Method for manufacturing silicon nitride substrate

By using a continuous heating furnace and appropriate laminated space configuration in the manufacturing process of silicon nitride substrate, the silicon melting problem caused by excessive lamination of sheet molded bodies is solved, and efficient production and high-quality output of silicon nitride substrates are achieved. .

CN119032072APending Publication Date: 2024-11-26PROTERIAL LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202380027399.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-30
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During the manufacturing process of silicon nitride substrate, too many laminated sheets of the sheet-shaped molded body lead to heat concentration of reaction, which may trigger silicon melting, which will affect the adequacy and productivity improvement of the nitriding reaction.

Method used

Using a continuous heating furnace, the sheet-shaped molded laminated body of 5 or more pieces and less than 20 pieces is nitrided in a nitrogen atmosphere. By adjusting the spacing and arrangement of the laminated body, the concentration of reaction heat is controlled to prevent silicon melting. , improve the productivity of the silicon nitride substrate.

Benefits of technology

The productivity of the silicon nitride substrate is effectively improved, the adequacy of the nitriding reaction and the quality of the product are ensured, and the manufacturing cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032072A_ABST
    Figure CN119032072A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to improve the productivity of a silicon nitride substrate when manufacturing a silicon nitride substrate by nitriding a laminate in which a plurality of silicon-containing sheet-like molded bodies are stacked. As a solution, a method for manufacturing a silicon nitride substrate is used in a continuous heating furnace provided with an input port, an output port, a heating mechanism for heating the space between the input port and the output port, and a nitrogen supply mechanism for supplying nitrogen between the input port and the output port, a laminated body, in which 5-20 silicon-containing sheet-shaped molded bodies are laminated, is conveyed from an input port to an output port, thereby nitriding the laminated body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a silicon nitride substrate, and more particularly to a method for producing a silicon nitride substrate by nitriding and sintering a plurality of sheet-shaped molded bodies mainly composed of silicon powder in a stacked state. Background Art

[0002] Conventionally, a ceramic circuit substrate in which a silicon nitride substrate, a metal circuit, and a metal heat sink are bonded together has been used in semiconductor modules, power modules, and the like.

[0003] As a method for manufacturing a silicon nitride substrate, the following method is known: raw materials composed of silicon (Si) powder, a sintering aid, a binder, and a solvent are mixed to prepare a slurry, the slurry is formed into a sheet, thereby preparing a sheet-like molded body (green sheet), and the sheet-like molded body is degreased, nitrided, and sintered to obtain a silicon nitride substrate. In the degreasing, nitriding, and sintering steps, the sheet-like molded body is added to a batch furnace on the basis of stacking a plurality of sheets, thereby achieving an improvement in productivity (for example, refer to Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2015-199657 Summary of the invention

[0007] Technical problem to be solved by the invention

[0008] However, in the nitriding process, if too many sheets of sheet-like molded bodies are stacked, a chain reaction may occur due to the concentration of reaction heat, and silicon may melt. This may cause problems in the appearance of the manufactured silicon nitride substrate and the problem that the nitriding reaction in the substrate becomes insufficient. That is, there is a limit to improving the productivity of silicon nitride substrates by increasing the number of sheets of sheet-like molded bodies stacked during nitriding.

[0009] Therefore, an object of the present invention is to improve the productivity of silicon nitride substrates.

[0010] Technical solutions for solving technical problems

[0011] A method for manufacturing a silicon nitride substrate in one embodiment is as follows: in a continuous heating furnace having an input port and an output port, a heating mechanism for heating between the input port and the output port, and a nitrogen supply mechanism for supplying nitrogen between the input port and the output port, a stack of sheet-like molded bodies containing silicon and having more than 5 and less than 20 sheets stacked thereon is transported from the input port to the output port, thereby performing nitridation.

[0012] Effects of the Invention

[0013] According to the method for manufacturing a silicon nitride substrate according to one embodiment, the productivity of the silicon nitride substrate is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a perspective view showing a schematic structure of a nitriding treatment furnace in the embodiment.

[0015] Figure 2 It is a plan view showing a stacked body composed of a plurality of sheet-like molded bodies and a case in the embodiment.

[0016] Figure 3 yes Figure 2 Cross-sectional view along line AA.

[0017] Figure 4 It is a plan view showing an example of a conveyance method of a stacked body in the embodiment.

[0018] Figure 5 It is a plan view showing an example of a conveyance method of a stacked body in the embodiment.

[0019] Figure 6 It is a cross-sectional view showing a stacked body and a case composed of a plurality of sheet-like molded bodies in Comparative Example and Examples 1 and 2.

