Water-based adhesive compositions and related methods
By using a composition of water-soluble polymer with high weight average molecular weight and polymer binder, the filaments are generated, and the bonding effect and environmental pollution problems during spraying of water-based binder are solved, and better bonding is achieved Strength and permeability.
Patent Information
- Application Number
- CN202380030004.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-26
AI Technical Summary
Existing water-based adhesives are difficult to form filaments when spraying, resulting in poor bonding effects and excessive spraying and environmental pollution problems.
A water-soluble polymer with a weight average molecular weight of at least 90,000 g/mol is combined with a polymer binder to form a composition comprising water, a polymer binder dispersed in water and a water-soluble polymer dissolved in water by spraying Technology generates filaments.
Achieve better permeability and reduce overspraying, improve bond strength and environmental friendliness, suitable for textured surfaces and a variety of bonding applications.
Smart Images

Figure BDA0005057361320000211 
Figure BDA0005057361320000241 
Figure HDA0005057361330000011
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. Provisional Application No. 63 / 323,191, filed on March 24, 2022, the disclosure of which is incorporated herein by reference in its entirety. Background Art
[0003] Pressure sensitive adhesives (often referred to as PSAs) can be used for a variety of purposes. Applying a PSA can involve applying the adhesive polymer composition to a substrate in an organic solvent or as an oil-in-water emulsion and subsequently removing the solvent or water. Water-based adhesives have significant advantages over their traditional solvent-based counterparts in that they can have low or no volatile organic compounds and can be non-flammable.
[0004] Some references disclosing water-based adhesives and / or water-soluble polymers are disclosed in International Patent Application Publication No. WO 2020 / 169661, published on August 27, 2020; U.S. Patent Nos. 7,851,522 (Hardy et al.), 7,067,189 (Huynh-Tran et al.), and 6,168,781 (Ukaji et al.); and U.S. Patent Application Publication No. 2021 / 0071049 (Unverhau et al.). Filament-forming aerosols for artificial hair or insect capture are disclosed in Japanese Patent Application No. 2008 / 231652, published on October 2, 2008. Summary of the invention
[0005] The present disclosure provides a composition comprising a polymer binder and a water soluble polymer in water. When sprayed, the composition provides filaments, which may be superior to fine mist sprays when used on, for example, textured surfaces.
[0006] In one aspect, the present disclosure provides a composition comprising water, a polymer binder dispersed in the water or the composition and a water-soluble polymer dissolved in the water or the composition. The weight average molecular weight of the water-soluble polymer is at least 90,000 grams per mole. Typically and advantageously, after the composition is sprayed, the composition provides a filament comprising the polymer binder and the water-soluble polymer. In some embodiments, the filament is a pressure-sensitive adhesive filament.
[0007] In another aspect, the present disclosure provides a composition for use as a spray adhesive composition. The composition comprises water, a polymer binder dispersed in the water or the composition, and a water-soluble polymer having a weight average molecular weight of at least 90,000 g / mole dissolved in the water or the composition.
[0008] In another aspect, the present disclosure provides a composition for use as a filament spray binder. The composition comprises water, a polymer binder dispersed in the water or the composition, and a water-soluble polymer having a weight average molecular weight of at least 90,000 g / mole dissolved in the water or the composition.
[0009] In the above uses, upon spraying the composition, the composition generally provides filaments comprising the polymeric binder and the water-soluble polymer. In some embodiments, the filaments are filaments that are pressure-sensitive adhesive filaments.
[0010] In another aspect, the present disclosure provides a method of using a composition comprising water, a polymer binder dispersed in the water or the composition, and a water-soluble polymer dissolved in the water or the composition. The weight average molecular weight of the water-soluble polymer is at least 90,000 g / mol. The method includes spraying the composition to provide a filament comprising a polymer binder and a water-soluble polymer. In some embodiments, the filament is a pressure-sensitive adhesive filament.
[0011] In another aspect, the present disclosure provides a method of preparing the composition. The method includes mixing components of a solution comprising the water-soluble polymer dissolved in at least a portion of the water with an emulsion of the polymer binder.
[0012] In another aspect, the present disclosure provides a method for preparing a bonded article, the bonded article comprising a first substrate and a second substrate. The method comprises spraying the above composition to provide filaments comprising a polymer binder and a water-soluble polymer on at least one of the first substrate or the second substrate, and using the filaments to bond the first substrate and the second substrate.
[0013] In the present application, terms such as "one", "a kind of" and "the / said" are not intended to refer to only a single entity, but rather to general categories that include specific examples that can be used for illustration. The terms "one", "a kind of", "the" and "said" can be used interchangeably with the term "at least one (kind)". The phrases "at least one (kind) of..." and "comprising at least one (kind) of..." followed by a list refer to any one of the items in the list and any combination of two or more items in the list. Unless otherwise indicated, all numerical ranges include their end values and non-integer values between the end values (e.g., 1 to 5 includes 1, 1.5, 2, 2.75, 3, 3.8, 4, and 5, etc.).
[0014] The terms "first" and "second" are used in the present disclosure only in their relative sense. It should be understood that, unless otherwise indicated, these terms are used only for convenience in describing one or more of the embodiments.
[0015] As used herein, the term "acrylic" or "acrylate" includes compounds having at least one of an acrylic acid or a methacrylic acid group.
[0016] The term "(meth)acrylic" with respect to a monomer, oligomer or polymer means a vinyl functional alkyl ester formed as the reaction product of an alcohol and acrylic acid or methacrylic acid.
[0017] The term "(co)polymer" or "(co)polymerized" includes homopolymers and copolymers, as well as homopolymers and copolymers that can be formed in a miscible blend (e.g., by coextrusion or by reactions including, for example, transesterification reactions). The term "copolymer" includes random copolymers, block copolymers, graft copolymers, and star copolymers.
[0018] The term "crosslinking" refers to joining polymer chains together by covalent chemical bonds (usually via crosslinking molecules or groups) to form a polymer network. Crosslinked polymers are generally characterized by insolubility, but may be swellable in the presence of appropriate solvents.
[0019] "Alkyl groups" and the prefix "alk-" are inclusive of straight and branched chain groups as well as cyclic groups. In some embodiments, unless otherwise indicated, alkyl groups have up to 30 carbons (in some embodiments, up to 25, 20, 18, 16, or 15 carbons). Cyclic groups can be monocyclic or polycyclic.
[0020] The term "hydrocarbon" refers to a chemical compound having only carbon and hydrogen atoms.
[0021] The above summary of the present disclosure is not intended to describe each disclosed embodiment or each implementation of the present disclosure. The following description illustrates exemplary embodiments in more detail. Therefore, it should be understood that the drawings and the following description are only for illustrative purposes and should not be construed as undue limitations on the scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The present disclosure can be more fully understood with reference to the following detailed description of various embodiments of the present disclosure in conjunction with the accompanying drawings, in which:
[0023] Figure 1 is a graphic representation of the mist spray described in the Examples section;
[0024] Figure 2 is a graphic representation of the pebble spray described in the Examples section; and
[0025] Figure 3 is a graphic representation of the sprayed filaments observable in the compositions of the present disclosure and described in the Examples. DETAILED DESCRIPTION
[0026] It is known that certain solvent-based adhesives produce filaments when sprayed. We have found that such adhesive filaments tend to be very suitable for rough or textured surfaces of applications such as construction or foam bonding, while fine mist adhesives can be used for smooth surfaces, lamination, and other types of thin coating applications. Adhesives that produce filaments also tend to have low overspray, which can result in higher transfer of adhesive to substrates and less waste and environmental pollution.
[0027] We have observed that solvent-based adhesives and water-based adhesives behave differently when spraying. Water-based adhesives tend to produce fine mist when spraying. Adhesive polymers are usually at least partially soluble solvents and are easily entangled in solution, which can provide some resistance to breaking into small droplets when the adhesive is sprayed for the adhesive polymer. Low boiling point solvents are usually used, and solvent evaporation can induce some drying of the adhesive during spraying, thereby further preventing the formation of small droplets. Without being bound by theory, for at least the following reasons, we believe that it is quite challenging to realize these phenomena in water-based adhesive systems. Many adhesive polymers are insoluble in water, and water-based adhesives are usually latex materials or colloidal suspensions of discrete particles with limited interaction. Compared with solvents that are usually used for adhesive spraying, water has a higher boiling point and a lower vapor pressure, and will not evaporate in an amount sufficient to promote the formation of filaments during spraying.
