kDa, and / or less than 150 kDa, more preferably less than 140 kDa, more preferably less than 130 kDa, more preferably less than 120 kDa, or from 1 to 100 kDa, or from 1 to 50 kDa, or from 1 to 25 kDa, or from 15 to 120 kDa, or from 20 to 120 kDa, or from 25 to 120 kDa, or from 25 to 110 kDa, or from 25 to 100 kDa.
[0033] The oligomer component should include one or more reactive oligomers. "Reactivity" used herein refers to the ability to form a chemical reaction (preferably a polymerization reaction) with another molecule. Therefore, reactive compounds will be considered to have at least one reactive group or functional group. Preferably, this reactive group or functional group is a polymerizable group. Although some non-reactive oligomers can be used in certain embodiments of the present invention, the reactive oligomers of a large percentage are preferred. In one embodiment, the oligomer component is composed of reactive oligomers or is substantially composed of reactive oligomers.
[0034] In other embodiments, the reactive oligomer is telechelic. As used herein, "telechelic" means that such components (ie, oligomers in this case) contain reactive end groups at each chain end that are capable of forming intramolecular as well as intermolecular bonds.
[0035] Reactive oligomer components according to the present invention preferably comprise reactive oligomers with at least one polymerizable group, are substantially composed of reactive oligomers with at least one polymerizable group, or are composed of reactive oligomers with at least one polymerizable group. In a preferred embodiment, reactive oligomer components are composed of reactive oligomers with at least one polymerizable group. Polymerizable groups can be any known type. However, in one embodiment, polymerizable groups can comprise acrylate or methacrylate groups or any combination thereof, are substantially composed of acrylate or methacrylate groups or any combination thereof, or are composed of acrylate or methacrylate groups or any combination thereof. Reactive oligomers are preferably ethylenically unsaturated polymerizable compounds containing one or more than one reactive ethylenic double bonds.
[0036] Polymerizable groups can occur at any feasible point along the length of reactive oligomers, including such as polymerizable main chain groups or polymerizable end groups.Polymerizable main chain groups exist along the straight chain of the oligomer length or come from the straight chain branch, and polymerizable end groups are polymerizable groups present at the end of the oligomer.Polymerizable groups can be isolated from other polymerizable groups, or exist directly or indirectly adjacently, for example, exist with branching or bifurcated patterns at the end of the oligomer (synonymous herein as "termination point") .In a preferred embodiment, polymerizable groups include polymerizable end groups, are substantially composed of polymerizable end groups, or are composed of polymerizable end groups.
[0037] Reactive oligomers according to the present invention can have any known type consistent with the limitations specified elsewhere herein. However, according to a first aspect, the oligomer component preferably includes, consists of or is substantially composed of one or more carbamate oligomers, preferably reactive carbamate oligomers. The carbamate oligomer includes at least one carbamate group or part, and preferably at least includes a main chain, a polymerizable group, and a carbamate group that connects the main chain to the polymerizable group. In various embodiments, the reactive oligomer contains 0-5 carbamate groups, or 4 or more carbamate groups. According to certain embodiments, the carbamate oligomer includes (i) a hydroxyl or thiol-functional main chain compound (e.g., a polyol); (ii) an isocyanate compound (preferably a polyisocyanate); and (iii) the reaction product of an isocyanate-reactive hydroxyl-functional end-capping agent (preferably also having a (meth) acrylate moiety). In a preferred embodiment, the urethane oligomer has an Mn of 1000 g / mol to 10,000 g / mol, or 1200 g / mol to 9,000 g / mol.
[0038] Examples of suitable hydroxyl or thiol functional main chain compounds include polyether polyols, polyester polyols, polycarbonate polyols, polycaprolactone polyols, acrylic polyols and other polyols. These polyols can be used alone or in combination of two or more. In a preferred embodiment, the main chain of the urethane oligomer includes the reaction product of polyether polyols. In one embodiment, the main chain includes the reaction product of polypropylene glycol (PPG). As used herein, compounds derived from polypropylene glycol include end-capped PPG, such as EO-end-capped PPG. There is no particular limitation on the polymerization mode of the structural units in these polyols. Any of random polymerization, block polymerization, or graft polymerization is acceptable.
[0039] As used herein, block copolymer refers to a part of an oligomer or polymer, comprising many structural units, wherein at least one structural unit comprises a feature not present in an adjacent part. As used herein, single block, diblock and triblock copolymers refer to the average amount of a specific block present in an oligomer. In a preferred embodiment, a specific block refers to a polyether block, which is derived from one or more polyols described elsewhere herein, preferably a polyether polyol. In one embodiment, the block referred to by a single block, diblock and / or triblock copolymer is a polyether block derived from one or more polyols described elsewhere herein. In one embodiment, a single block copolymer can be described as a copolymer having only an average of about 1 or about 0.9 to less than 1.5 specific block (e.g., polyether block) units. In one embodiment, a diblock copolymer can be described as a copolymer having an average of about 2, or at least 1.5 to less than 2.5 specific block (e.g., polyether block) units. In one embodiment, the triblock copolymer can be described as a copolymer having an average of about 3, or at least 2.5 to less than 3.5, units of a particular block (e.g., polyether block). The number of polyether units in a given oligomer can be determined by the number of polyether polyol molecules used in synthesizing a single oligomer.
[0040] As examples of polyether polyols, polyethylene glycol, polypropylene glycol, polypropylene glycol-ethylene glycol copolymers, polytetramethylene glycol, polyhexamethylene glycol, polyheptamethylene glycol, polydecamethylene glycol, and polyether glycols obtained by ring-opening copolymerization of two or more ion-polymerizable cyclic compounds are given. Here, as examples of ion-polymerizable cyclic compounds, cyclic ethers such as ethylene oxide, isobutylene oxide, tetrahydrofuran, 2-methyltetrahydrofuran, 3-methyltetrahydrofuran, dioxane, trioxane, tetraoxane, cyclohexene oxide, styrene oxide, epichlorohydrin, isoprene monoxide, vinyloxetane, vinyltetrahydrofuran, vinylcyclohexene oxide, phenyl glycidyl ether, butyl glycidyl ether, and glycidyl benzoate are given. Specific examples of the combination of two or more ionically polymerizable cyclic compounds include: combinations for producing binary copolymers such as tetrahydrofuran and 2-methyltetrahydrofuran, tetrahydrofuran and 3-methyltetrahydrofuran, and tetrahydrofuran and ethylene oxide; and combinations for producing terpolymers such as combinations of tetrahydrofuran, 2-methyltetrahydrofuran and ethylene oxide, combinations of tetrahydrofuran, butene-1-oxide and ethylene oxide, etc. The ring-opening copolymers of these ionically polymerizable cyclic compounds may be random copolymers or block copolymers.
[0041] These polyether polyols include commercially available products such as PTMG1000, PTMG2000 (produced by Mitsubishi Chemical Corp.), PEG#1000 (produced by Nippon Oil and Fats Co., Ltd.), PTG650(SN), PTG1000(SN), PTG2000(SN), PTG3000, PTGL1000 and PTGL2000 (produced by Hodogaya Chemical Co., Ltd.), PEG400, PEG600, PEG1000, PEG1500, PEG2000, PEG4000 and PEG6000 (produced by Daiichi Kogyo Seiyaku Co., Ltd.), P710R, P1010, P2010 and 1044 P series (produced by BASF), and The series includes PPG725, PPG1000, PPG2000, PPG3000, PPG4000 and PPG8000, as well as The series includes PO / EO polyether diols with Mw of 2800 or 40000 (produced by Covestro). In addition, AGC Chemicals also offers diols such as Preminol S 4013F (Mw 12,000), Preminol 4318F (Mw 18,000) and Preminol 5001F (Mw 4,000).
[0042] Polyester diols obtained by reacting polyols with polyacids are examples of polyester polyols. Examples of polyols include ethylene glycol, polyethylene glycol, tetramethylene glycol, polytetramethylene glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, etc. Examples of polyacids include phthalic acid, dimer acid, isophthalic acid, terephthalic acid, maleic acid, fumaric acid, adipic acid, sebacic acid, etc.
[0043] These polyester polyol compounds can be sold under trade names such as MPD / IPA500, MPD / IPA1000, MPD / IPA2000, MPD / TPA500, MPD / TPA1000, MPD / TPA2000, A-1010, A-2010, PNA-2000, PNOA-1010, and PNOA-2010 (produced by Kuraray Co., Ltd.) were purchased.
[0044] Triols, such as polyester triols or polyether triols are also known. It is particularly preferred to use oligomeric triols herein, which have the general formula: A(-----OH)3; wherein A is a chemical organic structure, such as an aliphatic, cycloaliphatic, aromatic or heterocyclic structure, "-----" is an oligomeric chain, such as a polyether chain, a polyester chain, a polyhydrocarbon chain or a polysiloxane chain, and "OH" is a terminal hydroxyl group. In one embodiment, the triol comprises, consists of or consists essentially of a polyether triol, a PO homopolymer, a PE homopolymer, a PO-EO block copolymer, a random copolymer or a mixed block-random copolymer. In practice, the polyether triol can be based on glycerol or trimethylolpropane, PO, EO or a PO and EO copolymer (wherein EO is located in a terminal block or an inner block), and has a MW of 500 to 15,000 Daltons. Another class of polyether triols are copolymers based on glycerol or trimethylolpropane, such as THF-PO, THF-EO, THF-PO-EO or THF-EO-PO, and have a molecular weight of about 500 to 15,000 g / mol. In one embodiment, the triols are derived from bio-based or natural reactants, such as certain vegetable oils and fats.
[0045] Commercial examples of suitable triols include Related propylene oxide based polyether triols are available from Carpenter under the GP designation, such as GP-1000, GP-1500, GP-1500-60, GP-3000, GP-4000, GP-5017, GP-5017-60, GP-5171, GP-6015, GP-6015-60, GP-6037-60 and GP-700. Other triols are available from Covestro under the Arcol LHT-240 (molecular weight "Mw" indicated by the manufacturer is about 700 g / mol), Arcol LHT-112 (Mw 1500 g / mol), Arcol LHT LG-56 (Mw 3000 g / mol) and Arcol LHT-42 (Mw 4200 g / mol), Trade names such as Multranol 9199 (Mw 4525 g / mol), Multranol 3900 (Mw 4800 g / mol), Multranol 3901 (Mw 6000 g / mol) and Multranol 9139 (Mw 6000 g / mol), and Acclaim 703 (Mw 700 g / mol), Acclaim 3300N (Mw 3000 g / mol), Acclaim 6300 (Mw 6000 g / mol), and Acclaim 6320 (Mw 6000 g / mol). In addition, AGC Chemicals also offers products under the trade name Triols such as Preminol S 3011 (Mw 10,000 g / mol), Preminol 7001K (Mw 7,000 g / mol) and Preminol 7012 (Mw 10,000 g / mol).
[0046] There is no inherent limitation on the number of RH groups (OH and SH, respectively) present in the hydroxyl or thiol functional backbone compound, although the hydroxyl or thiol functional backbone compound preferably has 4 or fewer RH groups. In a preferred embodiment, (i) comprises a hydroxyl functional backbone compound having at least two hydroxyl groups, or at least three hydroxyl groups, or four hydroxyl groups.