[0020] Figure 7 It is a plan view showing the conveyance mode of the laminated body in Comparative Example and Examples 1 and 2. DETAILED DESCRIPTION

[0021] In all the drawings for explaining the embodiments, the same reference numerals are given to the same components in principle, and repeated descriptions thereof are omitted. It should be noted that, in order to make the drawings easier to understand, hatching may be given even in the top view and the side view.

[0022] <Silicon nitride substrate>

[0023] The silicon nitride substrate in this embodiment is a silicon nitride substrate having two surfaces as main surfaces, for example, a silicon nitride substrate having a first main surface as the front surface and a second main surface as the opposite surface thereof as the back surface. It should be noted that the terms front surface and back surface are used for the convenience of distinguishing each surface.

[0024] The silicon nitride substrate of this embodiment can be used as an insulating substrate used in a power module, for example. A power module is an electronic device that constitutes an inverter circuit that controls a motor included in an electric vehicle, a hybrid electric vehicle, a railway vehicle, or an industrial device.

[0025] <Method for producing silicon nitride substrate>

[0026] Next, a method for manufacturing a silicon nitride substrate according to the present embodiment will be described.

[0027] (1-1) Preparation of slurry (slurry preparation process)

[0028] First, rare earth element oxides and magnesium compounds are added as sintering aids to silicon powder, which is a raw material of the substrate, to prepare raw material powder, which is then pulverized by a medium dispersion method to prepare slurry. The raw materials used are described in detail below.

[0029] (a) Silicon

[0030] As the silicon used here, silicon powder of an industrially available grade can be used. The purity of the silicon powder is preferably 99% or more, more preferably 99.5% or more. Impurity oxygen contained in silicon is one of the main reasons for hindering the thermal conduction of the silicon nitride substrate obtained by reaction sintering, and is preferably as small as possible. In addition, impurity carbon contained in silicon is likely to hinder the growth of silicon nitride particles in the silicon nitride substrate obtained by reaction sintering. As a result, insufficient densification becomes one of the main reasons for reduced thermal conduction and insulation.

[0031] (b) Rare earth element oxides (sintering aids)

[0032] As the rare earth element oxide used here, oxides of Y, Yb, Gd, Er, Lu, etc. which are easily available and stable as oxides are preferred. Specific examples of rare earth element oxides include Y2O3, Yb2O3, Gd2O3, Er2O3, Lu2O3, etc.

[0033] (c) Magnesium compounds (sintering aids)

[0034] As the magnesium compound, one or more magnesium compounds containing silicon (Si), nitrogen (N) or oxygen (O) can be used. In particular, magnesium oxide (MgO), magnesium silicon nitride (MgSiN2), magnesium silicide (Mg2Si), magnesium nitride (Mg3N2) and the like are preferably used.

[0035] (d) Crushing

[0036] Rare earth element oxides and magnesium compounds are added to silicon powder as sintering aids in a predetermined ratio, a dispersion medium (organic solvent) and a dispersant as needed are added, and the powder is pulverized using a ball mill to prepare a slurry (dispersion of raw material powder). The types of the dispersion medium and the dispersant are not particularly limited and can be arbitrarily selected according to the sheet forming method, etc.

[0037] As the dispersion medium, ethanol, n-butanol, toluene, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK) or the like can be used, and as the dispersant, for example, a sorbitan ester type dispersant, a polyoxyalkylene type dispersant or the like can be used.

[0038] The time for pulverizing varies depending on the grinding device used and the amount and characteristics of the starting raw materials, and is therefore not particularly limited. It is preferred that the time be selected so that the raw material powders can be fully pulverized and mixed. The pulverizing time is, for example, preferably 6 hours or more and 48 hours or less, and more preferably 12 hours or more and 24 hours or less. If the pulverizing time is too short, the pulverizing cannot be performed sufficiently, and sometimes the silicon nitride substrate having the characteristics required in the present embodiment cannot be obtained. If the pulverizing time is too long, the amount of impurity oxygen slowly increases, and sometimes the thermal conductivity of the silicon nitride substrate decreases.

[0039] (1-2) Preparation of sheet-shaped molded body (sheet molding process)

[0040] To the obtained slurry, a dispersion medium, an organic binder, a dispersant, etc. are added as necessary, and vacuum degassing is performed as necessary to adjust the viscosity within a predetermined range to prepare a slurry for coating.

[0041] The prepared coating slurry is formed into a sheet using a sheet forming machine, cut into a specified size, and then dried to obtain a sheet-like molded body. The organic binder used in the preparation of the coating slurry is not particularly limited, and PVB resin (polyvinyl butyral resin), ethyl cellulose resin, acrylic resin, etc. can be listed. The amount of dispersion medium, organic binder, dispersant, etc. is preferably adjusted appropriately according to the coating conditions. The method for forming the coating slurry into a sheet is not particularly limited, and for example, a sheet forming method such as a scraper method can be used.