[0028] The present disclosure provides water-based compositions, which are usually and advantageously formed into filaments rather than fine mists when sprayed. The composition comprises water, a polymer binder dispersed in water, and a water-soluble polymer dissolved in water. Although the present disclosure is not bound by theory, it is believed that a water-soluble polymer having a weight average molecular weight of at least 90,000 g / mol imparts enough entanglement to keep the polymer filaments together during spraying. The adhesive filaments have advantages for some applications, including better penetration into the substrate and reduced overspray.
[0029] In some embodiments, the long filament comprising a polymer binder and a water-soluble polymer is a pressure sensitive adhesive (PSA) filament. It is well known to those of ordinary skill in the art that PSA has the following properties: (1) powerful and lasting tackiness, (2) can adhere with a pressure not exceeding finger pressure, (3) has the ability to be enough to remain on the adherend, and usually, (4) has enough cohesive strength to be cleanly removed from the adherend. PSA is viscous and has the ability to adhere when not activated by any energy source (such as light, heat or chemical reaction). It has been found that the material that can be used well as PSA is such a polymer, which is designed and formulated to show required viscoelasticity, thereby obtaining the desired balance of adhesion, peel adhesion and shear holding power. A method that can be used to identify pressure sensitive adhesives is Dahlquist criterion. As described in Handbook of Pressure Sensitive Adhesive Technology, Donatas Satas, ed., 2nd ed., p. 172, Van Nostrand Reinhold, New York (NY), 1989, this criterion defines a pressure sensitive adhesive as having a pressure greater than 3×10 -6 cm 2 Alternatively, since modulus is roughly the inverse of creep compliance, a pressure sensitive adhesive may be defined as having a storage modulus of less than about 3×10 5 N / m 2 Adhesive.
[0030] The present disclosure and / or compositions that can be used to practice the present disclosure include water and a polymer binder dispersed in the water or the composition. "Dispersed" means that the polymer binder in the water is a heterogeneous mixture of discrete particles or droplets in water. "Dispersed" does not cover "dissolved". Therefore, generally, the polymer binder is insoluble in water (that is, the solubility at 20°C is less than 5 grams (g) / liter, less than 1g / liter or less than 0.5g / liter). The polymer binder can be liquid or solid in water. Therefore, the dispersion of the polymer binder in water can be an emulsion, latex or colloidal suspension. The example of the available polymer binder that can be dispersed in water includes acrylic polymers, natural rubber, synthetic polyisoprene, polybutadiene, styrene / butadiene rubber (SBR), styrene / isoprene / butadiene rubber and nitrile rubber. Various main chain geometries and connectivity can be present in these polymers, such as in polybutadiene and polyisoprene, a large amount of cis geometries can be present. The combination of two or more polymer binders in these polymer binders may be present in compositions, such as natural rubber and SBR. In some embodiments, the polymer binder includes at least one of the following: a copolymer of at least one of acrylic polymer, natural rubber or styrene and isoprene or butadiene. In some embodiments, the polymer binder includes at least one of SBR or acrylic polymer. The polymer binder dispersed in water does not include water-soluble polymers, such as starch.
[0031] The weight average molecular weight (Mw) of the polymer binder can range, for example, from 10,000 to 1,000,000 g / mole, from 50,000 to 500,000 g / mole, or from 50,000 to 200,000 g / mole as determined by gel permeation chromatography using polystyrene standards.
[0032] The particle size or droplet size of the polymer binder dispersed in water can be in the range of 50 nanometers (nm) to 10 microns, 50 nanometers to 5 microns, or 200 nanometers to 500 nanometers, as measured by dynamic light scattering measurements, which is a technique known to those skilled in the art of aqueous dispersions. In some embodiments, the droplet size or particle size is 500 nm or less, 400 nm or less, or 300 nm or less. In some embodiments, the droplet size or particle size is at least 50 nm, at least 100 nm, or at least 130 nm.
[0033] In some embodiments, polymer binder comprises acrylic copolymer.As used herein, " acrylic " and similar terms are intended to cover both acrylate and methacrylate.Multiple acrylic polymers can be used in said composition.In some embodiments, acrylic polymer is made of hydrophobic acrylic monomers, and these hydrophobic acrylic monomers comprise acrylate and / or methacrylate of the straight or branched alcohol with at least 4 carbon atoms (in some embodiments, 4 to 14 carbon atoms, 4 to 10 carbon atoms, 4 to 8 carbon atoms or 6 to 8 carbon atoms).The example of this monomer that is suitable for using in acrylic polymer comprises isooctyl acrylate, 4-methyl-2-pentyl acrylate, 2-methylbutyl acrylate, isopentyl acrylate, sec-butyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, isodecyl methacrylate, isononyl acrylate, isodecyl acrylate, and their mixture. Other suitable monomers for preparing acrylic polymers include at least partially hydrophilic monomers, such as acrylic acid, methacrylic acid, fumaric acid, maleic acid, itaconic acid, crotonic acid, oligomeric acrylic acid, 2-hydroxyethyl acrylate, (methyl) methyl acrylate, (methyl) ethyl acrylate, N-vinyl-2-pyrrolidone and mixtures thereof. Based on the gross weight of the monomer for preparing acrylic polymers, such hydrophilic monomers are usually used in an amount of up to 2 % by weight, 1 % by weight or 0.5 % by weight. If there is an acid functional group in the acrylic polymer, they can be neutralized using, for example, amines (for example, dimethylethanolamine, ammonia, triethanolamine, dimethylethylethanolamine and N', N'-dimethylaminopropylamine) or alkali metal salts (for example, sodium hydroxide or potassium hydroxide). Other monomers can be effectively incorporated into the acrylic polymer, such as styrene, vinyl toluene, nitrile (for example, acrylonitrile and methacrylonitrile), vinyl and vinylidene halides and vinyl esters (for example, vinyl acetate).
[0034] In addition to the acid-functional monomers, the acrylic polymer may further include monomer units of other polar monomers, including at least one ketone, amide, amine, alcohol, or combination thereof. Examples of polar monomers with hydroxyl groups include: hydroxyalkyl (meth) acrylates (e.g., 2-hydroxyethyl (meth) acrylate, 2-hydroxypropyl (meth) acrylate, 3-hydroxypropyl (meth) acrylate, and 4-hydroxybutyl (meth) acrylate), hydroxyalkyl (meth) acrylamides (e.g., 2-hydroxyethyl (meth) acrylamide or 3-hydroxypropyl (meth) acrylamide), ethoxylated hydroxyethyl (meth) acrylates (e.g., monomers commercially available from Sartomer (Exton, PA, USA) under the trade names CD570, CD571, and CD572) and aryloxy-substituted hydroxyalkyl (meth) acrylates (e.g., 2-hydroxy-2-phenoxypropyl (meth) acrylate). Examples of polar monomers with primary amide groups include (meth) acrylamide. Examples of polar monomers with secondary amide groups include N-alkyl (meth) acrylamides, such as N-methyl (meth) acrylamide, N-ethyl (meth) acrylamide, N-isopropyl (meth) acrylamide, N-tert-octyl (meth) acrylamide or N-octyl (meth) acrylamide. Examples of polar monomers with tertiary amide groups include N-vinyl caprolactam, N-vinyl-2-pyrrolidone, (meth) acryl morpholine, and N, N-dialkyl (meth) acrylamides (such as N, N-dimethyl (meth) acrylamide, N, N-diethyl (meth) acrylamide, N, N-dipropyl (meth) acrylamide, and N, N-dibutyl (meth) acrylamide). Polar monomers with amino groups include various (meth) acrylic acid N, N-dialkylaminoalkyl esters and N, N-dialkylaminoalkyl (meth) acrylamides. Examples include N,N-dimethylaminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylamide, N,N-dimethylaminopropyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylamide, N,N-diethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylamide, N,N-diethylaminopropyl (meth)acrylate, and N,N-diethylaminopropyl (meth)acrylamide. Examples of polar monomers containing ketones include diacetone acrylamide and acetoacetoxyethyl methacrylate. In some embodiments, no more than 2% by weight, 1% by weight, 0.5% by weight, 0.25% by weight, 0.1% by weight, 0.05% by weight, or 0.01% by weight of monomer units in the acrylic polymers that can be used in the compositions and methods of the present disclosure include at least one ketone, amide, amine, alcohol, or a combination thereof. The acrylic polymer may be free of polar monomer units.