[0047] The theoretical molecular weight derived from the hydroxyl number of these polyols is generally from about 50 g / mol to about 15,000 g / mol, and preferably from about 500 to 12,000 g / mol, or from about 1,000 to about 8,000 g / mol.
[0048] In addition to hydroxy-functional compounds such as polyols, thiol-functional compounds can also be used as (i). Suitable thiol-functional compounds can be prepared from suitable hydroxy-functional compounds by well-known methods.
[0049] In a preferred embodiment, (i) comprises, consists of, or consists essentially of a hydroxyl-functional backbone compound. In one embodiment, the hydroxyl-functional backbone compound comprises a polyether, polyester, polybutadiene, polycarbonate or silicone moiety.
[0050] The reactive urethane oligomer also preferably includes (ii) the reaction product of a (poly)isocyanate compound. The reaction product of a (poly)isocyanate compound (preferably a diisocyanate compound) can be utilized to generate the urethane groups or parts in the reactive urethane oligomer according to the first aspect of the present invention. The isocyanate compound used herein is defined as any organic compound having at least one isocyanate group per molecule. Examples of suitable isocyanates include diisocyanates such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, (hydrogenated) xylene diisocyanate, 1,3-xylene diisocyanate, 1,4-xylene diisocyanate, 1,5-naphthalene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 3,3′-dimethyl-4,4′-diphenylmethane diisocyanate, 4,4′-diphenylmethane diisocyanate, 3,3′-dimethylphenylene diisocyanate, 4,4′-biphenyl diisocyanate, 1,6-hexane diisocyanate, isophorone diisocyanate, methylenebis(4-cyclohexylene)diisocyanate, diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, hexamethylene diisocyanate, 2,4- and / or 4,4'-methylene dicyclohexyl diisocyanate, diphenylmethane diisocyanate, tetramethylxylene diisocyanate, 1,5-pentane diisocyanate, bis(2-isocyanato-ethyl)fumarate, 6-isopropyl-1,3-phenyl diisocyanate, 4-diphenylpropane diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylene diisocyanate, tetramethylxylene diisocyanate, lysine isocyanate, and the like.
[0051] These diisocyanate compounds may be used alone or in combination of two or more. Preferred diisocyanates are isophorone diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate and hexamethylene diisocyanate, 2,4-toluene diisocyanate and 2,6-toluene diisocyanate.
[0052] As used herein, "polyisocyanate" means an isocyanate compound having two or more isocyanate moieties per molecule. In one embodiment, the oligomer component comprises, consists essentially of, or consists of a urethane oligomer that is a reaction product of one or more polyisocyanates. In addition to the diisocyanates noted above, polyisocyanates having three isocyanate groups per molecule, i.e., triisocyanates, may also be used. Known triisocyanates include biuret made from hexamethylene diisocyanate (HDI) or HDI trimer, which is available from Covestro under the trade name Commercially available, and include, but are not limited to, Desmodur N 3200, Desmodur N 3300, Desmodur N 3390, Desmodur N 3600, Desmodur N 3800, Desmodur N 3900, Desmodur NXP 2580, Desmodur XP 2599, Desmodur XP 2675, Desmodur XP 2731, Desmodur XP 2714, and Desmodur XP 2803.
[0053] Other commercially available triisocyanates include those available from Evonik for use in 2k systems. Polyisocyanate crosslinkers of the T (IPDI trimer) and HT (HDI trimer) series.
[0054] Reactive carbamate oligomers also preferably include the reaction product of (iii) a hydroxyl functional end-capping agent. According to the compound (iii), preferably, it has reactivity with the isocyanate compound from (ii). Preferably, the carbamate oligomer also includes the reaction product of an isocyanate reactive compound with an ethylenically unsaturated portion as (iii). Preferably, the ethylenically unsaturated portion is a (meth) acrylate portion. Any suitable (meth) acrylate can be used, including monomers and oligomers, although (meth) acrylate monomers are preferred. Such isocyanate reactive (meth) acrylates preferably include hydroxyl-containing (meth) acrylate compounds, because it is known that such compounds have reactivity with isocyanates (including polyisocyanates of (ii)). Examples of hydroxyl-containing (meth)acrylates include (meth)acrylates derived from (meth)acrylic acid and epoxides and (meth)acrylates containing alkylene oxides, more specifically, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and hydroxyethyl caprolactone acrylate, ethoxylated trimethylolpropane diacrylate, glycerol di(meth)acrylate, and glycerol acrylate methacrylate (i.e., 3-(acryloyloxy)-2-hydroxypropyl methacrylate). In a preferred embodiment, (iii) includes, consists essentially of, or consists of hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, caprolactone (meth)acrylate, glycerol acrylate methacrylate, glycerol di(meth)acrylate, or a combination thereof.
[0055] The hydroxy functional capping agent (iii) preferably further comprises one or two ethylenically unsaturated moieties, more preferably the hydroxy functional capping agent (iii) further comprises one ethylenically unsaturated moiety.The compound according to (iii) may have more than one hydroxyl group per molecule.
[0056] In the reaction of the components for generating the urethane oligomers, it is also preferred to use one or more urethanization catalysts. Such catalysts include, by way of example, copper naphthenate, cobalt naphthenate, zinc naphthenate, bismuth, di-n-butyltin dilaurate, triethylamine and triethylenediamine-2-methyltriethyleneamine. The catalyst can be used in any suitable amount, or for example, about 0.01 to about 1 weight percent of the total amount of reactants. The reaction can be carried out at any suitable temperature, for example, a temperature of about 10 to about 90° C., and preferably about 30 to about 80° C.
[0057] In one embodiment, the composition or formulation comprises at least one oligomer further comprising the reaction product of a single PPG diol as (i), a single diisocyanate compound as (ii), and a hydroxy-functional (meth)acrylate compound as (iii).
[0058] The oligomer (a) reactants (i), (ii) and (iii) are selected and configured in a specified ratio. The composition comprises at least one oligomer (a), wherein the molar ratio of the number of isocyanate groups in (ii) to the number of hydroxyl and thiol groups in (i) is less than or equal to 1.0. One or more oligomers (a) are the reaction products of (iii) a hydroxyl functional end-capping agent further comprising an ethylenically unsaturated portion, (ii) an isocyanate compound and (i) a hydroxyl or thiol functional main chain compound, and the molar amount of isocyanate groups in (ii) is less than or equal to the molar amount of hydroxyl and thiol groups in (i). Therefore, since the oligomer according to (a) is the reaction product of all three components (iii), (ii) and (i), one or more oligomers (a) are hydroxyl or thiol functional. In one embodiment, the composition comprises at least one oligomer (a), wherein the molar ratio of the number of isocyanate groups in (ii) to the number of hydroxyl and thiol groups in (i) is greater than or equal to 2:3 and less than or equal to 1.0. Thus, in certain embodiments, the composition has at least one oligomer (a) having the aforementioned molar ratio, preferably about 0.67 to 1.0, or equal to 1.0. Surprisingly, the inventors have found that oligomers configured in this manner (which otherwise meet the requirements and preferences set forth herein) tend to have lower viscosity values. This is helpful because the use of such oligomers tends to minimize the need for large amounts of volatile diluents, which can be included in larger amounts in the overall composition.
[0059] Thus, in one embodiment, the composition or formulation comprises at least one oligomer having a viscosity of less than 15 Pa·s, or less than 12, or less than 10 Pa·s, or between 1 and 15 Pa·s, or between 2 and 12 Pa·s, or between 3 and 10 Pa·s, wherein the viscosity is between 25°C and 2500s -1 Measured at a shear rate of .
[0060] The various oligomers of the first aspect can be configured to have a wide range of functionality. In one embodiment, at least one monofunctional oligomer is utilized. "Monofunctional" as used herein refers to having an average of 0.5 to 1.4 polymerizable groups per molecule, for example as determined by nuclear magnetic resonance spectroscopy (NMR) methods.
[0061] In one embodiment, difunctional oligomers and / or trifunctional oligomers can be used additionally or alternatively. "Difunctional" as used herein refers to that each molecule has an average of 1.95 to 2.05 polymerizable groups, for example as measured by NMR methods. Similarly, "trifunctional" as used herein refers to that each molecule has an average of 2.95 to 3.05 polymerizable groups. In a preferred embodiment, the oligomer component includes, is essentially composed of, or is composed of one or more reactive urethane oligomers having an average (meth) acrylate functionality of 1.5 to 4.2, or 1.8 to 3.8, or 1.8 to 3.2, or 1.8 to 2.8. In one embodiment, the average (meth) acrylate functionality of the oligomer component is 1.5 to 4.2, or 1.8 to 3.8, or 1.8 to 3.2, or 1.8 to 2.8.
[0062] In a preferred embodiment, the composition or formulation comprises at least one difunctional or higher functional oligomer to promote sufficient crosslinking for use as a primary coating for optical fiber. In further embodiments, the composition or formulation contains a mixture of different oligomers with different functionalities, such as at least one monofunctional oligomer and at least one difunctional oligomer, or at least one monofunctional oligomer and at least one trifunctional oligomer, or at least one monofunctional oligomer, at least one difunctional oligomer and at least one trifunctional oligomer. Of course, other combinations can be envisioned by those skilled in the art of application of the present invention.
[0063] According to many embodiments of the first aspect, the composition or formulation contains more than one oligomer. In embodiments of the first aspect, the optical fiber primary coating composition comprises (a) one or more oligomers, the oligomers being the reaction product of (i) a hydroxyl or thiol functional backbone compound, (ii) an isocyanate compound, and (iii) a hydroxyl functional capping agent, the capping agent further comprising an ethylenically unsaturated moiety, wherein the molar ratio of (ii) to (i) is less than or equal to 1.0 (as described above), and further optionally comprises (b), one or more urethane (meth) acrylate oligomers other than the urethane (meth) acrylate oligomers mentioned in (a). In various embodiments of the first aspect, the one or more oligomers according to (a) are present in a large amount, such as greater than or equal to 20 wt%, or greater than or equal to 30 wt%, or greater than or equal to 40 wt%, and less than or equal to 95 wt%, or less than or equal to 90 wt%, or less than or equal to 80 wt%, or less than or equal to 70 wt%, relative to the entire relevant composition. If the optical fiber primary coating composition does not contain oligomer (b), and one or more oligomers (a) present in the optical fiber primary coating composition are monofunctional with respect to polymerizable groups, then those skilled in the art will understand that one or more reactive diluent monomers (c) need to be present, and at least a portion of (c) needs to be at least difunctional with respect to polymerizable groups, in order for the optical fiber primary coating composition to form a network. If the optical fiber primary coating composition does not contain oligomer (b) and does not contain reactive diluent monomer (c), or one or more reactive diluent monomers (c) are monofunctional with respect to polymerizable groups, then those skilled in the art will understand that at least a portion of one or more oligomers (a) needs to be at least difunctional with respect to polymerizable groups, in order for the optical fiber primary coating composition to form a network.
[0064] Since it is incorporated into the overall composition in such high amounts, the one or more oligomers (a) are preferably configured to have a sufficiently low viscosity to enable adequate processing in optical fiber coating applications. As described above, the aforementioned molar ratio of (ii) to (i) can contribute favorably to this property of the oligomer (a). Alternatively or additionally, the total number of carbamate bonds present in the one or more oligomers (a) can also contribute favorably thereto. Thus, in one embodiment, the oligomer according to (a) has from 1.8 to 2.2 carbamate bonds per molecule. Third, the inventors surprisingly discovered that by configuring the oligomer so that one end thereof is terminated with a hydroxyl group or a thiol group, an oligomer having a sufficiently low viscosity can be obtained.