[0042] The sheet-like slurry is then transported to a drying chamber set at a predetermined temperature and humidity to evaporate the solvent and form a dry sheet-like molded body. The coated sheet is passed through a drying zone, where the temperature is gradually increased and dried.

[0043] The thickness of the sheet-like molded body formed in the molding step can be adjusted so that the thickness of the finally obtained silicon nitride substrate becomes a desired thickness, for example, 0.15 mm to 0.8 mm. In addition, the sheet-like molded body can be cut into a predetermined size by a punching machine or the like as needed.

[0044] (1-3) Heating of the molded body (heating step)

[0045] The obtained sheet-like molded body is heated to nitride the silicon contained in the molded body, and then densification is performed. The heating process includes: a degreasing process to remove the organic binder in the molded body; a nitriding process to nitridate the silicon (Si) contained in the molded body by heating the sheet-like molded body in a nitrogen atmosphere so that the silicon (Si) contained in the molded body reacts with nitrogen (N); and a sintering process to densify after nitridation. These processes can be performed sequentially in different furnaces or continuously in the same furnace.

[0046] In this embodiment, during the heating step, powdered boron nitride (BN) is applied to the first main surface of the sheet-like molded body to form a boron nitride (BN powder) layer. This boron nitride (BN) also functions as a separation material that facilitates separation after sintering when a plurality of sheet-like molded bodies are stacked. Therefore, when a plurality of sheet-like molded bodies are stacked, boron nitride (BN) exists between the sheet-like molded bodies, and each sintered body can be easily separated from the stack of sintered bodies obtained after sintering.

[0047] The sheet-shaped molded body coated with boron nitride powder (BN powder) is placed in an electric furnace, degreased (removed from organic binders, etc.), decarburized at 900°C to 1300°C in a nitriding furnace, heated to a predetermined temperature in a nitrogen atmosphere to nitride, and then sintered using a sintering device. At this time, it is preferred to heat the molded body while applying a load of 10Pa to 1000Pa. Degreasing is preferably performed at a temperature of 800°C or less.

[0048] It should be noted that as the above-mentioned separation material, a BN powder layer with a thickness of about 3 μm or more and 20 μm or less is preferably used. The BN powder layer can be formed by spraying, brushing or screen printing a slurry of BN powder on one side of each sheet-like molded body. The BN powder preferably has a purity of 95% or more and an average particle size (D50) of 1 μm or more and 20 μm or less.

[0049] Here, a laminate of sheet-like molded bodies is prepared by overlapping a plurality of sheet-like molded bodies in contact with each other. It is considered that the above-mentioned BN powder layer exists between the sheet-like molded bodies that constitute the laminate and overlap each other up and down. In addition, in the present application, a case where the laminate is composed of a plurality of sheet-like molded bodies that are stacked in contact with each other is described.

[0050] Below, use Figure 1~Figure 5 , the structure of the nitriding furnace, the sheet-like molded body conveyed in the nitriding furnace, and the structure of the stacked body are described.

[0051] Figure 1 is a perspective view of a nitriding furnace (continuous heating furnace) 1. Figure 1 In FIG. 1 , a part of the nitriding furnace 1 is broken to show the inside. Figure 1 As shown, the nitriding furnace 1 has a cylindrical structure with a rectangular cross section, for example, and a conveyor 4 for conveying a stack 5 of sheet-like molded bodies along the longitudinal direction of the nitriding furnace 1 is arranged inside. The conveyor 4 is, for example, a cylindrical rod supported so as to be axially rotatable, and a plurality of the rods are arranged in a radial direction (the conveying direction of the stack 5).

[0052] The nitriding furnace 1 includes an input port 2 for inputting the stacked body 5 and an output port 3 for outputting the stacked body 5. The nitriding furnace 1 also includes a heating mechanism for heating between the input port 2 and the output port 3 and a nitrogen supply mechanism for supplying nitrogen between the input port 2 and the output port 3. In the nitriding process, the stacked body 5 is inputted into the nitriding furnace 1 from the input port 2, conveyed by the conveyor 4, and outputted from the output port 3 to the outside of the nitriding furnace 1.

[0053] During such transportation, the plurality of sheet-like molded bodies constituting the stacked body (degreased body) 5 are nitrided by heating them up in a nitrogen atmosphere. That is, the stacked body 5 is nitrided by being transported from the input port 2 to the output port 3. In order to prevent the temperature in the nitriding furnace 1 from dropping, a shutter that is closed except when the stacked body 5 passes through may be provided at the input port 2 and the output port 3. Figure 1 In FIG. 1 , the conveying direction of the stacked body 5 is indicated by a white arrow.