[0035] Crosslinked acrylic polymer adhesive can be prepared, for example, by including one or more multifunctional crosslinking monomers (for example, multifunctional acrylate or multifunctional methacrylate) in the monomer for preparing the polymer. Suitable multifunctional monomers include the diacrylates of glycols, such as ethylene glycol diacrylate, diethylene glycol diacrylate, propylene glycol diacrylate, butanediol diacrylate, butane-1,3-diyl diacrylate, pentanediol diacrylate, hexanediol diacrylate (including 1,6-hexanediol diacrylate), heptanediol diacrylate, octanediol diacrylate, nonanediol diacrylate, decanediol diacrylate and the dimethacrylate of any of the aforementioned diacrylates. Other suitable multifunctional monomers include the polyacrylates of polyols, such as glycerol triacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, neopentyl glycol diacrylate, dipentaerythritol pentaacrylate, the methacrylate of the aforementioned acrylates and combinations thereof. Other suitable multifunctional crosslinking monomers include divinylbenzene, allyl methacrylate, diallyl maleate, diallyl phthalate and combinations thereof. Further suitable multifunctional crosslinking monomers include multifunctional acrylate oligomers comprising two or more acrylate groups. Multifunctional acrylate oligomers can be methacrylates of carbamate acrylate oligomers, epoxy acrylate oligomers, polyester acrylates, polyether acrylates, polyacrylic acid acrylates, any of the aforementioned acrylates, or combinations thereof. The combination of any crosslinking monomer in these crosslinking monomers can be available. In some embodiments, monomer units that are no more than 1 % by weight, 0.5 % by weight, 0.25 % by weight, 0.1 % by weight, 0.05 % by weight or 0.01 % by weight in the acrylic polymers that can be used in the compositions and methods of the present disclosure are derived from crosslinking monomers. Acrylic polymers can be free of crosslinking monomer units.
[0036] Other cross-linked monomer units may be present in the acrylic polymer used as a polymer binder. In some embodiments, the acrylic polymer can be cross-linked after removing water. For example, N-hydroxymethyl acrylamide (NMA) is a monomer that can be used to introduce N-hydroxymethyl groups into the acrylic polymer. The hydroxymethyl group of an acrylic polymer chain can react with the hydroxymethyl group of another acrylic polymer chain, wherein formaldehyde and water molecules are cut to provide cross-linking. The degree of unsaturation in silane (such as vinyl silane and methacryloxy silane) allows to be incorporated into the acrylic polymer chain. After the coating is dried, pH declines and triggers alkoxysilane to hydrolyze into silanol (Si-OH), which is then combined with the available second silanol on the polymer chain and forms siloxane (Si-O-Si) key. The acrylic monomer (for example, diacetone acrylamide, acrolein, vinyl methyl ketone, methacrylic acid acetoacetoxyethyl ester and allyl acetoacetate) comprising aldehyde and / or ketone functional groups can react with a cross-linking agent, which has at least two functional groups reactive to the carbonyl functional group of the acrylic copolymer. Any nitrogen-containing compound with at least two amine nitrogens that can react with carbonyl groups can be used as a crosslinking agent. Such crosslinking agents can be aliphatic or aromatic, polymeric or non-polymeric, and can be used alone or in combination of two or more. The example of a suitable crosslinking agent includes adipic acid dihydrazide, diamines (for example, ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine) and tetraaminoethylene. In some embodiments, the crosslinking agent is present in the composition in an amount in the range of 0.02 equivalent to 5 equivalents, 0.1 equivalent to 3 equivalents or 0.5 equivalent to 2 equivalents of the carbonyl groups contained in the acrylic polymer per equivalent. In some embodiments of the composition of the present disclosure, after the composition is applied to the substrate and as the water in the emulsion evaporates, the hydrazide group and the carbonyl group are crosslinked to form a solidified filament due to dehydration condensation.
[0037] The polymer binder dispersed in water can be prepared, for example, by emulsion polymerization in which monomers (such as any of those described above) are polymerized in water, optionally in the presence of an emulsifier, a catalyst, and / or a chain transfer agent (e.g., carbon tetrabromide, alcohols, mercaptans such as, for example, isooctyl thioglycolate, and mixtures thereof).
[0038] In some embodiments, the acrylic polymer that can be used as a polymer binder is a core-shell polymer with different monomer compositions in the core and shell. For example, the core-shell polymer can be prepared by emulsion polymerization, in which the monomer composition is changed during polymerization to provide polymer particles with different glass transition temperatures or different reactivities between the core and shell. Examples of core-shell polymers that can be used as polymer binders include those described in U.S. Patent Nos. 5,461,125 (Lu et al.) and 10,221,343 (Qie et al.).
[0039] The above-mentioned various polymer binders can have different pH values, at which they are useful. For example, natural rubber emulsion can be available at, for example, pH 13 or 14. In some embodiments, the composition of the present disclosure further comprises an alkali, for example, to increase the pH. In some embodiments, the pH is increased to at least 7, 8, 9, 10, 11, 12, or 13. The example of a suitable alkali includes ammonia (e.g., aqueous ammonia or ammonium hydroxide), ethanolamine, sodium hydroxide, triethylamine, and sodium carbonate.
[0040] Some acrylic polymers useful in practicing the present disclosure are commercially available, for example, as emulsions under the trade designations “AC 2403,” “AC 3630,” and “AC 2514” from Alberdingk Boley, Greensboro, NC; under the trade designations “RHOPLEX” grades “AC-1034,” “GL-618,” and CS-4000 from Dow, Midland, Mich.; and under the trade designation “CARBOSETGA 7487” from The Lubrizol Corporation, Wickliffe, Ohio. Corporation, Wickliffe, Ohio); under the trade designation "ACRONAL" from BASF, Ludwigshafen, Germany; and under the trade designation "ENCOR" from Arkema, King of Prussia, PA.
[0041] Some natural rubber polymers and SBR polymers useful in practicing the present disclosure are commercially available, for example, as emulsions under the trade designation "ALCANTEX" from Alcan Rubber and Chemical, New York, NY and under the trade designation "BUTOFAN" from BASF.
[0042] Depending on the amount of any of the water-soluble polymers and tackifiers and other additives described below, in some embodiments, the compositions of the present disclosure may include at least 70 wt%, 75 wt%, 80 wt%, 90 wt%, 95 wt%, 98 wt%, or 99 wt% of the polymer binder described above in any of its embodiments, based on the total amount of solids in the composition (i.e., excluding water). In some embodiments, the polymer binder is present in the composition in an amount of at least 25 wt% or no more than 75 wt%, based on the total weight of the composition (i.e., including water).
[0043] The compositions of the present disclosure and / or compositions that can be used to practice the present disclosure include water-soluble polymers that are dissolved in water or the compositions. As used herein, the term water-soluble polymer refers to a polymer having a solubility of at least 5 grams (g) / liter of water per liter of water at 20°C. In some embodiments, the solubility of the water-soluble polymer at 20°C is at least 10 g / liter of water, 15 g / liter of water, 20 g / liter of water, 25 g / liter of water, 50 g / liter of water, or 100 g / liter of water. In some embodiments, the solubility of the water-soluble polymer at 20°C or higher temperatures is up to 1000 g / liter of water.