[0065] In other embodiments of the first aspect, oligomer (b) is preferably present in an amount of 29.95 wt % or less relative to the entire relevant composition. Oligomer (b) may also include the reaction product of (i) a hydroxyl-functional backbone compound, (ii) an isocyanate compound, and (iii) a hydroxyl-functional end-capping agent. However, in contrast to oligomer (a), according to certain embodiments, oligomer (b) has a molar ratio of the number of isocyanate groups in (ii) to the number of hydroxyl groups in (i) of the urethane (meth) acrylate oligomer (b) of greater than 1.0, or from about 1.5 to about 2.0.
[0066] According to embodiments of the first aspect, the concentration of acrylate groups in the optical fiber primary coating composition and / or the concentration of carbamate groups in the optical fiber primary coating composition and / or the concentration of acrylate groups in the oligomer present in the optical fiber primary coating composition can advantageously contribute to the ability to reduce the volatile content of the optical fiber primary coating composition while still being suitable for optical fiber coating applications, particularly maintaining acceptable viscosity and cure speed and on-fiber performance as desired by the industry, particularly in terms of cure speed (measured by low T30%, modulus maximum, especially those below 1.2 seconds, more preferably below 1.0 seconds), low modulus (measured by low G' value, especially those below 600 kPa, more preferably below 500 kPa, more preferably below 400 kPa, more preferably below 300 kPa) and / or low viscosity (especially those below 9 Pascal seconds, more preferably below 5 Pascal seconds). The concentration of acrylate groups is preferably less than or equal to 2.50 mol / kg, more preferably less than or equal to 2.00 mol / kg, more preferably less than or equal to 1.50 mol / kg, more preferably less than or equal to 1.20 mol / kg, more preferably less than or equal to 1.00 mol / kg, more preferably less than or equal to 0.80 mol / kg, relative to the entire relevant composition. The concentration of urethane groups is preferably greater than or equal to 0.20 mol / kg, or greater than or equal to 0.25 mol / kg, or greater than or equal to 0.30 mol / kg, or greater than or equal to 0.31 mol / kg, or greater than or equal to 0.35 mol / kg, or greater than or equal to 0.40 mol / kg, or greater than or equal to 0.45 mol / kg, or greater than or equal to 0.50 mol / kg, and preferably lower than 1.5 mol / kg, or less than or equal to 0.90 mol / kg, preferably less than or equal to 0.70 mol / kg, relative to the entire relevant composition. As used herein, the concentration of acrylate groups and the concentration of urethane groups are determined by calculation from the feed ratio of each component. The total concentration of acrylate groups present in oligomers (a) and (b) is preferably greater than or equal to 0.05 mol / kg oligomers (a) + (b) and less than or equal to 0.80 mol / kg oligomers (a) + (b), or less than or equal to 0.70 mol / kg oligomers (a) + (b), or less than or equal to 0.60 mol / kg oligomers (a) + (b), or less than or equal to 0.50 mol / kg oligomers (a) + (b), or less than or equal to 0.40 mol / kg oligomers (a) + (b), or less than or equal to 0.30 mol / kg oligomers (a) + (b), or less than or equal to 0.28 mol / kg oligomers (a) + (b).
[0067] Whether or not included in the first aspect, it is preferred that the total oligomer content (whether (a) alone or (b) if present) is very high relative to the weight of the entire composition associated with such oligomer or oligomers. In one embodiment, the oligomers are present in an amount of at least 70 wt%, or at least 80 wt%, or at least 90 wt%, or at least 95 wt%, or at least 98 wt%, relative to the weight of the entire composition. Preferably, the oligomers according to (a) and (b) are present in an amount greater than or equal to 80 wt%, and less than or equal to 96 wt%, relative to the weight of the entire composition.
[0068] Reactive diluent component (c)
[0069] The composition according to the first aspect of the invention also includes a diluent component (c); that is, a collection of one or more individual diluents having one or more specific structures or types. As used herein, "diluent" refers to a substance that reduces the viscosity of a larger composition to which it is added or associated. Various diluents can be used to maximize the fluidity, and thus the processability, of the optical fiber coating composition to which it is associated.
[0070] In order to maximize the curability of the composition associated therewith, the diluent component preferably comprises, is composed of, or is substantially composed of a reactive diluent. As described elsewhere herein with respect to the definition of the oligomer component, "reactivity" refers to the ability to form a chemical reaction, preferably a polymerization reaction, with another molecule. Therefore, a reactive compound is considered to have at least one reactive or functional group. Preferably, this reactive or functional group is a polymerizable group.
[0071] It is further preferred that the diluent component includes reactive diluent monomers, is composed of reactive diluent monomers, or is substantially composed of reactive diluent monomers. A monomer is a molecule of low relative molecular mass, the structure of which can be polymerized to provide constitutional units for the basic structure of a macromolecule. As used herein, if a certain component also has a number average molecular weight (Mn) less than about 1000 g / mol, the component is considered to be a monomer. In one embodiment, the reactive diluent component is composed of one or more reactive diluent monomers, and the monomer has an Mn of about 86 g / mol (molar mass of methacrylate) to 750 g / mol, or 100 g / mol to 350 g / mol, as determined by an NMR method. In various embodiments, the reactive diluent has an Mn of less than 500 g / mol.
[0072] The diluent component according to the invention comprises, consists essentially of or consists of a reactive diluent monomer having at least one polymerizable group. In a preferred embodiment, the reactive diluent monomer component consists of reactive diluent monomers having on average one polymerizable group. The polymerizable group(s) of the reactive diluent monomers are preferably capable of (co)polymerization with the polymerizable groups present in the associated reactive oligomer component.
[0073] The polymerizable group of the reactive diluent may be of any known type. However, in one embodiment, the polymerizable group may include, consist essentially of, or consist of an acrylate, acrylamide, or N-vinylamide group, or any combination thereof. The reactive diluent is preferably an ethylenically unsaturated polymerizable compound containing at least one reactive olefin double bond.
[0074] The polymerizable group(s) may occur at any practicable point along the length of the reactive diluent. However, in a preferred embodiment, the polymerizable group comprises, consists essentially of, or consists of a polymerizable terminal group.
[0075] The diluent component according to the present invention may include any known type of compound or material consistent with the definitions specified elsewhere herein. However, in a preferred embodiment, the diluent component comprises, consists essentially of, or consists of one or more reactive diluent monomers containing one double bond.
[0076] Typical examples of such reactive diluent monomers containing one double bond are alkyl or hydroxyalkyl acrylates, such as methyl, ethyl, butyl, 2-phenoxyethyl, 2-ethylhexyl and 2-hydroxyethyl acrylates, isobornyl acrylate, methyl and ethyl acrylates, lauryl acrylate, ethoxylated nonylphenol acrylate and diethylene glycol-ethylhexyl acrylate (DEGEHA). Other examples of these monomers are acrylonitrile, acrylamide, N-substituted acrylamides, vinyl esters such as vinyl acetate, styrene, alkyl styrenes, halogenated styrenes, N-vinyl pyrrolidone, N-vinyl amides such as N-vinyl caprolactam, vinyl chloride and vinylidene chloride. Examples of monomers containing more than one double bond are ethylene glycol diacrylate, propylene glycol diacrylate, tripropylene glycol diacrylate, neopentyl glycol diacrylate, hexanediol diacrylate, bisphenol A diacrylate, 4,4'-bis(2-acryloxyethoxy)diphenylpropane, trimethylolpropane triacrylate, pentaerythritol tri- and tetraacrylate and vinyl acrylate.
[0077] In a preferred embodiment, if used, component (c) includes 2-ethylhexyl acrylate, 2-phenoxyethyl acrylate, 2-(2-ethoxyethoxy)ethyl acrylate, n-vinyl pyrrolidone, dimethyl acrylamide, n-vinyl caprolactam, ethoxylated 2-phenoxyethyl acrylate, 4-hydroxybutyl acrylate, lauryl acrylate, isobornyl acrylate, caprolactone acrylate, ethoxylated nonylphenol acrylate, tridecyl acrylate, or isodecyl acrylate, or a combination thereof.
[0078] In a preferred embodiment, the diluent component comprises, consists essentially of, or consists of one or more monofunctional diluent monomers. In a preferred embodiment, the diluent component comprises, consists of, or consists essentially of functional monomers (e.g., (meth)acrylic monomers).
[0079] One or more of the above-mentioned diluents may be used in any suitable amount in the composition according to the present invention to adjust the viscosity of the formulation associated therewith to be suitable for the optical fiber coating process used therewith according to methods well known in the field of application of the present invention, and may be selected alone or in combination with one or more of the types listed herein.
[0080] However, in various preferred embodiments, it is desirable to minimize the amount of low molecular weight components present in the composition or formulation. This is because such components are inherently more volatile than their higher molecular weight oligomeric analogs and are more likely to evaporate or separate from the liquid composition during application. This problem is particularly acute when the composition is exposed to and maintained at elevated temperatures, such as experienced during its high speed application and processing onto optical fiber. During the optical fiber curing process, the evaporation of volatiles is extremely undesirable because these volatile components can then condense or coalesce on the inner surface of the conduit in which the optical fiber coating process is performed. As more and more components are deposited on the conduit surface, they will inevitably inhibit the ability of the radiation source to effectively cure the optical fiber coating composition because they will block a portion of the light from reaching there. In addition, these volatiles can also clog the inner surface of the conduit, thereby requiring more frequent inconvenient and process-stopping cleaning operations. The inventors have surprisingly discovered that by constructing a composition or formulation of the type described herein, for example by including the above-described oligomers (a) and (b), the amount of reactive diluent present in the composition can be reduced while still maintaining adequate cure speed, processability, and on-fiber performance.
[0081] Thus, in a preferred embodiment, component (c) is present in an amount of less than 30 wt %, or 29.95 wt % or less, or less than 20 wt %, or less than 10 wt %, or less than 5 wt %, or less than 2 wt % relative to the total weight of the composition or formulation with which it is associated. In yet other preferred embodiments, component (c) is not present at all in the composition or formulation.
[0082] Photoinitiator component (d)
[0083] According to a first aspect, the composition and / or formulation preferably includes a photoinitiator component; that is, a collection of one or more individual photoinitiators having one or more specific structures or types. A photoinitiator is a compound that undergoes a chemical change to produce at least one of free radicals, acids and bases due to the action of light or the synergistic effect between the action of light and the electronic excitation of a sensitizing dye. Well-known types of photoinitiators include cationic photoinitiators and free radical photoinitiators. According to one embodiment of the present invention, the photoinitiator is a free radical photoinitiator.
[0084] In one embodiment, the photoinitiator component includes, consists of, or consists essentially of one or more acylphosphine oxide photoinitiators. Acylphosphine oxide photoinitiators are known and disclosed, for example, in U.S. Patent Nos. 4,324,744, 4,737,593, 5,942,290, 5,534,559, 6,020,529, 6,486,228, and 6,486,226. Preferred types of acylphosphine oxide photoinitiators used in the photoinitiator component include bisacylphosphine oxide (BAPO) or monoacylphosphine oxide (MAPO). More specifically, examples include 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide (CAS#84434-11-7) or 2,4,6-trimethylbenzoyldiphenylphosphine oxide (CAS#127090-72-6).