[0054] In the nitriding step, the nitrogen partial pressure during nitriding is preferably 0.05 MPa to 0.7 MPa, more preferably 0.07 MPa to 0.2 MPa. The nitriding temperature is preferably 1350° C. to 1500° C., more preferably 1400° C. to 1450° C. The holding time after heating to the nitriding temperature is preferably 3 hours to 12 hours, more preferably 5 hours to 10 hours.

[0055] like Figure 1 As shown, a plurality of stacked bodies 5 are arranged in a first direction (column direction) intersecting the conveying direction when viewed from above. Here, for example, four stacked bodies 5 are arranged in a direction orthogonal to the conveying direction when viewed from above. By arranging and conveying a plurality of stacked bodies 5 in the column direction, a plurality of stacked bodies 5 can be nitrided at one time. In addition, by arranging a plurality of rows of stacked bodies 5 arranged in the column direction in the conveying direction and conveying them, a plurality of stacked bodies 5 can be nitrided continuously.

[0056] Here, in Figure 2 as well as Figure 3 Shown in Figure 1 The specific structure of the stacked body 5 arranged on the conveyor 4. Figure 3 yes Figure 2 The cross-sectional view at AA. Figure 2 as well as Figure 3 As shown, the stack 5 is placed in a housing 6 composed of a plate-shaped BN (boron nitride) setter 6a and a BN frame 6b surrounding the side of the stack 5 on the BN setter 6a. That is, the stack 5 is conveyed on the conveyor 4 while being placed in the housing 6.

[0057] The planar shape of the sheet-like molded body 5a constituting the stacked body 5 is a rectangle having a long side (first long side) and a short side (first short side), that is, a rectangular. The long side of the sheet-like molded body 5a is 100 mm or more, and the short side is 100 mm or more. Here, the long side of the sheet-like molded body 5a is, for example, 257 mm, and the short side is, for example, 190 mm. The shape in the top view of the BN setter 6a is a rectangle having a long side and a short side, that is, a rectangular. The long side of the BN setter 6a is, for example, 280 mm, and the short side is, for example, 210 mm.

[0058] like Figure 3 As shown in FIG. 1 , four BN setters 6a are stacked at intervals. Here, one stack 5 is placed on the surface of the lowest BN setter 6a, and another stack 5 is placed on the surface of the third BN setter 6a from the bottom. That is, the stack 5 is stacked in two layers when viewed from above. The stacked stacks 5 are not connected to each other in the height direction (vertical direction), and are separated from each other at a predetermined interval.

[0059] As one of the main features of this embodiment, the number of sheet-like molded bodies 5a constituting one stacked body 5 is within a range of 5 to 20. Specifically, one stacked body 5 is constituted by 15 sheet-like molded bodies 5a stacked in contact with each other in the height direction.

[0060] The thickness of one BN setter 6a is, for example, 1 mm or more and 5 mm or less. The thickness of one stacked body 5 is, for example, 7 mm. The interval between the stacked body 5 and the BN setter 6a thereon is, for example, 3 mm or more and 23 mm or less. The shortest distance between the BN setters 6a overlapping in the height direction, that is, the height of the BN frame 6b is, for example, 10 mm or more and 30 mm or less.

[0061] Here, the stacked body 5 is not arranged between the second BN setter 6a from the bottom and the third BN setter 6a from the bottom. As one of the main features of this embodiment, the shortest interval between the two stacked bodies 5 overlapping in the height direction is 9.0 mm or more and 35.0 mm or less. Specifically, here, the interval is 27 mm.

[0062] Thus, here, the stacked body 5 in which a plurality of sheet-like molded bodies 5a are overlapped is subjected to a single nitriding treatment. In addition, the stacked bodies 5 are separated from each other and overlapped in a plurality and subjected to a single nitriding treatment. Thus, the number of sheet-like molded bodies 5a subjected to nitriding treatment per unit time can be increased, and thus the manufacturing cost of the silicon nitride substrate can be reduced. Here, the number of stacked bodies 5 overlapped is 2 layers, but it can also be 3 layers or more depending on the space in the nitriding treatment furnace 1. In this case, as described above, it is also necessary to ensure that the interval between the overlapping stacked bodies 5 is greater than the prescribed distance (9.0 mm or more).