[0044] The weight average molecular weight of the water-soluble polymer is at least 90,000 grams per mole (g / mol), as measured by gel permeation chromatography in water relative to poly (methacrylic acid) standards, relative to polystyrene standards, or using the methods described in the following examples. Such water-soluble polymers have enough entanglements so that when the composition of the present disclosure is sprayed, a filament comprising a polymer binder and a water-soluble polymer is formed. In some embodiments, the weight average molecular weight of the water-soluble polymer is at least 95,000 g / mol, 100,000 g / mol, 125,000 g / mol, or 150,000 g / mol. In some embodiments, the weight average molecular weight of the water-soluble polymer is no greater than 9,000,000 g / mol, 8,000,000 g / mol, 7,000,000 g / mol, 6,000,000 g / mol, 5,000,000 g / mol, 4,000,000 g / mol, 3,000,000 g / mol, 2,000,000 g / mol, or 1,000,000 g / mol. When the weight average molecular weight of the water-soluble polymer is less than 90,000 g / mol, the water-soluble polymer may not have sufficient entanglement to provide filaments comprising a polymeric binder and a water-soluble polymer when the composition is sprayed. When the weight average molecular weight of the water-soluble polymer is greater than 9,000,000 g / mol, the water-soluble polymer may provide filaments that are too thick and sparse to provide good coverage of the polymeric binder when the composition is sprayed on a substrate.
[0045] In some embodiments, the water-soluble polymer includes at least one of polyacrylamide, poly(ethylene oxide), poly(vinyl pyrrolidone), polyvinyl alcohol, or polyvinyl acetate. Such polymers can be obtained from various commercial sources at various molecular weights. For example, suitable commercially available water-soluble polymers include polyvinyl alcohol purchased from Kuraray, Okayama, Japan; polyacrylamide purchased from Kemira, Helsinki, Finland; poly(ethylene oxide) purchased from DuPont, Collegeville, PA, and polyvinyl acetate purchased from Wacker Chemical Corporation, Ann Arbor, MI, under the trade name "VINNAPAS". In some embodiments, the water-soluble polymer includes at least one of polyacrylamide, poly(ethylene oxide), or poly(vinyl pyrrolidone). In some embodiments, the water-soluble polymer comprises at least one of polyacrylamide or poly(ethylene oxide). In some embodiments, the water-soluble polymer comprises anionic and / or cationic groups. That is, the water-soluble polymer can be anionic, cationic, or both (i.e., amphoteric). In some embodiments, the water-soluble polymer does not comprise a cationic group. In some embodiments, the water-soluble polymer is nonionic. According to U.S. Patent No. 10,113,006 (Rissanen et al.), microfibrillated cellulose is not water-soluble. In some embodiments, the water-soluble polymer is not cellulose.
[0046] In some embodiments, the water-soluble polymer is present in the composition in an amount of at least 0.05 % by weight (wt.%) or not more than 5 % by weight based on the total weight of the composition. In some embodiments, the water-soluble polymer is present in the composition in an amount of at least 0.05 % by weight, 0.075 % by weight or 0.1 % by weight based on the total weight of the composition. In some embodiments, the water-soluble polymer is present in the composition in an amount of not more than 5 % by weight, 4 % by weight, 3 % by weight, 2.5 % by weight, 2 % by weight or 1.5 % by weight based on the total weight of the composition. In some embodiments, if the water-soluble polymer is present in the composition in an amount less than 0.05 % by weight, the filaments comprising polymer binder and water-soluble polymer may not be provided when the composition is sprayed. In some embodiments, if the water-soluble polymer is present in the composition in an amount greater than 5 % by weight, it can negatively affect the bonding strength of the adhesive formed by the composition.
[0047] In some embodiments of the present disclosure and / or compositions that can be used to practice the present disclosure, the composition further comprises a tackifier. In some embodiments, the tackifier comprises at least one of rosin, rosin esters, esters of hydrogenated rosin, polyterpenes (e.g., those based on α-pinene, β-pinene or limonene), aliphatic hydrocarbon resins (e.g., those based on cis- or trans-piperylene, isoprene, 2-methyl-but-2-ene, cyclopentadiene, dicyclopentadiene or combinations thereof), aromatic resins (e.g., based on styrene, α-methylstyrene, methylindene, indene, coumarone or combinations thereof) or mixed aliphatic-aromatic hydrocarbon resins. In some embodiments, the tackifier comprises at least one of rosin, rosin esters, esters of hydrogenated rosin, aliphatic hydrocarbon resins, aromatic resins or mixed aliphatic-aromatic hydrocarbon resins. The aromatic hydrocarbon resin may be a C9 type petroleum resin obtained by copolymerizing the C9 fraction produced by the thermal decomposition of naphtha, and the aliphatic hydrocarbon resin may be a C5 type petroleum resin obtained by copolymerizing the C5 fraction produced by the thermal decomposition of naphtha. The mixed aliphatic / aromatic resin may be a C5 / C9 type petroleum resin obtained by polymerizing a combination of a C5 fraction and a C9 fraction produced by the thermal decomposition of naphtha. Any of these tackifying resins may be hydrogenated (e.g., partially or completely). The term rosin as used herein includes: refined or unrefined natural rosin (refined rosin will generally contain about 90% by weight rosin acid and about 10% by weight inert matter), such as log board rosin, natural gum rosin, and tall oil rosin; refined or unrefined modified rosin, such as disproportionated rosin, hydrogenated rosin, polymerized rosin; and pure or substantially pure acid containing rosin, alone or in a mixture. In some embodiments, the tackifier is a hydrocarbon tackifier. In some embodiments, useful tackifiers have a number average molecular weight of up to 10,000 g / mole, a softening point of at least 30° C. (as determined using a ring and ball instrument), and a glass transition temperature of at least −30° C. (as determined by differential scanning calorimetry). Useful tackifiers are generally amorphous. In some embodiments, the tackifier is miscible with the polymer binder of the composition such that macroscopic phase separation does not occur in the composition. In some embodiments, a combination of tackifiers can be used to obtain a good balance of compatibility and adhesive properties (e.g., high temperature performance).
[0048] Examples of suitable tackifiers include those available under the trade designations "FORAL 85E" (a glycerol ester of highly hydrogenated refined gum rosin) from Eastman, Middelburg, NL; "FORAL 3085" (a glycerol ester of highly hydrogenated refined wood rosin) from Pinova, Brunswick, GA; "ESCOREZ 2520" and "ESCOREZ 5615" (aliphatic / aromatic hydrocarbon resins) available from ExxonMobil Corp., Houston, TX; "REGALITE 7100" (partially hydrogenated hydrocarbon resin), available from Eastman, Kingsport, Tennessee; and fully and partially hydrogenated hydrocarbon tackifiers available from Arakawa, Osaka, Japan, under the trade designation "ARKON". Some suitable tackifiers are available as emulsions from Eastman Chemical, Kingsport, Tennessee, under the trade designation "TACOLYN" and from Kraton Corporation, Houston, TX, under the trade designation "AQUATAC".
[0049] In some embodiments, the tackifier is present in the composition in a range of 2 to 30 parts by weight per hundred parts of polymeric binder. In some embodiments, the tackifier is present in a range of 2 to 25 parts, 2 to 20 parts, 5 to 25 parts, 10 to 25 parts, 10 to 20 parts, 2 to 15 parts, or 2 to 10 parts by weight per hundred parts of polymeric binder.
[0050] In some embodiments, the present disclosure and / or compositions that can be used to practice the present disclosure further include an emulsifier. In the compositions of the present disclosure, there is usually an emulsifier for emulsion polymerization to form a polymer binder. In some embodiments, the emulsifier is an anionic surfactant. Available anionic surfactants include those surfactants comprising the following: at least one hydrophobic part (such as alkyl, alkylaryl and / or alkenyl groups of about 6 carbon atoms to about 12 carbon atoms) and at least one anionic group selected from carboxylate, sulfate, sulfonate, phosphate, polyoxyethylene sulfate, polyoxyethylene sulfonate, polyoxyethylene phosphate and / or the salt of such anionic groups (such as alkali metal salts (such as sodium salts, potassium salts) and ammonium salts). Any fatty acid soap (for example, alkyl succinate), ethoxylated fatty acid and / or its alkali metal salt ammonium salt, dialkyl sulfosuccinate and sulfated oil can be useful. Some useful anionic surfactants include sodium lauryl sulfate, sodium lauryl ether sulfate, sodium dodecylbenzene sulfonate and sulfosuccinate. Representative commercially available examples of anionic surfactants include sodium lauryl sulfate, available under the trade name "POLYSTEP B-3" from Stepan Chemical Co.; sodium lauryl ether sulfate, available under the trade name "POLYSTEP B-12" from Stepan Chemical Co.; and sodium dodecylbenzene sulfonate, available under the trade name "RHODACAL DS-10" from Rhodia, Incorporated. Combinations of any of these surfactants may be used.