[0085] The photoinitiator component may also optionally include, consist of, or consist essentially of an α-hydroxyketone photoinitiator. For example, suitable α-hydroxyketone photoinitiators are α-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 2-hydroxy-2-methyl-1-(4-isopropylphenyl)propanone, 2-hydroxy-2-methyl-1-(4-dodecylphenyl)propanone, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propan-1-one, and 2-hydroxy-2-methyl-1-[(2-hydroxyethoxy)phenyl]propanone.
[0086] In another embodiment, the photoinitiator component comprises, consists of, or consists essentially of: an α-aminoketone, such as 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone, 2-benzyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-(4-methylbenzyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-1-butanone, or 2-benzyl-2-(dimethylamino)-1-[3,4-dimethoxyphenyl]-1-butanone; a benzophenone, such as benzophenone, 2,4,6-trimethylbenzophenone, 4-methylbenzophenone, 2-methylbenzophenone, 2-methoxycarbonylbenzophenone, 4,4'-bis(chloromethyl)-benzophenone, 4-chlorobenzophenone, 4-phenylbenzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, methyl 2-benzoylbenzoate, 3,3'-dimethyl-4-methoxybenzophenone, 4-(4-methylphenylthio)benzophenone, 2,4,6-trimethyl-4'-phenylbenzophenone or 3-methyl-4'-phenylbenzophenone; ketal compounds such as 2,2-dimethoxy-1,2-diphenylethanone; and monomeric or dimeric phenylglyoxylates such as methylphenylglyoxylate, 5,5'-oxy-bis(ethyleneoxydicarbonylphenyl) or 1,2-(benzoylcarboxy)ethane.
[0087] Further suitable photoinitiators for use in the photoinitiator component also include oxime esters, such as those disclosed in US Pat. No. 6,596,445. Another class of photoinitiators suitable for use in the photoinitiator component also includes, for example, phenylglyoxylic acid esters, such as those disclosed in US Pat. No. 6,048,660.
[0088] In another embodiment, the photoinitiator component may include, consist of, or essentially consist of one or more alkyl, aryl or acyl substituted compounds not mentioned above in this document.
[0089] According to another embodiment, the composition may contain a photoinitiator which is an alkyl, aryl or acyl substituted compound. In one embodiment, the alkyl, aryl or acyl substituted photoinitiator has an atom from the carbon (Group 14) group or is centered on an atom from the carbon (Group 14) group. In this case, the Group 14 atom present in the photoinitiator compound forms a free radical under excitation (by absorbing radiation). Thus, such a compound may produce a free radical having an atom selected from silicon, germanium, tin or lead or centered on an atom selected from silicon, germanium, tin or lead. In one embodiment, the alkyl, aryl or acyl substituted photoinitiator is an acylgermanium compound. Such photoinitiators are described in US9708442 assigned to Covestro (Netherlands) BV, which is incorporated herein by reference in its entirety. Known specific acylgermanium photoinitiators include benzoyltrimethylgermanium (BTG), tetraacylgermanium or diacylgermanyl (which can be used as Commercially available from Ivoclar Vivadent AG, 9494 Schaan / Liechtenstein).
[0090] The photoinitiator according to the present invention can be used alone or in combination as a blend. Suitable photoinitiator blends are disclosed, for example, in U.S. Patent No. 6,020,528 and U.S. Patent Application No. 60 / 498,848. According to one embodiment, the photoinitiator component includes the following photoinitiator blends, such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (CAS#162881-26-7) and 2,4,6,-trimethylbenzoylethoxyphenylphosphine oxide (CAS#84434-11-7), in a weight ratio of about 1:11, 1:10, 1:9, 1:8 or 1:7.
[0091] Another particularly suitable photoinitiator blend is a mixture of bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide and 2-hydroxy-2-methyl-1-phenyl-1-propanone (CAS#7473-98-5) in a weight ratio of, for example, about 3:1:15 or 3:1:16 or 4:1:15 or 4:1:16. Another suitable photoinitiator blend is a mixture of bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2-hydroxy-2-methyl-1-phenyl-1-propanone in a weight ratio of, for example, about 1:3, 1:4 or 1:5.
[0092] One or more of the foregoing photoinitiators may be used in the photoinitiator component of the composition according to the first aspect of the invention in any suitable amount, and may be selected alone or in combination with one or more of the types listed herein. In a preferred embodiment, the photoinitiator component comprises, consists of, or consists essentially of a free radical photoinitiator. In one embodiment, the photoinitiator component is present in an amount of about 0.1 wt % to about 10 wt %, or about 0.1 wt % to about 5 wt %, or about 1 wt % to about 5 wt %, or 0.04 wt % to 8 wt %, relative to the total weight of the composition.
[0093] Additive (e)
[0094] The compositions and / or formulations according to the first aspect of the invention optionally include an additive component; that is, a collection of one or more individual additives having one or more specific structures or types. Additives are also often added to optical fiber coatings to achieve certain desired properties, such as improved adhesion to glass optical fiber, improved shelf life, improved oxidation and hydrolytic stability of the coating, etc. There are many different types of desirable additives, and the invention discussed herein is not intended to be limited to these, although they are included in the envisioned embodiments because they have the desired effect.
[0095] Examples of additives used in the additive component include thermal inhibitors, which are intended to prevent premature polymerization, examples being hydroquinone, hydroquinone derivatives, p-methoxyphenol, β-naphthol or sterically hindered phenols, such as 2,6-di(tert-butyl)-p-cresol. For example, the storage life in the dark can be increased by using copper compounds (e.g. copper naphthenate, copper stearate or copper octoate), phosphorus compounds (e.g. triphenylphosphine, tributylphosphine, triethyl phosphite, triphenyl phosphite or tribenzyl phosphite), quaternary ammonium compounds (e.g. tetramethylammonium chloride or trimethylbenzylammonium chloride).
[0096] To block atmospheric oxygen during the polymerization process, additives such as paraffin or similar waxy substances can be added; due to their low solubility in the polymer, they migrate to the surface at the start of polymerization and form a transparent surface layer that blocks the ingress of air. Oxygen barrier layers can also be applied.
[0097] Other potentially suitable additives include light stabilizers. Light stabilizers include UV absorbers, such as the well-known commercial UV absorbers of the hydroxyphenylbenzotriazole, hydroxyphenylbenzophenone, oxalamide or hydroxyphenyl-s-triazine type. Such compounds may be used alone or in mixtures, with or without sterically hindered relatively non-basic amine light stabilizers (HALS). Sterically hindered amines are, for example, based on 2,2,6,6-tetramethylpiperidine. UV absorbers and sterically hindered amines include, for example, the following:
[0098] 2-(2-Hydroxyphenyl)-2H-benzotriazole, such as the known commercial hydroxyphenyl-2H-benzotriazole and benzotriazole disclosed in U.S. Pat. Nos. 3,004,896; 3,055,896; 3,072,585; 3,074,910; 3,189,615; 3,218,332; 3,230,194; 4,127,586; 4,226,763; 4,275,004; 4,278,589; 4,315,848 ; 4,347,180; 4,383,863; 4,675,352; 4,681,905; 4,853,471; 5,268,450; 5,278,314; 5,280,124; 5,319,091; 5,410,071; 5,436,349; 5,516,914; 5,554,760; 5,563,242; 5,574,166; 5,607,987; 5,977,219; 6 , 166, 218 and 6,166, 218, such as 2-(2-hydroxy-5-methylphenyl)-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-2H-benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)-2H-benzotriazole, 5-chloro-2-(3,5-di-tert-butyl-2-hydroxyphenyl)-2H-benzotriazole, 5-chloro-2-(3,5-di-tert-butyl-2-hydroxyphenyl)-2H-benzotriazole, -5-methylphenyl)-2H-benzotriazole, 2-(3-sec-butyl-5-tert-butyl-2-hydroxyphenyl)-2H-benzotriazole, 2-(2-hydroxy-4-octyloxyphenyl)-2H-benzotriazole, 2-(3,5-di-tert-amyl-2-hydroxyphenyl)-2H-benzotriazole, 2-(3,5-bis-α-cumyl-2-hydroxyphenyl)-2H-benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-(2-(ω-hydroxy-octa-(ethyleneoxy)carbonyl-ethyl)-,phenyl)-2H-benzotriazole, 2-(3-dodecyl-2-hydroxy-5-methylphenyl)-2H-benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-(2-octyloxycarbonyl)ethylphenyl)-2H-benzotriazole, dodecyl 2-(2-hydroxy-5-methylphenyl)-2H-benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-(2-octyloxycarbonylethyl)phenyl)-5-chloro-2H-benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-(2-octyloxycarbonylethyl)phenyl)-5-chloro-2H-benzotriazole, 2-(3-tert-butyl-5-(2-(2-ethylhexyloxy)-carbonylethyl)-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-(2-methoxycarbonylethyl)phenyl)-5-chloro-2H-benzotriazole, 2- (3-tert-butyl-2-hydroxy-5-(2-methoxycarbonylethyl)phenyl)-2H-benzotriazole, 2-(3-tert-butyl-5-(2-(2-ethylhexyloxy)carbonylethyl)-2-hydroxyphenyl)-2H-benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-(2-isooctyloxycarbonylethyl)phenyl-2H-benzotriazole, 2,2'-methylene-bis(4-tert-octyl-(6-2H-benzotriazol-2-yl)phenol), 2-(2-hydroxy-3-α-cumyl-5-tert-octylphenyl)-2H-benzotriazole, 2-(2-hydroxy-3-tert-octyl-5-α-cumylphenyl)-2H-benzotriazole, 5-fluoro-2-(2-hydroxy-3,5-di-α-cumylphenyl)- 2H-benzotriazole, 5-chloro-2-(2-hydroxy-3,5-di-α-cumylphenyl)-2H-benzotriazole, 5-chloro-2-(2-hydroxy-3-α-cumyl-5-tert-octylphenyl)-2H-benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-(2-isooctyloxycarbonylethyl)phenyl)-5-chloro-2H-benzotriazole, 5-trifluoromethyl-2-(2-hydroxy-3-α-cumyl-5-tert-octylphenyl)-2H-benzotriazole, 5-trifluoromethyl-2-(2-hydroxy-5-tert-octylphenyl)-2H-benzotriazole, 5-trifluoromethyl-2-(2-hydroxy-3,5-di-tert-octylphenyl)-2H-benzotriazole, methyl 3-(5-trifluoromethyl-2H-benzotriazole -2-yl)-5-tert-butyl-4-hydroxyhydrocinnamate, 5-butylsulfonyl-2-(2-hydroxy-3-α-cumyl-5-tert-octylphenyl)-2H-benzotriazole, 5-trifluoromethyl-2-(2-hydroxy-3-α-cumyl-5-tert-butylphenyl)-2H-benzotriazole, 5-trifluoromethyl-2-(2-hydroxy-3,5-di-tert-butylphenyl)-2H-benzotriazole, 5-trifluoromethyl-2-(2-hydroxy-3,5-di-α-cumylphenyl)-2H-benzotriazole, 5-butylsulfonyl-2-(2-hydroxy-3,5-di-tert-butylphenyl)-2H-benzotriazole and 5-phenylsulfonyl-2-(2-hydroxy-3,5-di-tert-butylphenyl)-2H-benzotriazole. ,
[0099] Another exemplary class includes 2-hydroxybenzophenones, such as 4-hydroxy, 4-methoxy, 4-octyloxy, 4-decyloxy, 4-dodecyloxy, 4-benzyloxy, 4,2',4'-trihydroxy, and 2'-hydroxy-4,4'-dimethoxy derivatives.