[0063] As described above. By setting the interval between the stacked bodies 5 when viewed from above to 9.0 mm or more, the heat of reaction is concentrated on the stacked bodies 5 during the heating process in the nitriding process, thereby preventing the sheet-like molded body 5a from melting. In addition, by setting the interval between the stacked bodies 5 when viewed from above to 35.0 mm or less, even in a nitriding furnace with a relatively low internal space height, the number of sheet-like molded bodies to be nitrided can be increased.

[0064] In addition, if Figure 1 As shown in FIG. 1 , by arranging a plurality of stacked bodies 5 in a direction perpendicular to the conveying direction when viewed from above, the manufacturing cost of the silicon nitride substrate can be reduced. Figure 4 As shown, each stack 5 is placed with its long side along the conveying direction ( Figure 4 The plurality of stacked bodies 5 arranged in the row direction are respectively conveyed in the direction along the long side direction thereof. Thus, the number of stacked bodies 5 arranged in the row direction on the conveyor 4 can be increased to the maximum (here, 4). Therefore, the number of sheet-like molded bodies 5a subjected to nitriding treatment per unit time is increased, and thus the manufacturing cost of the silicon nitride substrate can be reduced.

[0065] In addition, if Figure 5 As shown, it can also be considered that each stacked body 5 is arranged with its short side direction along the conveying direction ( Figure 5 The stacked bodies 5 are arranged on the conveyor 4 in the direction of the white arrow shown in FIG. 1 . That is, the plurality of stacked bodies 5 arranged in the row direction are conveyed in the direction along the short side direction thereof. By arranging the stacked bodies 5 in this way, the number of stacked bodies 5 arranged in the row direction on the conveyor 4 in the conveying direction, i.e., the longitudinal direction of the nitriding treatment furnace 1, can be increased to the maximum (here, 4). Therefore, the number of sheet-like molded bodies 5a subjected to nitriding treatment per unit time is increased, and thus the manufacturing cost of the silicon nitride substrate can be reduced.

[0066] Along the Figure 4 as well as Figure 5When the stack 5 is arranged in any direction, the interval L1 between adjacent stacks 5 in the column direction is 10 mm or more. In addition, in the conveying direction of the stack 5, the interval L2 between adjacent stacks 5 is also 10 mm or more. In this way. When viewed from above, by setting the intervals L1 and L2 between adjacent stacks 5 during conveyance to 10 mm or more, the reaction heat is concentrated on the stack 5 during the heating treatment of the nitriding process, and the melting of the sheet-like molded body 5a can be suppressed. The intervals L1 and L2 are more preferably 100 mm or more. By setting the intervals L1 and L2 to 100 mm or more, the reaction heat is concentrated on the stack 5 during the heating treatment of the nitriding process, and the melting of the sheet-like molded body 5a can be further suppressed. The intervals L1 and L2 are further preferably 200 mm or more. By setting the intervals L1 and L2 to be 200 mm or more, the reaction heat is concentrated on the laminate 5 during the heating process in the nitriding process, and melting of the sheet-like molded body 5a can be further suppressed, and deformation due to expansion of the sheet-like molded body 5a can be suppressed.

[0067] By the above method, a silicon nitride substrate as the present embodiment can be obtained. The nitridation rate of the silicon nitride substrate is 90% or more. More specifically, the nitridation rate of the silicon nitride substrate is 90% or more in both the central portion SC and the end portion SE in the top view of the silicon nitride substrate. The positions of the central portion SC and the end portion SE of the silicon nitride substrate mentioned here are the same as Figure 2 The positions of the center portion SC and the end portion SE of the sheet-like molded body 5a shown correspond to each other. The end portion SE is, for example, one of the four corners of the rectangular silicon nitride substrate, that is, a corner portion.

[0068] The nitridation rate of the silicon nitride substrate referred to in the present application is determined based on the following formula (1) from the silicon content of test pieces cut out from the central portion SC and the end portion SE of the silicon nitride substrate in a plan view, respectively, and measured by X-ray analysis.

[0069] Nitriding rate (%) = 100-Silicon (wt%)····(1)

[0070] For example, when the measured silicon content is 10 mass %, the nitridation rate is 90%, and when the measured silicon content is 0 mass %, the nitridation rate is 100%.

[0071] The silicon nitride substrate obtained in this manner has, for example, two main surfaces and four side surfaces, and the surface roughness Ra1 of one first main surface is 0.50 μm or less.

[0072] The silicon nitride substrate is rectangular in shape, preferably with each side being 100 mm or more. The thickness of the silicon nitride substrate is preferably 0.15 mm or more and 0.8 mm or less. The silicon nitride substrate has good thermal conductivity and is suitable for the above-mentioned uses, such as power modules and the like. Its thermal conductivity is preferably 100 W / m·K or more, more preferably 110 W / m·K or more, and further preferably 130 W / m·K or more. In the method for manufacturing a silicon nitride substrate having a nitriding process described in detail above, the purity of silicon nitride can be improved, so a silicon nitride substrate having a thermal conductivity of 110 W / m·K or more can be easily manufactured, which is preferred.