[0051] In some embodiments, emulsifier can be copolymerized with monomer or monomer mixture, and become incorporated into polymer binder.This copolymerizable emulsifier has at least one group or only one group that can react with monomer or monomer mixture.Such reactive groups include ethylenically unsaturated groups such as vinyl and acrylate groups.The example of polymerizable emulsifier includes sodium styrene sulfonate (available from Alfa Aesar), sodium vinyl sulfonate, sodium polystyrene sulfonate, polyoxyethylene alkyl phenyl ether ammonium sulfate (available from Montello, Inc., Kyoto, Japan with trade name "HITENOL BC"), including polyoxyethylene-nonyl propenyl phenyl ether ammonium sulfate, polyoxyethylene styrenated phenyl ether ammonium sulfate (such as available from Montello with trade name "HITENOL AR") and polyoxyethylene alkyl ether sulfate (for example available from Montello with trade name "HITENOL KH").
[0052] The total amount of surfactant in the compositions of the present disclosure and / or that can be used to practice the present disclosure is typically 5 wt % or less, 3 wt % or less, 2 wt % or less, 1.75 wt % or less, 1.5 wt % or less, or 1.3 wt % or less, based on the total weight of solids in the composition (that is, excluding water). In some embodiments, the total amount of emulsifier employed is anionic in nature.
[0053] In some embodiments, a small amount (e.g., less than 5% by weight of the total surfactant amount) of a nonionic surfactant may be used as desired. Such surfactants are well known to those skilled in the art. Representative commercial examples of nonionic surfactants include the "TRITON X" series of surfactants (octylphenol ethoxylates), "TRITON CG 600" (polyalkyl glucoside) available from Dow Chemical Company, and polymerizable surfactants, including polyoxyethylene alkylphenyl ethers, such as those available from Montello Corporation under the trade name "NOIGEN RN".
[0054] In addition to the polymer binders, water-soluble polymers, tackifiers, and emulsifiers and water described above in any embodiment thereof, the following additives may also be optionally included in the compositions of the present disclosure and / or useful in practicing the present disclosure: inhibitors such as hydroquinone, pigments, dyes, rheology modifiers, thickeners, plasticizers, antioxidants (e.g., hindered phenols, amines, and sulfur and phosphorus hydroperoxide decomposers), stabilizers (e.g., UV absorbers, hindered amine light stabilizers, and heat stabilizers), fillers (e.g., inorganic fillers such as talc, zinc oxide, titanium dioxide, aluminum oxide), preservatives, biocides, corrosion inhibitors, flame retardants, and defoamers. These and other conventional additives, if used, will be present in conventional concentrations known to those skilled in the art to the extent that they do not unacceptably affect the advantages provided by the present disclosure.
[0055] Composition of the present disclosure and / or can be used for practicing the composition of the present disclosure and comprise water.The amount of the water in the said composition is generally based on the gross weight of the said composition, at least 25 % by weight or 30 % by weight.The amount of the water in the said composition can be based on the gross weight of the said composition at most 75 % by weight, 70 % by weight, 65 % by weight, 60 % by weight, 55 % by weight, 50 % by weight, 45 % by weight or 40 % by weight.The available amount of the water in the said composition can be in the scope of 25 % by weight to 55 % by weight, 25 % by weight to 50 % by weight or 30 % by weight to 40 % by weight based on the gross weight of the said composition.
[0056] In some embodiments, the compositions of the present disclosure and / or useful for practicing the present disclosure exhibit a viscosity of 12,000 centipoise (12,000 MPa-s) or less, as measured using a Brookfield viscometer, spindle 6, at 20 rpm. In some embodiments, the viscosity of the composition is no greater than 10,000 centipoise (10,000 mPa-s), 7500 centipoise (75000 mPa-s), 5000 centipoise (5000 mPa-s), 3000 centipoise (3000 mPa-s), or 1000 centipoise (1000 mPa-s). In some embodiments, the viscosity of the composition is at least 300 centipoise (300 mPa-s) or at least 500 centipoise (500 mPa-s).
[0057] In some embodiments, the present disclosure and / or compositions that can be used to practice the present disclosure are substantially free of organic solvents. Common organic solvents include any organic solvents having a boiling point of up to 150° C. at atmospheric pressure. The term “substantially free” means that the composition may contain up to 0.5 wt %, 0.1 wt %, 0.05 wt %, or 0.01 wt % of any of these solvents, or may not contain any of these solvents. These weight percentages are based on the total weight of the composition.
[0058] In some embodiments, the present disclosure and / or compositions that can be used to practice the present disclosure further include organic solvents. Available organic solvents include those that can be compatible with water and can provide homogeneous compositions. The example of available solvents includes esters (for example, methyl acetate and butyl acetate), alcohols (for example, methanol, ethanol and isopropanol), polyols (for example, ethylene glycol, propylene glycol and glycerol) and ketones (for example, acetone). In some embodiments, the organic solvent includes at least one of ethyl acetate, ethanol or acetone. The total amount of organic solvent is generally based on the gross weight of the composition, 20 % by weight or less, 10 % by weight or less or 5 % by weight or less or 1 % by weight or less, and can be greater than 0.5 % by weight, at least 1 % by weight, at least 2 % by weight, at least 3 % by weight, at least 4 % by weight or at least 5 % by weight. Such solvents can be used for example to keep water-soluble polymers dissolved in the presence of a polymer binder that is dispersed in the composition.
[0059] The present disclosure provides the use of the composition of the present disclosure as described above in any embodiment thereof as a spray adhesive composition and / or as a filament spray adhesive. The method using the composition of the present disclosure includes spraying the composition as described above in any embodiment thereof to provide a filament comprising a polymer adhesive and a water-soluble polymer. The spray pattern provided by the composition may include a combination of filaments and other features (such as large droplets or small droplets). This combination pattern can also be used for many adhesive applications. Although droplets generally have an aspect ratio of about 1: 1, the filaments produced by spraying the composition of the present disclosure generally have a length-to-width aspect ratio of at least 2: 1, 3: 1, 5: 1, 10: 1, 100: 1 or more, wherein the length is the longest dimension of the filament, and the width is the dimension perpendicular to the length. The composition of the present disclosure generally provides such as Figure 3 The following examples show that commercially available water-based adhesives are formed into a fine mist spray. For example, in Comparative Examples 1 to 3, an acrylic emulsion is sprayed onto a surface and forms a fine mist typically at Figure 1 When a water-soluble polymer is added to an acrylic emulsion, a spray pattern is formed, usually in Figure 3 The spray pattern represented by Figure 2 (pebble spray) and Figure 3 As shown in Table 3, the lap shear strength of birch wood substrates bonded with the Example composition and the Comparative Example composition is reported. When a water-soluble polymer is added, the bonding strength of the polymer adhesive can be maintained.
[0060] In some embodiments, the composition disclosed and / or can be used to practice the present disclosure is encapsulated in a spray container.Any spray container in a variety of different spray containers can be used to deliver the composition of the present disclosure and can be used in the method of using the composition or preparing the method of bonding products according to the present disclosure.For example, an air-assisted spray system can be useful.The example of an available air-assisted spray system includes those purchased from 3M Company, St.Paul, Minnesota under the trade name "3M Accuspray ONE Spray Gun System with Standard PPS" and "3M Accuspray Paint Spray System with PPS2.0".Therefore, the spray container can be a disposable cup or cup and a disposable liner attached to a spray gun with an atomizing head or nozzle.Compressed air can be used, for example, at a pressure within the range of 0.13 MPa (MPa) to 0.21 MPa.
[0061] In other embodiments, an airless spray system can be used for the compositions and methods of the present disclosure. A pressure tank (such as a 1 liter tank with a pressure of up to 225 psi (1.24 MPa), available from, for example, Apache Stainless Steel Equipment Corporation, Beaver Dam, Wisconsin) can be connected to a nylon hose (e.g., available from 3M Company, St. Paul, Minnesota, under the trade name "3M Cylinder Adhesive Hose"). The hose can be, for example, up to 8, 7, 6, 5, 4, 3, 2, or 1 meter. A high throughput metal spray gun (e.g., available under the trade designations "GunJet" and "H GunJet" from Spray Systems Co., Minnetonka, Minnesota, with a brass nozzle, e.g., available under the trade designations "4001 UniJet", "6501 UniJet", "9501 UniJet", "1100050 UniJet", and "800050 UniJet" from Spray Systems Co.) can be conveniently attached to the hose. The tank can be pressurized with dry nitrogen or any desired gas.