[0100] Yet another exemplary class includes esters of substituted and unsubstituted benzoic acids, such as 4-tert-butylphenyl salicylate, phenyl salicylate, octylphenyl salicylate, dibenzoylresorcinol, bis(4-tert-butylbenzoyl)resorcinol, benzoylresorcinol, 2,4-di-tert-butylphenyl 3,5-di-tert-butyl-4-hydroxybenzoate, hexadecyl 3,5-di-tert-butyl-4-hydroxybenzoate, octadecyl 3,5-di-tert-butyl-4-hydroxybenzoate, 2-methyl-4,6-di-tert-butylphenyl 3,5-di-tert-butyl-4-hydroxybenzoate.
[0101] Additional additives suitable for use in the additive component include compounds that accelerate photopolymerization, such as so-called photosensitizers, which offset or broaden the spectral sensitivity of the composition incorporated therein. Photosensitizers particularly include aromatic carbonyl compounds, such as benzophenone derivatives, thioxanthone derivatives, anthraquinone derivatives and 3-acylcoumarin derivatives, and 3-(aroylmethylene)thiazolines, and eosin, rhodamine and erythrosine dyes. Alternatively, non-aromatic carbonyl compounds can be used. An example of a non-aromatic carbonyl is dimethoxyanthracene.
[0102] In particular, the curing process can be assisted by using additives that produce or promote the production of colored compositions. Such additives include pigments such as titanium dioxide, and also include additives that form free radicals under thermal conditions, such as azo compounds such as 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), triazenes, diazosulfides, pentazodiene or peroxide compounds, such as hydroperoxides or peroxycarbonates, such as tert-butyl hydroperoxide, as described in U.S. Patent No. 4,753,817. Other suitable substances for this purpose include benzopinacol compounds.
[0103] The additive component may include a photoreducible dye, such as a xanthene, benzoxanthene, benzothioxanthene, thiazine, pyronine, porphyrin or acridine dye, and / or a trihalomethyl compound that can be cleaved by radiation. Such additives are described, for example, in U.S. Pat. No. 5,229,253.
[0104] Depending on the intended application, other conventional additives may be used. Examples include fluorescent brighteners, fillers, pigments, dyes, wetting agents or leveling aids. Thick and pigmented coatings may also contain glass microspheres or glass fiber powder, as described, for example, in U.S. Pat. No. 5,013,768.
[0105] In one embodiment, the additive component includes one or more various additives for enhancing one or more properties of the primary coating. These additives include antioxidants (e.g., Irganox 1035, thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] or tert-butylhydroquinone), adhesion promoters, inhibitors (e.g., acrylic acid), photosensitizers, carrier surfactants, tackifiers, catalysts, stabilizers, surfactants, and fluorescent brighteners.
[0106] In a preferred embodiment, the additive component includes, consists of, or consists essentially of one or more adhesion promoter compounds. The adhesion promoter provides a connection between the polymer primary coating and the glass optical fiber surface. Hydrolyzable silane coupling agents have been used as glass adhesion promoters. Silane coupling agents are described in U.S. Patent No. 4,932,750. In one embodiment, the adhesion promoter is a hydrolyzable silane compound containing a thiol group and / or multiple alkoxy groups. Such adhesion promoters are known and described in U.S. Patent Application No. 20020013383, the relevant parts of which are incorporated herein by reference.
[0107] In one embodiment, the adhesion promoter includes one or more of γ-mercaptopropyltrimethoxysilane, trimethoxysilylpropyl acrylate or 3-trimethoxysilylpropane-1-thiol. Alternatively, the silane coupling group can react with the oligomer in the oligomer component; in this case, they will not be considered as additives, but as part of the oligomer component. Therefore, in one embodiment, the adhesion promoter includes an oligomer adhesion promoter, preferably an adhesion promoter with carbamate and acrylate groups. If used, the oligomer carbamate acrylate adhesion promoter preferably includes at least 2 carbamate groups and is the reaction product of a monofunctional telechelic carbamate acrylate oligomer containing a telechelic hydroxyl group; preferably by reacting with an isocyanate silane adhesion promoter or a diisocyanate with a hydroxyl, mercapto or amino-functional silane.
[0108] One or more of the above-mentioned additives may be used in the composition according to the present invention in any suitable amount, and may be selected alone or in combination with one or more of the types listed herein. In a preferred embodiment, the additive component is present in an amount of about 0% to 20% by weight, or 0% to 10% by weight, or 0% to 5% by weight, 0.01% to 20% by weight, or 0.01% to 10% by weight, or 0.01% to 5% by weight, or 0.1% to 2% by weight, relative to the total weight of the composition. According to another embodiment, the additive component is present in an amount of 1% to 20% by weight, or 1% to 10% by weight, or 1% to 5% by weight, relative to the weight of the entire radiation curable composition.
[0109] As described above, the compositions formulated according to the various embodiments of the first aspect may be configured to have certain desirable properties. Specifically, such compositions and / or formulations, in addition to containing a small amount of volatile diluent, may also be capable of forming a cured product having a sufficiently low modulus value and / or rapid curing. This makes such coatings and / or formulations useful in optical fiber coating applications where resistance to microbending-induced attenuation and high processing speeds are desirable and even required. As used herein, an indicator of microbending-induced attenuation is the storage modulus (G'). It is known that, all other conditions being equal, a primary coating composition with a lower modulus will impart better resistance to microbending-induced attenuation. In addition, as used herein, an indicator of curing speed is the time required for a particular coating or formulation to reach 30% of its final storage modulus value.
[0110] Thus, in various specific further embodiments, the optical fiber primary coating composition according to any embodiment of the first aspect is configured to have a storage modulus (G') of less than 600 kPa, or 1 to 550 kPa, or 10 to 500 kPa, or less than 300 kPa, or 1 to 200 kPa, or 10 to 150 kPa when cured into a film according to the process and dimensions specified elsewhere herein.
[0111] In addition, in various other specific further embodiments, the optical fiber primary coating composition according to any embodiment of the first aspect is configured to have a time to reach a 30% increase in storage modulus of less than 1.2 seconds, or less than 1 second when cured into a film according to the process and dimensions specified elsewhere herein.
[0112] The composition and / or formulation of the first aspect also preferably has a viscosity value suitable for optical fiber applications and curing processes. Therefore, in yet other specific further embodiments, the optical fiber primary coating composition according to any embodiment of the first aspect is configured to have a viscosity of at least> 0.1 Pascal seconds (Pa·s), or at least 0.2, or at least 0.5, or at least 1 Pa·s, and / or less than 15 Pa·s, or less than 12, or less than 10 Pa·s; or 1 to 15 Pa·s, or 2 to 12 Pa·s, or 3 to 10 Pa·s, wherein the viscosity is at 25°C and 2500s -1 Measured at a shear rate of .
[0113] The second aspect of the present invention is a method for coating an optical fiber, comprising providing a glass optical fiber, preferably drawing the glass optical fiber through a drawing tower; applying a primary coating composition to the surface of the glass optical fiber; optionally, applying a dose of ultraviolet light sufficient to at least partially cure the primary coating composition; applying a secondary coating composition to the primary coating composition; exposing the primary coating composition and the secondary coating composition to at least one radiation source capable of emitting ultraviolet radiation to affect the curing of the primary coating composition and the secondary coating composition to form a cured primary coating on the surface of the optical fiber and a cured secondary coating on the surface of the cured primary coating; wherein the primary coating composition is a composition according to any embodiment of the first aspect of the present invention.
[0114] The third aspect of the present invention is a coated optical fiber, which includes a glass core and a cladding in contact with and surrounding the glass core; and a coating portion, the coating portion further including a primary coating in contact with and surrounding the cladding; and a secondary coating in contact with and surrounding the primary coating. According to this aspect, the primary coating is a cured product of a radiation-curable composition according to any embodiment of the first aspect, and the primary coating and the secondary coating are applied and cured according to any embodiment of the second aspect.
[0115] According to one embodiment of the third aspect, the optical fiber comprises a core, a cladding, a primary coating contacting and surrounding an outer annular cladding region, and a secondary coating. According to some embodiments of the third aspect, the core comprises pure silica glass (SiO2) or silica glass with one or more dopants, the dopants increasing the refractive index of the glass core relative to pure, undoped silica glass. Suitable dopants for increasing the refractive index of the core include, but are not limited to, GeO2, Al2O3, P2O5, TiO2, ZrO2, Nb2O5, Ta2O5, and / or combinations thereof.
[0116] The cladding may comprise pure silica glass (SiO2), silica glass with one or more dopants that increase the refractive index (e.g., GeO2, Al2O3, P2O5, TiO2, ZrO2, Nb2O5 and / or Ta2O5) (e.g., when the cladding is "up-doped"), or silica glass with dopants that decrease the refractive index (e.g., fluorine) (e.g., when the inner cladding is "down-doped"), as long as the maximum relative refractive index of the core [Δ 1MAX ] is greater than the maximum relative refractive index of the cladding [Δ 4MAX ]. According to one embodiment, the cladding is also pure silica glass.
[0117] According to some embodiments of the third aspect, the primary coating is a typical primary coating having an in-situ (or on-fiber) tensile modulus of less than 1.5 MPa, or less than 1.0 MPa, or less than 0.6 MPa, or less than 0.5 MPa, or less than 0.3 MPa, or 0.15 to 0.8 MPa, and in other embodiments less than 0.2 MPa. Methods for describing in-situ moduli are well known in the art and are particularly described in US 7,171,103 and US 6,961,508, each of which is assigned to Covestro (Netherlands) BV. In one embodiment, the cured primary coating has an in-situ glass transition temperature of less than -35°C, or less than -40°C, or less than -45°C, and in other embodiments does not exceed -50°C. A primary coating with a low in-situ modulus reduces microbending, which is a coupling mechanism between modes propagating in a fiber. The low in-situ glass transition temperature ensures that the in-situ modulus of the primary coating will remain low even if the fiber is deployed in very cold environments.
[0118] The primary coating maintains sufficient adhesion to the glass fiber during heat and hydrolytic aging, and can be stripped from the glass fiber for splicing (if necessary). The primary coating typically has a thickness in the range of 20 to 50 μm (e.g., about 25 or 32.5 μm), with a thinner thickness in the range of 15 to 25 μm for 200 μm fibers. In other embodiments, the primary coating preferably has a thickness of less than about 40 μm, more preferably about 20 to about 40 μm, and most preferably about 20 to about 30 μm.
[0119] The secondary coating is in contact with and surrounds the primary coating. For example, the secondary coating is a polymerized product of a coating composition whose molecules become highly cross-linked when polymerized. According to one embodiment, the secondary coating may have an in-situ tensile modulus greater than 800 MPa, or greater than 1110 MPa, or greater than 1300 MPa, or greater than 1400 MPa, or greater than 1500 MPa. A secondary coating with a high in-situ modulus reduces microbending, which is a coupling mechanism between modes propagating in a fiber.