[0073] The laminated body 5 is a laminated body of sintered bodies formed by sintering the sheet-like molded bodies 5a through the subsequent sintering step. That is, a plurality of silicon nitride substrates as sintered bodies can be obtained from the laminated body.

[0074] The sintered silicon nitride substrate is mainly composed of β-phase silicon nitride and contains rare earth elements and magnesium. The rare earth elements can be in a single state or in a compound with other substances. The magnesium contained in the silicon nitride substrate can be in a single state or in a compound with other substances.

[0075] (1-4) Others

[0076] The silicon nitride substrate manufactured as described above preferably has a dense structure with a relative density of 98% or more. If the relative density of the silicon nitride substrate is less than 98%, a high thermal conductivity cannot be obtained. Such a dense silicon nitride substrate is less likely to be hindered by heat conduction due to voids, and in particular, the thermal conductivity of the silicon nitride substrate in the thickness direction of the present embodiment is preferably 110 W / m·K or more.

[0077] The thickness of the silicon nitride substrate is not particularly limited and can be any thickness. For example, when used as an insulating heat dissipation substrate for semiconductor elements and electronic devices, the thickness is preferably 0.05 mm or more and 2.5 mm or less, more preferably 0.1 mm or more and 1 mm or less, and particularly in the case of a silicon nitride circuit substrate for a power module, it is further preferably 0.2 mm or more and 0.7 mm or less. With regard to the thickness of the sintered silicon nitride substrate, the desired thickness can be adjusted by adjusting the thickness of the sheet molding in the sheet molding process in consideration of the effect on the thickness during sintering.

[0078] <Effects of the present embodiment>

[0079] In use Figure 1In the nitriding process in the nitriding furnace described above, for example, about 45 or more and about 90 or less sheet-like molded bodies are stacked in a mutually contacting manner in the height direction and carried into the nitriding furnace for heat treatment. The purpose of increasing the number of stacked sheet-like molded bodies in this way is to increase the number of sheet-like molded bodies that are nitrided per unit time and reduce the manufacturing cost of the silicon nitride substrate.

[0080] However, as described in the technical problem to be solved by the invention, in the nitriding process, if the number of stacked sheets of the sheet-like molded body becomes too large as described above, a chain reaction may occur due to the concentration of reaction heat, causing silicon to melt. This may cause problems in the appearance of the manufactured silicon nitride substrate and insufficient nitriding reaction in the substrate.

[0081] In addition, it is considered that after reducing the number of laminated sheets in one laminate of the sheet-like molded body, the laminated body formed by stacking two layers separated in the height direction is carried into the nitriding furnace for nitriding treatment. However, if the distance between the two stacked laminated bodies is too close, heat may accumulate during the nitriding treatment, causing silicon to melt.

[0082] Therefore, in the method for manufacturing a silicon nitride substrate of the present embodiment, the number of sheets of the sheet-like molded bodies 5a constituting one stack 5 is set within a range of 5 or more and 20 or less. In addition, the interval between the stacks 5 stacked when viewed from above is set to be 9.0 mm or more. Thus, the number of sheet-like molded bodies subjected to nitridation treatment per unit time is increased, the manufacturing cost of the silicon nitride substrate is reduced, and the reaction heat is prevented from being concentrated on the stack 5 during the heating treatment of the nitridation treatment step, thereby preventing the sheet-like molded bodies 5a from melting. Therefore, the productivity of the silicon nitride substrate can be improved.

[0083] In addition, the nitriding treatment is performed while conveying a plurality of stacked bodies 5 arranged in a direction intersecting the conveying direction, and at this time, the interval between adjacent stacked bodies 5 is set to be 10 mm or more when viewed from above. Thus, the number of sheet-like molded bodies subjected to nitriding treatment per unit time is increased, the manufacturing cost of the silicon nitride substrate is reduced, and the reaction heat is prevented from concentrating on the stacked bodies 5 during the heating treatment of the nitriding treatment step, thereby preventing the sheet-like molded bodies 5a from melting. Therefore, the productivity of the silicon nitride substrate can be improved.