[0062] In other embodiments, aerosol cans can be used for compositions and methods of the present disclosure. Aerosol cans can be obtained from various sources, for example, purchased from Ball Metalpack (Ball Metalpack, Broomfield, Colorado) in Broomfield, Colorado under the trade name "Classic Tinplate Can". Any aerosol actuator (e.g., obtained from Aptar (Aptar, Mukwonago, Wisconsin) under the trade name "Seaquist 802-24-20 / 0890-20FS" in Mukwonago, Wisconsin, with a color-changing valve purchased from Aptar under the trade name "AR-83") can be available. Aerosols typically include propellants. Examples of suitable propellants include nitrogen, carbon dioxide, ethane, propane, isobutane, n-butane, dimethyl ether, 1,1-difluoroethane, trans-1,3,3,3-tetrafluoropropylene and mixtures thereof. Typically, liquid aerosol propellants, such as propane, butane, and isobutane, are added to the composition in an amount ranging from about 5% to about 45% by weight based on the total weight of the composition. When gases such as nitrogen and carbon dioxide are used as propellants, the gaseous propellant is typically present in an amount ranging from up to about 10%, 8%, 6%, 5%, or 2% by weight based on the total weight of the composition.
[0063] The method for preparing the composition of the present disclosure includes mixing the components of the solution of the water-soluble polymer dissolved in at least a portion of water with the emulsion of the polymer binder. It is also possible to mix the pure water-soluble polymer with the emulsion of the polymer binder. Other components can be mixed into the composition as solid, liquid, dissolved in water or emulsified in water. In the embodiment where the composition includes a tackifier, the second emulsion of the tackifier can be mixed with the emulsion of the polymer binder and the solution of the water-soluble polymer. The order of addition is not limited. In some embodiments, the emulsion comprising the polymer binder also includes a tackifier. In some embodiments, the monomer for preparing the polymer binder can be polymerized in the presence of a tackifier. For example, a tackifier and at least one (meth) alkyl acrylate can be combined to form a solution, which can be combined with water and an emulsifier. Then the at least one (meth) alkyl acrylate can be polymerized to form an emulsion having droplets comprising both an acrylic polymer and a tackifier. The solution may include any other optional monomers described above.
[0064] According to the method for manufacturing a bonding article including a first substrate or a second substrate of the present disclosure, the composition of the present disclosure or the method of the present disclosure is sprayed to provide a filament comprising a polymer adhesive and a water-soluble polymer on at least one of the first substrate or the second substrate. The method further includes bonding the first substrate and the second substrate using filaments. The present disclosure provides an article comprising a first substrate and a second substrate bonded together with the composition of the present disclosure. The surface of the first substrate and the second substrate can be any desired material. In some embodiments, at least one of the surface of the first substrate or the surface of the second substrate includes at least one of metal, glass, polymer, paper, painted surface, nonwoven or woven fabric, or composite material. The material of the surface of the first substrate and the second substrate can be found in the entire substrate, or the surface can include a material different from the substrate body. In some embodiments, the surface of the first substrate and / or the second substrate includes at least one of metal (e.g., steel, stainless steel or aluminum), glass (e.g., it can be coated with indium tin oxide), polymer (e.g., plastic, rubber, thermoplastic elastomer or thermosetting material), paper, painted surface or composite material. Composite materials can be made of any two or more constituent materials with different physical or chemical properties. When components are combined to prepare composite materials, materials with properties different from individual components are generally obtained. Some examples of available composite materials include fiber-reinforced polymers (e.g., carbon fiber-reinforced epoxy resins and glass-reinforced plastics), metal matrix composites, and ceramic matrix composites. The surface of at least one of the first substrate or the second substrate may include polymers, such as polyolefins (e.g., polypropylene, polyethylene, high-density polyethylene, polypropylene blends), polyamide 6 (PA6), acrylonitrile butadiene styrene (ABS), polycarbonate (PC), PC / ABS blends, polyvinyl chloride (PVC), polyamide (PA), polyurethane (PUR), thermoplastic elastomers (TPE), polyoxymethylene (POM), polystyrene, polyesters (e.g., polyethylene terephthalate), poly(methyl) methacrylate (PMMA), and combinations thereof. The surface of at least one of the first substrate or the second substrate may also include a metal coating on such polymers. In some embodiments, at least one of the first substrate or the second substrate includes a transparent material, such as glass or a polymer (e.g., acrylic acid or polycarbonate).
[0065] In some embodiments, at least one of the first substrate or the second substrate has a textured surface. Textured surfaces are common in construction. In some embodiments, at least one of the first substrate or the second substrate is a fiber substrate or a foam substrate (e.g., a polymer foam, such as polyurethane, EPDM, and polyethylene foam).
[0066] Fibrous substrates include woven or nonwoven fabrics. The term "nonwoven" refers to a material having a structure of individual fibers or spun yarns that are interlayered, but not interlayered in an identifiable manner such as with a knitted fabric. Examples of nonwoven webs include spunbond webs, spunlace webs, needle-punched webs, air-laid webs, melt-blown webs, and bonded carded webs. Useful nonwovens can be made from natural fibers (e.g., wood fibers or cotton fibers), synthetic fibers (e.g., thermoplastic fibers), or a combination of natural and synthetic fibers. Examples of suitable materials for forming thermoplastic fibers include polyolefins (e.g., polyethylene, polypropylene, polybutene, ethylene copolymers, propylene copolymers, butene copolymers, and copolymers and blends of these polymers), polyesters, and polyamides. The fiber can also be a multicomponent fiber, for example, with a core of a thermoplastic material and an outer skin of another thermoplastic material. Examples of woven fabrics include twill and canvas.
[0067] In some embodiments, at least one of the first substrate or the second substrate is a low surface energy substrate. The term "low surface energy substrate" refers to substrates having a surface energy of less than 34 dynes / cm. Such materials include polypropylene, polyethylene [e.g., high density polyethylene (HDPE), low density polyethylene (LDPE) and linear low density polyethylene (LLDPE)], and blends of polypropylene (e.g., PP / EPDM, TPO). In some embodiments, at least one of the first substrate or the second substrate is a medium surface energy substrate. The term "medium surface energy substrate" refers to substrates having a surface energy in the range of 34 dynes / cm to 70 dynes / cm, typically 34 dynes / cm to 60 dynes / cm, and more typically 34 dynes / cm to 50 dynes / cm. Such materials include polyamide 6 (PA6), acrylonitrile butadiene styrene (ABS), polycarbonate (PC) / ABS blends, PC, PVC, polyamide (PA), polyurethane (PUR), thermoplastic elastomer (TPE), polyoxymethylene (POM), polystyrene, and poly(methyl methacrylate) (PMMA). Surface energy is typically determined by contact angle measurements as described, for example, in ASTM D7490-08.
[0068] Compositions of the present disclosure can be used in multiple applications. Compositions of the present disclosure can also be used for bonding different materials together. In some of these embodiments, the first substrate includes metal, and the second substrate includes rubber or plastic. In some embodiments, the first substrate and the second substrate are dissimilar plastics. Compositions of the present disclosure can also be used for foam lamination, wherein the first substrate or the second substrate is foam (for example, polymer foam, such as polyurethane, EPDM and polyethylene foam). Compositions of the present disclosure can also be used for packaging, wherein the first substrate or the second substrate is paper (for example, paper coated with polymer) or paperboard.
[0069] According to the present disclosure and / or can be used for practicing the composition of the present disclosure generally and advantageously do not need external coagulant, such as citric acid, lactic acid, acetic acid or zinc sulfate.Therefore, the method for preparing the bonding product comprising the first substrate and the second substrate does not need to include the second part of this coagulant in a predetermined ratio with the composition of the present disclosure.Therefore, the composition and method of the present disclosure avoid the shortcomings relevant to the two-part system, such as the co-spraying equipment is expensive and needs to maintain and monitor the complexity of the ratio of the two parts (that is, coagulant and adhesive composition).In addition, according to the present disclosure and / or by the spray adhesive composition or the composition prepared by the method of the present disclosure does not need to form long filaments when spraying or after spraying.