[0120] According to other embodiments, the secondary coating has a high in-place modulus (e.g., greater than about 800 MPa at 25° C.) and a high T g (e.g., greater than about 50°C). In other preferred embodiments, the in-situ secondary modulus is from about 1000 MPa to about 8000 MPa, more preferably from about 1200 MPa to about 5000 MPa, and most preferably from about 1500 MPa to about 3000 MPa. g Preferably between about 50° C. and about 120° C., more preferably between about 50° C. and about 100° C. In one embodiment, the secondary coating has a thickness of less than about 40 μm, more preferably between about 20 and about 40 μm, most preferably between about 20 and about 30 μm.
[0121] Materials suitable for use as outer (or secondary) coating materials and considerations associated with the selection of such materials are well known in the art and are described, for example, in U.S. Pat. Nos. 4,962,992 and 5,104,433 to Chapin. As an alternative to these, low oligomer content coating systems may also be used to obtain high modulus coatings, as described in U.S. Pat. No. 6,775,451 to Botelho et al. and U.S. Pat. No. 6,689,463 to Chou et al. In addition, non-reactive oligomer components have been used to achieve high modulus coatings, as described in U.S. Application Publication No. 20070100039 to Schissel et al. As is well known in the art, the secondary coating may also include ink. In this case, the secondary coating may be referred to as a "colored secondary coating."
[0122] Alternatively, the coated optical fiber may include one or more additional layers disposed on the secondary layer. Most notably, these layers include a separate "ink" layer that is applied and cured separately from the secondary coating. Other multilayer coating systems are known and disclosed, for example, in WO 2017173296.
[0123] It is known in the art how to formulate typical optical fiber coatings for primary and secondary coatings of fibers as described above, as well as how to formulate inks and matrix materials that are cured using broadband UV lamps. A detailed discussion of this technology and related chemistry and testing methods can be found in the textbook "Specialty Optical Fibers Handbook" written by A. Mendez and T. F. Morse and published by Elsevier, Elsevier Inc. 2007, Section 4.6 to the end of Chapter 4.
[0124] Any fiber type may be used in embodiments of the second aspect of the invention. However, in a preferred embodiment, the coated fiber has a mode field diameter of 8 to 10 μm at a wavelength of 1310 nm, or a mode field diameter of 9 to 13 μm at a wavelength of 1550 nm, and / or a mode field diameter of 20 to 200 μm. 2 In view of the fact that the coating process of these fibers is expected to require higher line or processing speeds, such fibers can be single-mode and / or large effective area fibers. However, other fiber types, such as multimode fibers, can also be used.
[0125] The fourth aspect of the present invention is an optical fiber cable, wherein the optical fiber comprises at least one optical fiber according to any embodiment of the third aspect of the present invention, and / or wherein the optical fiber is a cured product of the composition according to the first aspect of the present invention, and / or wherein the optical fiber is coated according to the second aspect of the present invention.
[0126] The improved compositions of the present invention (and the coated optical fibers produced therefrom) can be formulated by selecting the components specified herein above, and can be further readily modified by one of ordinary skill in the art to which the present invention applies by following the formulation guidance herein and by extrapolating from the general methods employed in the embodiments shown in the examples below. The following examples will further illustrate the present invention, but of course should not be construed as limiting its scope in any way. Example
[0127] These examples illustrate embodiments of the present invention. Table 1 describes the various components of the compositions used in this example. Table 2 describes the relative amounts of the reagents described in Table 1, which were used to synthesize the oligomers used in this example. Table 3 provides a summary of further analysis of the oligomers characterized in Table 2, wherein the methods for analyzing such oligomers are further described herein below.
[0128] Table 1 - Formulation Components
[0129]
[0130]
[0131] Synthesis of oligomers 1-16
[0132] First, the reactor is purged with dry, dilute air. Then the amounts specified in Table 2 below: first, (1) BHT (e.g., 1.32 parts for oligomer 1); then (2) the appropriate isocyanate (e.g., 86.62 parts of TDI for oligomer 1), followed by (3) acrylic acid (e.g., 0.09 parts for oligomer 1) are charged into the reactor (equipped with a stirrer, air inlet, dropping funnel, and condenser). After the additions, the reactor is heated to 45°C. Then, half of the specified DBTDL catalyst (e.g., DBTDL 0.06 g) and a hydroxyl-functional end-capping agent (e.g., HEA, 57.87 parts in oligomer 1) are charged into the reactor in sequence under stirring. Wait one (1) hour for the reaction to start, and then raise the temperature to 60°C. At 60°C, add the hydroxyl- or thiol-functional backbone component (e.g., HO-PPG 1000 -OBu, 661.01 g / oligomer 1) and a second portion of catalyst (eg 0.07 g) were added and the reaction temperature was then raised to 85°C and maintained for an additional two (2) hours.
[0133] After this additional two (2) hours of reaction time, the amount of isocyanate (NCO) content was measured with a potentiometric titrator to ensure that it was below 0.1% relative to the total weight of the composition. If the isocyanate content was not below this value, the mixture was returned to the reaction chamber (again at 85°C) for additional increments of 15 minutes and checked again, and this step was repeated until the isocyanate content fell within the desired range. Finally, the resulting synthesized oligomer was slowly cooled and discharged for use in the experiments described elsewhere herein.
[0134] The resulting oligomers have the ideal structures given in Table 2. Oligomer 1 has the following ideal structure (wherein "T" represents the reaction product of a diisocyanate compound, "PPG 1000 " means polyol PPG 1000 and "H-" represents the reaction product of a hydroxyl functional end-capping agent HEA):
[0135] HT-PPG 1000 -OH
[0136] Notes for oligomer 16: Two oligomers were generated using a one-pot synthesis:
[0137] 80%HT-PDMS3000-OH(a)+20%HT-PDMS3000-TH(b)
[0138] Oligomer 17
[0139] The oligomer was prepared as described in WO2021021971 (oligomer 1 in WO2021021971) using 95.32 parts of Acclaim 6320N, 6.15 parts of HEA, 503 parts of Acclaim 8200N, 18.97 parts of TDI, 0.3 parts of DBTDL, 0.824 parts of BHT, 0.29 parts of acrylic acid, and 190.4 parts of SR489D. The ideal structure is as follows (wherein "T" represents the reaction product of the diisocyanate compound TDI, "-H" represents the reaction product of the hydroxyl functional end-capping agent HEA, and "PPG 6000 "(Triol)" means the reaction product of the polyol Acclaim 6320N):
[0140] PPG 6000 (Triol)-(T-PPG 8000 -TH)3
[0141] Oligomer 18
[0142] First, the reactor was purged with dry, thin air. Then 0.28 g of BHT, 150.77 g of oligomer 3 (HT-PPG4000-OH) and 0.02 g of acrylic acid were charged into the reactor (equipped with a stirrer, air inlet, dropping funnel and condenser). After the additions, the reactor was heated to 75°C and then 0.03 g of DBTDL was added, followed by 8.65 g of 3-(triethoxysilyl)propyl isocyanate, after which the mixture was stirred for an additional 2 hours. After this additional two (2) hours of reaction time, the amount of isocyanate (NCO) content was measured with a potentiometric titrator to ensure that it was less than 0.1% relative to the total weight of the composition. If the isocyanate content was not less than this value, the mixture was returned to the reaction chamber (again at 85°C) in additional increments of 30 minutes and checked again, repeating this step until the isocyanate content fell within the desired range. Finally, the resulting synthesized oligomer was slowly cooled and discharged for use in the experiments described elsewhere herein. The resulting oligomer has the following ideal structure (wherein "T" represents the reaction product of a diisocyanate compound and "H-" represents the reaction product of a hydroxyl functional end-capping agent HEA):
[0143] HT-PPG 4000 -OC(O)NHC3H5Si(OC2H5)3
[0144] Oligomer 19
[0145] First, a 500 ml reactor was purged with dry, thin air. Then 0.5 parts of BHT, 0.03 parts of acrylic acid, and 300 parts of Acclaim 4200 were charged into the reactor (equipped with a stirrer, air inlet, dropping funnel, and condenser). After the additions, the reactor was heated to 85°C, at which temperature 0.06 parts of DBTDL were added. Next, 10.07 parts of 2-isocyanatoethyl acrylate were slowly added while stirring and kept at 85°C for another 2 hours, after which the NCO content was less than 0.1%.
[0146] The resulting oligomer has the following ideal structure (where "A" represents an acrylate group (ie, CH2CHCO2)):
[0147] A-C2H4NHC(O)O-PPG 4000 -OH
[0148] In the same manner as oligomer 18 above, 138.87 g of this intermediate oligomer (A-C2H4NHC(O)O-PPG 4000 -OH) and 7.3 g of 3-(triethoxysilyl)propyl isocyanate to prepare an oligomer. The resulting oligomer has the following ideal structure (wherein "A" represents an acrylate group (i.e., CH2CHCO2)):
[0149] A-C2H4NHC(O)O-PPG 4000 -OC(O)NHC3H6Si(OC2H5)3
[0150]
[0151]
[0152]
[0153] SEC characterization
[0154] After the various reactive oligomers were synthesized, they were then evaluated according to size exclusion chromatography (SEC) according to ASTM: D5296-11: "Standard Test Method for Molecular Weight Averages and Molecular Weight Distribution of Polystyrene by High Performance Size-Exclusion Chromatography," ASTM International, West Conshohocken, PA, (2011). In addition, ASTM standard D 5226-98: "Standard Practice for Dissolving Polymer Materials," ASTM International, West Conshohocken, PA, (2010) was used to facilitate the definition of solvents suitable for polymer analysis.
[0155] Specifically, all size exclusion chromatography measurements were performed using a Waters APC (Advanced Polymer Chromatography) system equipped with an RI detector, a Wyatt microDawn multi-angle light scattering instrument, and a Wyatt microViscoStar capillary-bridge differential viscometer. For chromatographic separation, chromatographic columns were used: 4.6 x 76 mm, Acquity APC XT 450 2.5 μm, 125 2.5 μm, 45 1.7 μm. The detector and chromatographic column were operated at 40 ° C. Before SEC, each corresponding polymer was dissolved in tetrahydrofuran (THF) containing 1 wt % acetic acid in a concentration range of 1.0 to 1.5 mg / ml. The THF solution was also used as an eluent in SEC analysis at a flow rate of 0.5 ml / min.
[0156] After dissolution was complete, the molar mass and molar mass distribution were then determined using the triple detection method mentioned above, using the refractive index, differential viscosity and right-angle light scattering signals. To calculate the molecular weight average and molar mass distribution, a refractive index increment (dn / dc) of approximately 0.07 ml / g was used. Specifically, the dn / dc values of oligomers 1-19 were determined accordingly and reported in ml / g in Table 3 of this article. The refractive index increment and the molecular weight average and molar mass distribution were determined by integrating the entire refractive index chromatogram. The IV-DP signal was also used to set the integration limits. The sample recovery from the chromatographic column was between 95% and 105%, which is a typical value obtained by size exclusion chromatography.
[0157] Using the methods described above, record and report the values of Mn, Mw, Mz and dn / dc.
[0158] Oligomer Tg
[0159] The glass transition temperature (Tg) of the synthesized oligomers was determined on a Mettler Toledo DSC3+ differential scanning calorimeter. The temperature range adopted was from -80°C to 80°C. Therefore, only Tg values above -70°C can be reliably determined. The evaluation was performed using the Stare software with the first derivative of the second heating curve using a heating rate of 10°C / min.