[0084] (Example)

[0085] The present embodiment will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0086] (Slurry production process)

[0087] The BET specific surface area is 2.1 m 2 / g, a median particle size D50 of 8.2μm, and an oxygen content of 0.3% by mass, a total of 1.2mol% of Y2O3 powder and 9.8mol% of MgSiN2 powder were added as sintering aids relative to silicon (silicon nitride conversion), rare earth element oxides (trivalent oxide conversion) and magnesium compounds (MgO conversion) to obtain a raw material powder. A dispersion medium and a dispersant were added to the raw material powder to prepare a slurry with a concentration of 42% by mass, and the slurry was crushed for 24 hours using a ball mill using silicon nitride balls as the medium.

[0088] It should be noted that the amount of magnesium compound added is expressed as mol% when all magnesium compounds are converted to MgO. The BET specific surface area, median particle size D50 and oxygen content of the silicon powder before pulverization were measured using a BET specific surface area meter using a BET one-point method, a particle size distribution meter using a laser diffraction and scattering method, and an oxygen analyzer using an inert gas fusion-non-dispersive infrared absorption method.

[0089] (Sheet forming process)

[0090] The obtained slurry was added with a dispersion medium and an organic binder (acrylic resin) to adjust the concentration, and deaerated to prepare a slurry-like coating liquid. The coating slurry was applied to a transport film by a doctor blade method, and the molding speed was set to 600 mm / min or less to form a sheet with a thickness of 0.38 mm, which was cut into a size of 257 mm×191 mm to obtain a sheet-like molded body.

[0091] (Nitriding process)

[0092] The obtained sheet-like molded body had a boron nitride (BN powder) layer formed on the main surface. A laminated body 5 was prepared in which 15 sheet-like molded bodies were laminated with a boron nitride powder (BN powder) layer (thickness 4.5 μm) sandwiched therebetween. Figure 6 As shown in FIG. 1 , the housing 6A is formed by stacking six BN setters 6a at intervals. Here, the first stack 5 is placed on the surface of the lowest BN setter 6a, the second stack 5 is placed on the surface of the third BN setter 6a from the bottom, and the third stack 5 is placed on the surface of the fifth BN setter 6a from the bottom. That is, the stack 5 is stacked in three layers when viewed from above. The stacked stacks 5 are not connected to each other in the height direction (vertical direction), and are separated from each other at intervals of 28 mm.

[0093] use Figure 1 The nitriding furnace shown, Figure 7The stacked bodies 5 of the comparative example and the examples 1 and 2 were arranged as shown, and degreasing treatment and nitriding treatment were performed as follows. The stacked bodies were stacked body (1), stacked body (2), stacked body (3), and stacked body (4) in order from the inlet side of the nitriding treatment furnace. In addition, in the conveying direction of the stacked bodies 5, the interval L2 between adjacent stacked bodies 5 was 10 mm in the comparative example, 100 mm in the example 1, and 200 mm in the example 2. It should be noted that the nitriding treatment furnace used was a nitriding treatment furnace having a plurality of zones set in the nitriding treatment furnace. The nitriding treatment furnace was 330 mm wide, 7200 mm deep, and 110 mm high. The length of each zone was set to 450 mm and divided into 16 zones. From the inlet side, the 1st to 13th zones (1st to 13th zones) were set as heating zones, and the 14th to 16th zones (14th to 16th zones) were set as cooling zones. Here, the nitrogen supply pipes are provided in zones 1 to 16, and the internal atmosphere exhaust pipes are provided in zones 1 to 7. The supply pipes and the exhaust pipes are arranged below the device and above the device in a countercurrent manner with respect to the conveying direction of the sheet-like molded body.

[0094] As a heating mechanism of the nitriding treatment furnace, SiC heaters are provided in zones 1 to 13, and as a conveying mechanism, a roller conveyor is provided.

[0095] Using this nitriding treatment apparatus, nitriding treatment was performed under the conditions shown in Table 1. At this time, the holding time indicates the holding time at the nitriding temperature, and the pressure in the furnace was 15 to 20 Pa. In addition, the oxygen concentration in the nitriding treatment furnace was always controlled to be less than 1 ppm.

[0096] [Table 1]

[0097]

[0098] The evaluation results of the sheet-like molded body (nitride body) obtained after the nitriding process are summarized in Table 2. Observe the appearance of the nitride body to confirm whether silicon melting has occurred. That is, the white part is the completion of silicon nitriding to become silicon nitride, and the black part is the melting of silicon but the nitriding is not completed. In Table 2, ○ is the case where no black part caused by silicon melting is confirmed in any of the 15 nitride bodies stacked in each layer of each stack, △ is the case where the proportion of the black part in the area of ​​the nitride surface is less than 1%, and × is the case where the proportion of the black part in the area of ​​the nitride surface exceeds 1%. In addition, observe the appearance of the nitride body to confirm whether expansion has occurred. That is, a protrusion with a height of more than 100μm relative to the surface of the nitride body is regarded as expansion. In Table 2, ○ indicates a case where no protrusion caused by expansion is confirmed in any of the 15 nitride bodies stacked in each layer of each stack, △ indicates a case where the proportion of the protrusion in the area of ​​the nitride surface is less than 5%, and × indicates a case where the proportion of the protrusion in the area of ​​the nitride surface exceeds 5%.