[0070] Some embodiments of the present disclosure
[0071] In a first embodiment, the present disclosure provides a composition comprising water, a polymer binder dispersed in the water or the composition, and a water-soluble polymer dissolved in the water or the composition, wherein the weight average molecular weight of the water-soluble polymer is at least 90,000 g / mol. In a second embodiment, the present disclosure provides a composition according to the first embodiment, wherein after spraying the composition, the composition provides a filament comprising the polymer binder and the water-soluble polymer. In a third embodiment, the present disclosure provides a composition according to the first embodiment or the second embodiment, wherein the composition is a spray adhesive composition.
[0072] In the fourth embodiment, the present disclosure provides a composition according to any one of the first embodiment to the third embodiment, wherein the polymer binder includes at least one of acrylic polymer, natural rubber, synthetic polyisoprene, polybutadiene, styrene / butadiene rubber, styrene / isoprene / butadiene rubber or acrylonitrile-butadiene rubber. In the fifth embodiment, the present disclosure provides a composition according to the fourth embodiment, wherein the polymer binder includes at least one of acrylic polymer or styrene / butadiene rubber. In the sixth embodiment, the present disclosure provides a composition or a spray adhesive composition according to the third embodiment or the fourth embodiment, and the composition or the spray adhesive composition further includes a tackifier. In the seventh embodiment, the present disclosure provides a composition according to the sixth embodiment, wherein the tackifier includes at least one of rosin acid, rosin ester, C5 aliphatic hydrocarbon resin, C9 aromatic resin or mixed aliphatic-aromatic hydrocarbon resin. In the eighth embodiment, the present disclosure provides a composition according to the sixth embodiment or the seventh embodiment, wherein the tackifier is present in the composition in the range of two to 30 parts per hundred parts of acrylic polymer.
[0073] In a ninth embodiment, the present disclosure provides a composition according to any one of the first to eighth embodiments, wherein the water-soluble polymer comprises at least one of polyacrylamide, poly(ethylene oxide), poly(vinyl pyrrolidone), polyvinyl alcohol, or polyvinyl acetate. In a tenth embodiment, the present disclosure provides a composition according to any one of the first to ninth embodiments, wherein the water-soluble polymer comprises at least one of polyacrylamide, poly(ethylene oxide), or poly(vinyl pyrrolidone). In an eleventh embodiment, the present disclosure provides a composition according to any one of the first to tenth embodiments, wherein the water-soluble polymer is nonionic. In a twelfth embodiment, the present disclosure provides a composition according to any one of the first to eleventh embodiments, wherein the weight average molecular weight of the water-soluble polymer is no greater than 9,000,000 g / mole, 8,000,000 g / mole, 7,000,000 g / mole, 6,000,000 g / mole, 5,000,000 g / mole, 4,000,000 g / mole, 3,000,000 g / mole, 2,000,000 g / mole, or 1,000,000 g / mole. In a thirteenth embodiment, the present disclosure provides a composition according to any one of the first to twelfth embodiments, wherein the water-soluble polymer is present in the composition in an amount of at least 0.05 wt % or no greater than 5 wt % based on the total weight of the composition.
[0074] In the fourteenth embodiment, the present disclosure provides a composition according to any one of the first to thirteenth embodiments, wherein the polymer binder is present in the composition in an amount of at least 25 weight % or no more than 75 weight % based on the total weight of the composition. In the fifteenth embodiment, the present disclosure provides a composition according to any one of the first to fourteenth embodiments, wherein the filaments comprising the polymer binder and the water-soluble polymer are pressure-sensitive adhesive filaments. In the sixteenth embodiment, the present disclosure provides a composition according to any one of the first to fifteenth embodiments, further comprising a propellant.
[0075] In the seventeenth embodiment, the present disclosure provides the composition according to any one of the first embodiment to the sixteenth embodiment, which is packaged in a spray container. In the eighteenth embodiment, the present disclosure provides the composition according to any one of the first embodiment to the seventeenth embodiment, the composition further comprises at least one of acetone, ethanol or methyl acetate, and its amount is greater than 0.5 weight % or at least 1 weight %, 2 weight %, 3 weight % or 4 weight % and at most 20 weight %, 10 weight % or 5 weight % based on the total weight of the composition. In the nineteenth embodiment, the present disclosure provides the purposes of the composition according to any one of the first embodiment to the eighteenth embodiment as a spray adhesive composition. In the twentieth embodiment, the present disclosure provides the purposes of the composition according to any one of the first embodiment to the eighteenth embodiment as a filament spray adhesive. In the twenty-first embodiment, the present disclosure provides a method of using the composition according to any one of the first embodiment to the eighteenth embodiment, the method comprising spraying the composition to provide a filament comprising the polymer binder and the water-soluble polymer.
[0076] In a twenty-second embodiment, the present disclosure provides a method for preparing a composition according to any one of the first to eighteenth embodiments, the method comprising mixing a component comprising a solution of a water-soluble polymer dissolved in at least a portion of the water with an emulsion of a polymer binder. In a twenty-third embodiment, the present disclosure provides a method according to the twenty-second embodiment, wherein the emulsion further comprises a tackifier. In a twenty-fourth embodiment, the present disclosure provides a method according to the twenty-third embodiment, wherein the components further comprise a second emulsion of a tackifier.
[0077] In the twenty-fifth embodiment, the present disclosure provides a method for manufacturing a bonded article comprising a first substrate and a second substrate, the method comprising spraying the composition according to any one of the first embodiment to the eighteenth embodiment to provide filaments comprising a polymer binder and a water-soluble polymer on at least one of the first substrate or the second substrate, and using these filaments to bond the first substrate and the second substrate. In the twenty-sixth embodiment, the present disclosure provides the method according to the twenty-fifth embodiment, wherein at least one of the first substrate or the second substrate has a textured surface. In the twenty-seventh embodiment, the present disclosure provides the method according to the twenty-fifth embodiment or the twenty-sixth embodiment, wherein at least one of the first substrate or the second substrate is a foam.
[0078] In order to more fully understand the present disclosure, the following examples are listed. It should be understood that these examples are only for illustrative purposes and should not be interpreted as limiting the present disclosure in any way.
[0079] Example
[0080] Unless otherwise indicated, all parts, percentages, ratios, etc. in the examples and the rest of the specification are by weight.
[0081] Table 1. Materials list
[0082]
[0083] Adhesive spray method
[0084] All adhesives were sprayed with an air-assisted sprayer (obtained from 3M Company, Lindstrom, Minnesota, under the trade names "3M Accuspray PPS ONE SprayGun System with Standard PPS" and "3M Accuspray Paint Spray System with PPS2.0"). The adhesive was fed through a gun having a gravity feed cup and a disposable 1.8 millimeter (mm) diameter disposable plastic nozzle (obtained from 3M Company, Lindstrom, Minnesota, under the trade name "Accuspray Atomizing Head" on the back. The gravity feed cup was filled with approximately 100 grams (g) of each adhesive formulation. Air pressure ranged from 10 pounds per square inch (psi) to 30 psi, obtained using household compressed air through a gas regulator attached to the bottom of the gun. The adhesive is sprayed from 10 centimeters (cm) to 25 cm from the paper and at a rate of 6 g / sec to 10 g / sec in a spray stroke of 30 cm to 60 cm.
[0085] Spray pattern characterization.
[0086] The following categories are used to characterize the spray patterns from the adhesive spray method. A "mist" spray is defined as a fine atomized spray pattern with very small droplets less than 1 mm to 2 mm in diameter. A "pebble-like" spray is defined as a mixture of fine mist and larger droplets with a diameter of about 1 mm to 5 mm. A "filament" spray pattern is defined as a spray pattern that produces filaments or strands of liquid adhesive on the surface. The spray patterns are recorded numerically in Table 2. A "mist" spray is rated as "1". A "pebble-like" spray is rated as "2". A "filament" pattern is rated as "3". When the spray pattern is between two levels, half is also used. The spray grade is determined by reporting the average spray pattern after dispensing approximately 100 g via the spray applicator and is reported in Table 2.