[0160] Formulations 1-42
[0161] Each of the formulations described in Table 4 below was prepared by conventional methods using a Speedmixer TM Specifically, 1 part by weight of photoinitiator BAPO and 0.25 parts of Irganox 1520L were added to the amounts of components specified in Table 4 below, resulting in a total of 10 g per formulation. The cup was then closed and the mixture was stirred in a Speedmixer. TM Mix vigorously in DAC150 FVZ for 30 seconds, stop, and then mix in the same manner for another 30 seconds.
[0162] These samples were tested according to the following methods to determine the viscosity, T 30%、模量最大值 and maximum G'. Viscosity values are reported in Pascal seconds (Pa·s) and rounded to two decimal places, while T 30%、模量最大值 It is expressed in seconds, also rounded to two decimal places. Maximum G' is reported in kilopascals (kPa), rounded to the nearest whole unit. The values of these measured properties are reported in Table 4 below.
[0163] Viscosity
[0164] The viscosity of the formulations was measured on a Brookfield CAP 1000 at 750 rpm and recorded after 30 seconds. -1 Three measurements were performed at a shear rate of 1.5 Å (the average values are shown in Table 4 below).
[0165] Determine the maximum modulus (G') and T 30%、模量最大值 value
[0166] The value of the maximum modulus (G') was determined according to the following procedure described herein. The hardware / equipment used in this procedure is as follows:
[0167] Rheometer + accessories
[0168] ARESG2 Rheometer (Manufacturer: TA Instruments)
[0169] APS temperature control device (Advanced Peltier System)
[0170] APS standard plate (lower geometry)
[0171] ARESG2 UV curing accessories (upper plate fixture, UV protection back cover and access door, collimating optical lens)
[0172] · Acrylic sheet with UV curing option Upper plate fixture (upper structure)
[0173] Silverline UV radiometer, UV light sensor (uncalibrated), UV sensor geometry and disposable plate holder
[0174] UV light source & others
[0175] Omnicure LX500 combined with 385nm LED and 8mm lens
[0176] Moeller Easy 412-DC-TC control relay (trigger box)
[0177] UV Power Puck II (Electronic Instrumentation & Technology, calibrated)
[0178] The hardware described above was then set up and arranged as follows. First, UV curing measurements were performed on an ARES G2 rheometer (TAInstruments). The rheometer was equipped with an APS temperature control unit, an APS standard plate (as the lower geometry), and the ARES G2 UV curing option. The upper geometry used was a combination of the upper plate fixture from the ARES G2 UV curing option with an acrylic plate of 20 mm diameter. As a UV light source, an Omnicure LX500 spot curing system was used in combination with a 385 nm LED (8 mm lens). The 385 nm LED was then inserted into the collimating optical lens of the ARES G2 UV curing accessory. The collimating lens was fixed to the light shield and aligned with the upper UV geometry mirror and the alignment screws were tightened. The original 5 mm diameter of the light guide support part of the collimating lens was increased to 12 mm to accommodate the 385 nm UV-LED.
[0179] The Omnicure LX500 spot curing system is then connected to the DIGITAL I / O connector on the ARESG2 via a Moeller Easy 412-DC-TC control relay. The control relay acts as a trigger box for the UV light source. The delay time of the trigger is set to 1.5 seconds, which means that the 385nmUV-LED automatically turns on with a delay of 1.5 seconds after the data collection of the modulus measurement starts on the ARESG2. The light intensity is set to 95%, and the duration of the UV light is fixed to 128 seconds.
[0180] UV Alignment: Alignment was performed before mounting the APS temperature control unit. The UV sensor geometry was attached to the disposable plate holder and mounted as the lower geometry. The UV light sensor connected to the Silverline UV radiometer was located in the outer hole of the UV sensor geometry. The upper geometry was positioned on top of the UV light sensor by applying an axial force of about 100 grams. The light intensity was then measured at four positions by rotating the lower geometry by about 90° between each consecutive measurement. In order to achieve the light distribution at each point to be as uniform as possible, the alignment of the collimating lens was then adjusted using the alignment screws on the light shield. The difference in light intensity at the four different positions was kept below 10%.
[0181] Determination of light intensity: Prior to the RT-DMA measurement, the UV intensity was measured with the aid of a calibrated UV Power Puck II. To achieve this, the sensor of the UV Power Puck II was placed directly below the surface of a 20 mm acrylic plate in the upper plate fixture (distance < 0.5 mm), where the surface of the acrylic plate completely covered the sensor surface. Next, the Omnicure LX 500 UV source was manually turned on (intensity value set to 95%) for 10 seconds. During this 10 second interval, the UVA2 intensity (i.e., radiation between 380-410 nm wavelengths) was measured with the UV Power Puck II instrument. The UVA2 intensity was measured to be 60-70 mW / cm 2 The actual value recorded is 67mW / cm 2 .
[0182] Determination of actual delay time : When starting a measurement, there is a delay between the start of data sampling and the start of UV illumination. In the settings of the Moeller Easy412-DC-TC control relay, the delay is set to 1.5 seconds, which means that UV illumination starts 1.5 seconds after the start of data sampling.
[0183] The actual delay time was measured using a light dependent resistor (LDR) and an oscilloscope (PicoScope 3424) to be 1.519 seconds. The delay time of 1.519 seconds is the average of 10 individual measurements with a standard deviation of 0.004 seconds.
[0184] RT-DMA measurement: RT-DMA UV cure measurements were then performed using an ARESG2 rheometer setup with an Advanced Peltier system as temperature control, an APS plate and an ARESG2 UV cure accessory. A 385nm LED equipped with an 8mm lens connected to an Omnicure LX500 was used as the UV light source.
[0185] Sample loading: Before loading each corresponding sample, the temperature of the bottom plate is set to 50°C. When the temperature reaches 50°C, the surface of the upper plate (acrylic plate with a thickness of 20 mm) is brought into contact with the lower plate (i.e., the gap is 0 mm) by applying an axial force between 200-400 grams, so that the upper parallel plates are equilibrated to the set temperature of 50°C. After the initial contact, the system is allowed to further equilibrate its temperature for at least 5 minutes. Next, a zero fixation procedure is performed according to well-known methods to determine the gap = 0 position. After determining the gap = 0 position, the upper plate is moved to a position 10 mm away. A portion of each corresponding sample is then transferred to the center of the lower plate using the tip of a small spatula, and the upper geometry is then lowered to the position of gap = 0.120 mm. The number of samples must be sufficient to ensure that after the upper geometry is lowered to the reduced gap, the excess sample will be pushed out of the gap and cover the entire periphery of the upper parallel plates. Next, the excess sample that has been moved out of the gap is removed, and the upper geometry is further lowered to the measurement position (gap = 0.100 mm). After loading the measurement position, the sample temperature is allowed to equilibrate to 50°C. Finally, when the sample temperature was measured to be stable between 49.90 and 50.10 °C, the measurement process was started by activating the trigger box (MoellerEasy412-DC-TC) and using the interfaces and interconnects provided by the TRIOS software package.
[0186] Measurement : The actual UV-curing RT-DMA measurement is a so-called "fast sampling" measurement performed at 50° C. That is, it is an oscillating fast sampling at 50° C., with a duration of 128 seconds, a strain of 1%, a rotation speed of 52.36 rad / s, and a measurement frequency of 50 points / s (i.e., 0.020 seconds between each consecutive measurement point).
[0187] The measurement was then started by pressing the Start button in the TRIOS software. Once data sampling began, the rheometer sent a signal to the control relay, which in turn activated the Omnicure LX500 UV light source to illuminate the corresponding sample, with the delay being 1.519 seconds after the start of data sampling. As described above, during the 128-second rapid sampling data collection process, 385nm UV light (intensity 60-70mW / cm 2 ) to illuminate the sample. After the measurement is completed, the TRIOS data file is exported to Microsoft Excel. The sample is then removed and the plate is subsequently cleaned thoroughly with ethanol before loading the next sample.
[0188] Data Analysis: As mentioned above, TRIOS data has been exported to Microsoft Excel. Excel was used to plot graphs and calculate various parameters to characterize the curing speed performance of the test formulations described below. These graphs include graphs corresponding to storage modulus (G'), where storage modulus (G') is a function of UV-time (UV-time is calculated by subtracting the delay time (1.519 seconds) from the actual time of each individual data point), and graphs corresponding to relative storage modulus (rel G'), where relative storage modulus (rel G') is a function of UV-time (rel G' is calculated by the quotient of the measured G' value at a specific UV-time and the maximum G' value obtained during the curing measurement). The maximum value observed in the graph of the G' graph is determined by taking the average value of the G' value between 110 and 120 seconds, and is reported in the column titled "Max.G'" in Table 4 below. For samples that were not fully cured within the test time, this column is marked with an "NFC" mark, indicating that Max.G' could not be reached within the test procedure and time limit adopted.
[0189] Meanwhile, the characteristic parameters include: (1) the time to reach 30% increase in total storage modulus (G'), and (2) average G'110-120s (the average storage modulus value of 6 data points at the end of the curing measurement). 30%、模量最大值 The results for each formulation for (1) are reported in the column titled.
[0190]
[0191]
[0192]
[0193] Results and Discussion
[0194] It can be seen that the compositions according to various aspects of the present invention tend to have properties that make them particularly suitable for use in optical fiber coating applications, and in particular as primary coatings for optical fibers. First, it will be apparent that, other things being equal, compositions containing little or no reactive diluent (in the above examples, EEOOA, DMA and / or nVC are used) are more preferred for use in optical fiber coating applications because the volatile content is minimized.
[0195] Furthermore, the results indicate that compositions with such low volatile content can be formulated in a variety of ways to exhibit stability that is further suitable for optical fiber coating applications, particularly with respect to: cure speed (via low T 30%、模量最大值 values, especially those below 1.2 seconds, more preferably below 1.0 seconds), low modulus (measured by low G' values, especially those below 600 kPa, more preferably below 500 kPa, more preferably below 400 kPa, more preferably below 300 kPa), and / or low viscosity (especially those below 9 Pascal seconds, more preferably below 5 Pascal seconds).
[0196] The above effect(s) can be demonstrated using a variety of oligomer types, amounts, combinations, and diluents.
[0197] Unless otherwise specified, the term "weight %" refers to the amount by mass of a particular ingredient relative to the entire liquid radiation curable composition into which it is incorporated.
[0198] In the context of describing the present invention (especially in the context of the following claims), the use of the terms "one", "a kind of" and "the" and similar references should be interpreted as covering both the singular and the plural, unless otherwise specified herein or clearly contradictory to the context. Unless otherwise specified, the terms "include", "have", "include" and "contain" should be interpreted as open terms (i.e., meaning "including but not limited to"). Unless otherwise specified herein, the numerical ranges listed herein are merely intended to be used as a convenient method for individually referring to each individual value falling within the range, and each individual value is incorporated into the specification as if it were listed separately herein. Unless otherwise specified herein or clearly contradictory to the context, all methods described herein can be performed in any suitable order. The use of any and all examples or exemplary language (e.g., "such as") provided herein is intended only to better illustrate the present invention, and unless otherwise stated, does not limit the scope of the present invention. Any language in the specification should not be interpreted as indicating that any unclaimed element is essential to the practice of the present invention.