[0099] [Table 2]

[0100]

[0101] In the comparative example, deformation due to melting of silicon and expansion of the substrate was observed in the laminates (1) to (4). In Example 1, melting of silicon was not observed in the laminates (1) to (4), and expansion of the nitride was observed in the first layer of the laminates (1) and (2). In Example 2, melting of silicon was not observed in the laminates (1) to (4), and slight expansion of the substrate was observed in the first layer of the laminates (1) and (4).

[0102] Therefore, from the viewpoint of suppressing melting of silicon, the interval between adjacent stacked bodies 5 is set to 100 mm or more. In addition, from the viewpoint of suppressing melting of silicon and suppressing deformation caused by expansion of nitride, the interval between adjacent stacked bodies 5 is more preferably 200 mm or more.

[0103] As mentioned above, the invention completed by the present inventors has been specifically described based on the embodiments thereof, but the present invention is not limited to the above-described embodiments, and various modifications can be made without departing from the gist of the invention.

[0104] The present invention can be widely used in a method for manufacturing a silicon nitride substrate.

[0105] Description of Reference Numerals

[0106] 1: nitriding treatment furnace (continuous heating furnace); 2: input port; 3: output port; 4: conveyor; 5: laminated body; 5a: sheet-shaped molded body; 6: shell; 6a: BN burner; 6b: BN frame.

Claims

1. A method for manufacturing a silicon nitride substrate, In a continuous heating furnace, a stacked body of sheet-shaped molded bodies containing silicon and stacked in a number of not less than 5 and not more than 20 sheets is conveyed from an input port to an output port, thereby performing nitridation. The continuous heating furnace includes the input port and the output port, a heating mechanism for heating between the input port and the output port, and a nitrogen supply mechanism for supplying nitrogen between the input port and the output port. The stacked bodies are transported in a state where a plurality of the stacked bodies are arranged in a first direction intersecting the transport direction when viewed from above. When viewed from above, the interval between the adjacent stacked bodies during transportation is 100 mm or more.

2. The method for manufacturing a silicon nitride substrate according to claim 1, wherein: A plurality of the stacked bodies are stacked in a height direction, The interval between the stacked layers in the height direction is 9.0 mm or more.

3. The method for manufacturing a silicon nitride substrate according to claim 1, wherein: The planar shape of the stacked body is a rectangle having a first long side and a first short side, The plurality of stacked bodies arranged in the first direction are respectively conveyed in a direction along the first long side.

4. The method for manufacturing a silicon nitride substrate according to claim 1, wherein: The planar shape of the stacked body is a rectangle having a first long side and a first short side, The plurality of stacked bodies arranged in the first direction are respectively conveyed in a direction along the first short side.

5. The method for manufacturing a silicon nitride substrate according to claim 1, wherein: The planar shape of the stacked body is a rectangle having a first long side and a first short side, The length of the first short side is greater than 100 mm.

6. The method for manufacturing a silicon nitride substrate according to claim 1, wherein: The sheet-like molded body has a thickness of 0.05 mm or more and 2.5 mm or less.

7. The method for manufacturing a silicon nitride substrate according to claim 1, wherein: By sintering the nitrided stacked body, a plurality of stacked sintered bodies are obtained.

8. The method for manufacturing a silicon nitride substrate according to claim 1, wherein: The nitridation rate of the sheet-like molded body after nitridation is 90% or more.

9. The method for manufacturing a silicon nitride substrate according to claim 7, wherein: The planar shape of the sintered body is a rectangle having a second long side and a second short side, The length of the second short side is greater than 100 mm.

10. The method for manufacturing a silicon nitride substrate according to claim 7, wherein: The sintered body has a thickness of 0.15 mm or more and 0.8 mm or less.

Citation Information

Patent Citations

  • Automatic heating device for heat treatment

    CN103352109A

  • Ferrite sheet having thickness of more than 200 [mu]m, preparation method and use thereof

    CN109545496A

  • Silicon nitride substrate production method and silicon nitride substrate

    CN112912356A

  • Transistor device with metal gate cut and recessed power rail

    CN113380880A

  • Silicon nitride substrate, silicon nitride substrate evaluation method, silicon nitride substrate evaluation device, silicon nitride substrate evaluation system, and silicon nitride circuit substrate

    CN116660236A