[0087] Overlap Shear (OSL) Testing
[0088] Birch substrates (2.54 cm x 10.16 cm x 0.32 cm panels obtained from Forest Product Supply, St. Paul, Minnesota) were used to analyze the bond strength of certain embodiments. The birch panels were stripped so that only 2.54 cm 2 As described in detail above in "Adhesive Spray Test Method", the adhesive was applied with a PPS gun and applied at 30 to 50 grams per square meter. Once the adhesive was sprayed onto the substrate, the bond was joined within 5 minutes (min), held with an adhesive clip, and allowed to stay for 16 to 24 hours. The lap shear strength was tested on a tensile tester ("QTEST_5", purchased from MTS Systems Corporation, Eden Prairie, Minnesota), where the sample was stretched at a rate of 5.08 cm / min, and the breaking strength was recorded in kilopascals (kPa). The data reported in Table 3 are the averages of three samples.
[0089] Example (EX) 1 to Example 18 and Comparative Example (CE) 1 to Comparative Example 3
[0090] First, prepare 1 liter (1 L) of a stock solution of a water-soluble polymer (referred to as "Polymer"). The "Polymer Solution Concentration" in Table 2 shows the weight percentage (wt%) of 1 L of the stock solution. Add the polymer powder or pellets to a glass jar, then add water until the volume is 1 L and roll overnight. Then, add the appropriate water-based adhesive to the glass jar in the amount from Table 2. An overhead stirrer (obtained under the trade name "Hei-Torque Core Overhead Stirrer" from Heidolph Instruments, Wood Dale, Illinois) with a glass overhead stirring shaft (obtained under the trade name "Kimble Kontes Stirrer Shaft" from DWK Life Sciences, Millville, New Jersey) and a PTFE stirring blade (obtained under the trade name "Kimble Kontes PTFE Stirrer Blade" from DWK Life Sciences) was used to mix the formulations listed in Table 2. Under stirring, the solution of the water-soluble polymer was slowly added over 5 minutes. The mixture was then stirred for an additional 10 minutes. The amounts and concentrations of the components of Examples 1 to 18 are listed in Table 2 below. Polymer wt% refers to the wt% of the polymer in a composition comprising water, a polymer binder, and a water-soluble polymer. Comparative Examples 1 to 3 are commercially available adhesive compositions.
[0091] Weight average molecular weight determination
[0092] The weight average molecular weight of the poly(ethylene oxide) samples is determined by comparison with narrow distribution poly(ethylene oxide) standards using gel permeation chromatography (GPC). GPC measurements can be performed on an Agilent 1100 instrument (available from Agilent Technologies, Santa Clara, Cal.) using an Agilent Plgel Mixed C 5μ 30 cm×7.5 mm column (available from Agilent Technologies) for samples with molecular weights less than 500,000 g / mole and an Agilent Plgel Mixed A 20μ 30 cm×7.5 mm column (available from Agilent Technologies) for samples with higher molecular weights. A refractive index detector can be used at 40° C. Solutions can be made from PEG samples at 25 mg / 20 mL of 1:1 stabilized tetrahydrofuran / chloroform. The samples are vortexed overnight to ensure complete solution. A sample volume of 50 microliters can be injected into an Agilent Plgel mixed C 5μ30cm×7.5mm column at a column temperature of 40°C. Sample volumes of 25 microliters and 50 microliters are injected into an Agilent Plgel mixed A 20μ30cm×7.5mm column. A flow rate of 0.6mL / minute is used, and the mobile phase is 1:1 stabilized tetrahydrofuran / chloroform. Molecular weight calibration can be performed using narrow distribution poly (ethylene oxide) standards purchased from Agilent Technologies, which are dissolved in 1:1 stabilized THF / chloroform with about 5mg to 10mg per 20mL solvent. These cover a molecular weight range of 1.7MDa to 600Da. Calibration and molecular weight distribution calculations can be performed using suitable GPC software, using a third-order polynomial to fit the molecular weight calibration curve. If necessary, those skilled in the art can modify columns and calibration standards for other water-soluble polymers.
[0093] Table 2. Formulations and spray levels of Examples 1 to 18 and Comparative Examples 1 to 3
[0094]
[0095] *n / a means not applicable
[0096] Table 3. Lap shear data
[0097] Example Adhesives polymer Weight % of polymer Birch OLS(kPa) CE 2 Acrylic 2 none n / a 407 10 Acrylic 2 PEO 1 0.2 421 12 Acrylic 2 PEO 2 0.3 364 15 Acrylic 2 PVP 1.1 579
[0098] The present disclosure is not limited to the embodiments described above, but is subject to the limitations set forth in the following claims and any equivalents of the claims.The present disclosure may be suitably practiced in the absence of any element not specifically disclosed in the present disclosure.
Claims
1. A composition comprising: water; a polymer binder dispersed in the composition; and a water-soluble polymer that is dissolved in the composition, wherein the water-soluble polymer has a weight average molecular weight of at least 90,000 g / mole, wherein upon spraying the composition, the composition provides filaments comprising the polymer binder and the water-soluble polymer.
2. The composition of claim 1, wherein the polymer binder comprises at least one of an acrylic polymer, a natural rubber, a synthetic polyisoprene, a polybutadiene, a styrene / butadiene rubber, a styrene / isoprene / butadiene rubber, or a nitrile rubber.
3. The composition according to claim 1 or 2, further comprising a tackifier, wherein the tackifier comprises at least one of rosin acid, rosin ester, C5 aliphatic hydrocarbon resin, C9 aromatic resin, or mixed aliphatic-aromatic hydrocarbon resin.
4. The composition of any one of claims 1 to 3, wherein the water-soluble polymer comprises at least one of polyacrylamide, poly(ethylene oxide), poly(vinyl pyrrolidone), polyvinyl alcohol, or polyvinyl acetate.
5. The composition according to any one of claims 1 to 4, wherein the water-soluble polymer is non-ionic.
6. The composition according to any one of claims 1 to 5, wherein the water-soluble polymer is present in the composition in an amount of at least 0.1 wt% or no greater than 5 wt%, based on the total weight of the composition.
7. The composition of any one of claims 1 to 6, wherein the water-soluble polymer has a weight average molecular weight of no greater than 9,000,000 g / mole.
8. The composition of any one of claims 1 to 7, wherein the polymer binder is present in the composition in an amount of at least 25 wt% or no greater than 75 wt%, based on the total weight of the composition.
9. The composition of any one of claims 1 to 8, wherein the filaments comprising the polymeric binder and the water-soluble polymer are pressure-sensitive adhesive filaments.
10. The composition according to any one of claims 1 to 9, which is at least one of the following: the composition further comprises a propellant or the composition is packaged in a spray container.
11. The composition according to any one of claims 1 to 10, further comprising at least one of acetone, ethanol or methyl acetate in an amount of greater than 0.5 wt% and up to 20 wt% based on the total weight of the composition.
12. A method for preparing a composition according to any one of claims 1 to 11, comprising: A component comprising a solution of the water-soluble polymer dissolved in at least a portion of the water is mixed with the emulsion of the polymer binder.
13. The method of claim 12, wherein the emulsion further comprises a viscosity increasing agent, or a second emulsion wherein the components further comprise a viscosity increasing agent.
14. A method of preparing a bonded article comprising a first substrate and a second substrate, the method comprising: spraying the composition according to any one of claims 1 to 11 to provide the filaments comprising the polymer binder and the water-soluble polymer on at least one of the first substrate or the second substrate; as well as The first substrate and the second substrate are bonded using the filaments.
15. Use of a composition according to any one of claims 1 to 11 as a spray adhesive composition.
Citation Information
Patent Citations
Artificial hair-forming composition, artificial hair forming aerosol, method for forming artificial hair, composition for capturing insect by aerosol filamentous formed material, insect capturing aerosol, and insect capturing method
JP2008231652A
Release liner comprising nanofibrillar cellulose
US10113006B2
One part, fast-setting, aqueous adhesive emulsions
US10221343B2
Adhesive based on materials containing latex and lignin and process for producing same
US20210071049A1
Spraying apparatus for artificial hair augmenting agent
US6168781B1