[0199] Preferred embodiments of the present invention are described herein, including the best mode of implementing the present invention known to the inventor. For those of ordinary skill in the art, after reading the above description, changes in these preferred embodiments will become apparent. The inventor expects that skilled technicians can adopt such variations as appropriate, and the inventor intends to practice the present invention in a manner different from that specifically described herein. Therefore, the present invention includes all modifications and equivalents of the subject matter described in the claims attached hereto as permitted by applicable law. In addition, unless otherwise stated herein or clearly contradictory to the context, the present invention covers any combination of the above-mentioned elements in all possible variations thereof.
[0200] While the invention has been described in detail and with reference to specific embodiments thereof, it will be apparent to one skilled in the art that various changes and modifications can be made therein without departing from the spirit and scope of the invention as claimed.
Claims
1. An optical fiber primary coating composition comprising the following components in an amount relative to the weight of the entire primary coating composition: (a) at least 0.01 wt. % of one or more oligomers which are the reaction product of (iii) a hydroxy-functional capping agent further comprising an ethylenically unsaturated moiety, (ii) an isocyanate compound, and (i) a hydroxy- or thiol-functional backbone compound; wherein the molar ratio of the number of isocyanate groups in (ii) to the number of hydroxyl groups and thiol groups in (i) is less than or equal to 1.0; (b) optionally, one or more urethane (meth)acrylate oligomers other than (a); (c) optionally, a reactive diluent monomer; (d) a photoinitiator; (e) optionally, one or more additives; The total amount of (a) + (b) is 70 wt % to 99 wt %.
2. The optical fiber primary coating composition of claim 1, wherein if (b) is absent, the one or more oligomers according to (a) have at least two ethylenically unsaturated groups, more preferably two ethylenically unsaturated groups.
3. The optical fiber primary coating composition of any of the preceding claims, wherein the one or more oligomers according to (a) are present in an amount greater than or equal to 0.1 wt. % and less than or equal to 96 wt. %; wherein (i) comprises a polyether, polyester, polybutadiene, polycarbonate or silicone moiety.
4. An optical fiber primary coating composition according to any one of the preceding claims, wherein the one or more oligomers according to (a) are present in an amount greater than 1 wt. %, preferably greater than 5 wt. %, preferably greater than 10 wt. %, preferably greater than 20 wt. %, preferably greater than 30 wt. %, preferably greater than 40 wt. %.
5. An optical fiber primary coating composition according to any one of the preceding claims, wherein the one or more oligomers according to (a) are present in an amount less than or equal to 95 wt. %, preferably less than or equal to 90 wt. %, preferably less than or equal to 80 wt. %, preferably less than or equal to 70 wt. %.
6. The optical fiber primary coating composition according to any one of the preceding claims, wherein the acrylate content in the composition is less than or equal to 2.50 mol / kg of the composition, preferably less than or equal to 2.00 mol / kg of the composition, more preferably less than or equal to 1.50 mol / kg of the composition, more preferably less than or equal to 1.20 mol / kg of the composition, more preferably less than or equal to 1.00 mol / kg of the composition, more preferably less than or equal to 0.80 mol / kg of the composition.
7. The optical fiber primary coating composition according to any one of the preceding claims, wherein the content of carbamate in the composition is 0.20 to 1.5 mol / kg of the composition.
8. The optical fiber primary coating composition according to any one of the preceding claims, wherein the carbamate content in the composition is less than or equal to 0.90 mol / kg of the composition, preferably less than or equal to 0.70 mol / kg of the composition.
9. The optical fiber primary coating composition according to any one of the preceding claims, wherein the carbamate content in the composition is greater than, or equal to, 0.25 mol / kg of the composition, or greater than, or equal to, 0.30 mol / kg of the composition, or greater than, or equal to, 0.31 mol / kg of the composition, or greater than, or equal to, 0.35 mol / kg of the composition, or greater than, or equal to, 0.40 mol / kg of the composition, or greater than, or equal to, 0.45 mol / kg of the composition, or greater than, or equal to, 0.50 mol / kg of the composition.
10. The optical fiber primary coating composition according to any one of the preceding claims, wherein the total acrylate content in oligomer (a) and oligomer (b) is from 0.05 mol / kg oligomer (a) + (b) to 0.80 mol / kg oligomer (a) + (b).
11. The optical fiber primary coating composition according to any one of the preceding claims, wherein the total acrylate content in the oligomer (a) and the oligomer (b) is less than or equal to 0.70 mol / kg of oligomer (a) + (b), or less than or equal to 0.60 mol / kg of oligomer (a) + (b), or less than or equal to 0.50 mol / kg of oligomer (a) + (b), or less than or equal to 0.40 mol / kg of oligomer (a) + (b), or less than or equal to 0.30 mol / kg of oligomer (a) + (b), or less than or equal to 0.28 mol / kg of oligomer (a) + (b).
12. An optical fiber primary coating composition according to any one of the preceding claims, wherein the oligomers according to (a) and (b) are present in an amount greater than or equal to 80 wt. % and less than or equal to 96 wt. %; wherein (i) comprises a polyether, polyester, polybutadiene, polycarbonate or silicone moiety.
13. An optical fiber primary coating composition according to any one of the preceding claims, wherein the hydroxyl or thiol functional backbone compound (i) comprises a polyether polyol, preferably polypropylene glycol.
14. The optical fiber primary coating composition according to any one of the preceding claims, wherein the molar ratio of the number of isocyanate groups in (ii) to the number of hydroxyl groups and thiol groups in (i) is greater than or equal to 2 / 3.
15. The optical fiber primary coating composition according to any one of the preceding claims, wherein the one or more oligomers according to (a) have a viscosity of less than 15 Pa·s, or less than 12, or less than 10 Pa·s, or less than 2 Pa·s, or from 1 to 15 Pa·s, or from 2 to 12 Pa·s, or from 3 to 10 Pa·s, wherein the viscosity is at 25°C and 2500 s -1 Measured at a shear rate of .
16. An optical fiber primary coating composition according to any one of the preceding claims, wherein the oligomer according to (a) has 1.8 to 2.2 urethane bonds; and / or wherein one or more oligomers according to (a) have a diblock or triblock structure.
17. An optical fiber primary coating composition according to any one of the preceding claims, wherein the one or more oligomers according to (a) have a number average molecular weight (Mn) of 1000 g / mol to 10000 g / mol, preferably 1200 g / mol to 9000 g / mol.
18. An optical fiber primary coating composition according to any one of the preceding claims, wherein the one or more oligomers according to (a) are terminated at one end with a hydroxyl group.
19. The optical fiber primary coating composition according to any one of the preceding claims, wherein (iii) the hydroxyl-functional capping agent further comprises one or two ethylenically unsaturated moieties, preferably, (iii) the hydroxyl-functional capping agent further comprises one ethylenically unsaturated moiety.
20. The optical fiber primary coating composition of any one of the preceding claims, wherein the (i) hydroxyl-functional backbone compound comprises at least two hydroxyl groups, or at least three hydroxyl groups, or four hydroxyl groups.
21. An optical fiber primary coating composition according to any one of the preceding claims, wherein the one or more oligomers according to (a) comprise the reaction product of a single PPG diol as (i), a single diisocyanate compound as (ii), and a hydroxyl-functional (meth)acrylate compound as (iii).
22. The optical fiber primary coating composition according to any one of the preceding claims, wherein the molar ratio of the number of isocyanate groups in (ii) to the number of hydroxyl groups in (i) in the one or more oligomers (a) is equal to 1.
0.
23. The optical fiber primary coating composition of any one of the preceding claims, wherein (ii) comprises, consists essentially of, or consists of composition: Isophorone diisocyanate, 2,4-isomer toluene diisocyanate, 4,4'-methylene dicyclohexyl diisocyanate, 1,5-pentane diisocyanate, 2,2,4-trimethyl-hexamethylene diisocyanate, 2,4,4-trimethyl-hexamethylene diisocyanate, or hexamethylene diisocyanate, or a combination thereof.
24. The optical fiber primary coating composition of any one of the preceding claims, wherein (iii) comprises, consists essentially of, or consists of composition: Hydroxyethyl methacrylate, hydroxyethyl acrylate, 2-hydroxypropyl methacrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl methacrylate, 4-hydroxybutyl acrylate, caprolactone methacrylate, caprolactone acrylate, glyceryl acrylate methacrylate, glyceryl dimethacrylate, glyceryl diacrylate, or a combination thereof.
25. An optical fiber primary coating composition according to any one of the preceding claims, wherein the one or more urethane (meth)acrylate oligomers (b) are present in an amount of 29.95 wt. % or less.
26. An optical fiber primary coating composition according to any one of the preceding claims, wherein the one or more urethane (meth)acrylate oligomers (b) further comprise the reaction product of (i) a hydroxyl-functional backbone compound, (ii) an isocyanate compound; and (iii) a hydroxyl-functional capping agent; The molar ratio of the number of isocyanate groups in (ii) to the number of hydroxyl groups in (i) in the urethane (meth)acrylate oligomer (b) is greater than 1.0, more preferably about 1.5 to about 2.
0.
27. The optical fiber primary coating composition according to claim 26, wherein for the oligomer according to (b), the molar ratio of the number of isocyanate groups in (ii) to the number of hydroxyl groups and thiol groups in (i) and (iii) is equal to 1.
0.
28. An optical fiber primary coating composition according to any one of the preceding claims, wherein (c) is present in an amount of 29.95 weight percent or less and comprises 2-ethylhexyl acrylate, 2-phenoxyethyl acrylate, 2-(2-ethoxyethoxy)ethyl acrylate, n-vinyl pyrrolidone, dimethyl acrylamide, n-vinyl caprolactam, ethoxylated 2-phenoxyethyl acrylate, 4-hydroxybutyl acrylate, lauryl acrylate, isobornyl acrylate, caprolactone acrylate, ethoxylated nonylphenol acrylate, tridecyl acrylate, or isodecyl acrylate, or a combination thereof.
29. The optical fiber primary coating composition according to any of the preceding claims, wherein the photoinitiator (d) is present in an amount of 0.04 wt% to 8 wt% and comprises, consists essentially of, or consists of 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, α-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 2-hydroxy-2-methyl-1-(4-isopropylphenyl)propanone, 2-hydroxy-2-methyl-1-(4-dodecylphenyl)propanone, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propan-1-one, or 2-hydroxy-2-methyl-1-[(2-hydroxyethoxy)phenyl]propanone, or a combination thereof.
30. An optical fiber primary coating composition according to any one of the preceding claims, wherein additive (e) is present in an amount less than 10 wt. % and further comprises an adhesion promoter.
31. An optical fiber primary coating composition according to any one of the preceding claims, in, applying the primary coating composition to a surface of a glass optical fiber; and applying a secondary coating composition to the primary coating composition; and exposing the coating composition and the secondary coating composition to at least one radiation source capable of emitting ultraviolet radiation to affect the curing of the primary coating composition and the secondary coating composition to form a cured primary coating on the surface of the optical fiber and a cured secondary coating on the surface of the cured primary coating, wherein the cured primary coating has an in-situ tensile modulus of less than 1.5 MPa.
32. An optical fiber primary coating composition according to any one of the preceding claims, in, The composition, when cured into a film according to the methods and dimensions specified elsewhere herein, has: a storage modulus (G') of less than 600 kPa, or from 1 to 550 kPa, or from 10 to 500 kPa, or less than 300 kPa, or from 1 to 200 kPa, or from 10 to 150 kPa; and / or The time to reach a 30% increase in storage modulus is less than 1.2 seconds, or less than 1 second.