Composite organic silicon defoaming agent and preparation method thereof
By using composite formula and filler heat treatment technology in silicone defoaming agents, a dual emulsion structure is formed, which solves the problems of stability and defoaming force caused by emulsifiers, and achieves efficient defoaming effect and long-term stability.
Patent Information
- Application Number
- CN202410847145.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-11-29
AI Technical Summary
During the preparation process of existing silicone defoaming agents, the addition of emulsifiers makes it difficult for the defoaming agent to balance stability and defoaming effectiveness, resulting in difficulty in taking into account both stability and defoaming force.
The composite silicone defoamer formula is adopted, including silicone compounds, dispersants, emulsifiers, solid fillers, filler treatment agents and catalysts. Through the filler heat treatment and secondary emulsification process, a double emulsion structure is formed to improve the dispersion of the defoamer. and stability while maintaining defoaming effectiveness.
It achieves good dispersion and stability of the defoaming agent, significantly improves the defoaming effect and storage time, takes into account stability and defoaming force, and is suitable for defoaming applications in water systems.
Smart Images

Figure BDA0004915983120000081 
Figure BDA0004915983120000091 
Figure BDA0004915983120000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of defoamers, and in particular relates to an organosilicon defoamer for eliminating and inhibiting foam in a foaming system in the fields of petrochemical industry, printing and dyeing industry and coating industry. Background Art
[0002] Foam is a two-phase system in which gas is dispersed in another continuous liquid as a discontinuous phase. The liquid-gas volume of common foam systems is relatively small, and is formed by a large volume of gas phase distributed in a small volume of liquid; when the liquid-gas volume of the foam system is relatively high, it can be regarded as an emulsion in which the solid phase is gas. Foam is thermodynamically unstable. Once it is formed, it is in a dynamic process of continuous downflow, evaporation, and rupture of the liquid film. It is usually formed by two ways: mechanical mixing of gas (usually air) and solution (usually surfactant), or release of gas due to changes in temperature, pressure, etc. in the foaming liquid. Especially for foams formed in the presence of surfactants, the action of surfactants hinders the aggregation of bubbles. This type of foam is undesirable in most cases, and it is often necessary to add defoaming agents to destroy and inhibit it.
[0003] Defoaming is the reverse process of foam stabilization, which usually includes two meanings: one is "foam suppression"; the other is "foam breaking". When a defoaming agent is added to a foam-containing liquid at a very low concentration, the generation of foam can be quickly controlled and the existing foam can be destroyed. Compounds suitable for defoaming agents must be easy to spread on the surface of the solution. When such a liquid spreads on the surface of the solution, it will take away a layer of solution adjacent to the surface, causing the liquid film to become thinner and rupture locally, and the foam will be destroyed. In general, the faster the defoaming agent spreads on the surface of the solution, the thinner the liquid film will become, and the critical thickness will be reached quickly, the foam will be destroyed faster, and the defoaming effect will be strengthened. Generally, liquids that can spread on the surface and play a defoaming role have a low surface tension and are easily adsorbed on the surface of the solution, which reduces the local surface tension of the solution surface (that is, the surface pressure increases), and an imbalance occurs. Therefore, spreading occurs locally from this point on, and at the same time, it will take away a layer of adjacent liquid under the surface, causing the liquid film to become thinner, thereby destroying the bubble film. Therefore, the reason for defoaming is that on the one hand, the defoamer molecules that are easy to spread and adsorb replace the foaming agent molecules to form a film with poor strength; at the same time, during the spreading process, part of the solution in the adjacent surface layer is taken away, making the foam liquid film thinner, reducing the stability of the foam and making it easy to be destroyed.
[0004] Among them, as a widely used defoamer, silicone defoamer has extremely low surface tension, which enables it to quickly spread on the foam surface and destroy the foam structure, thereby achieving a defoaming effect; it can also maintain its chemical stability at higher temperatures and is suitable for use under a variety of different temperature conditions; and because the Si-O bond in its chemical structure is very stable, silicone defoamer is difficult to react chemically with other substances, so it can be used in systems containing acids, alkalis, and salts; at the same time, silicone defoamers have also been proven to be harmless to humans and animals and can be safely used in food, medical and other industries; most importantly, silicone defoamers can effectively break the generated foam and significantly inhibit the regeneration of foam when used in small amounts, usually only one millionth of the weight of the foaming medium is needed to produce a defoaming effect. In summary, silicone defoamers have a wide range of application value in many industrial fields due to their low surface tension, excellent thermal stability, chemical stability and physiological inertness, as well as strong defoaming power.
[0005] Usually, in order to effectively disperse the defoamer in the bubble medium, the silicone defoamer is usually prepared in the form of an emulsion. However, in the preparation process of existing silicone defoamers, since polysiloxane is difficult to disperse and insoluble in water, its dispersion in the water system is hindered, and an emulsifier must be added. If the emulsifier is added in excess, the emulsion will be stable, but the defoaming effect will be poor. If the emulsifier is used in too little amount, the defoamer emulsion will be unstable and prone to stratification. Therefore, in actual operation, since the dosage is difficult to control, the stability and defoaming effect of the defoamer prepared by the prior art are often difficult to balance.
[0006] The Chinese patent application number CN201611154366.X discloses an organosilicon defoamer, the weight percentage of the raw materials for the preparation of the defoamer is: 10-40% polyether-modified polysiloxane, 10-25% silicone resin, 1-5% dispersant, 40-60% water, 5-25% emulsifier, and the total components are 100%. The organosilicon defoamer of this invention can provide a reasonable channel for the treatment of high-boiling byproducts of organosilicon, improve the stability and dispersibility of the emulsion, ensure the storage time, greatly improve the instant defoaming ability, and make the raw materials have a wider temperature range. However, the application simply selects conventional reagents for batching, and does not reveal the reasons for the improvement of emulsion stability, and how to achieve a balance between the defoaming effect and stability of the defoamer.
[0007] The Chinese patent with application number CN202111649422.8 discloses a polyether-modified organosiloxane emulsion defoamer, which belongs to the field of organosilicon defoamers. It includes the following components by weight: 30-50 parts of polyether-modified organosiloxane, 6-18 parts of polysiloxane, 10-20 parts of composite emulsifier, 1-4 parts of thickener, 0.1-3 parts of stabilizer, 8-14 parts of nano-dispersant and 60-80 parts of water; the nano-dispersant is a modified silica nano-sheet. This invention mainly reduces the effect of polyether modification on the defoaming and anti-foaming properties of the defoamer by composite polysiloxane, improves the stability of the emulsion by compounding the emulsifier, and further improves the dispersibility and defoaming performance by adding the nano-dispersant. However, this application requires the additional preparation of nano-dispersants to achieve a better dispersion effect, resulting in a cumbersome process.
[0008] The Chinese patent with application number CN201811271649.1 discloses a modified silicone defoamer, comprising the following raw materials in parts by weight: 20-40 parts of polysiloxane, 15-30 parts of hydrophobic silica, 5-15 parts of high carbon alcohol, 3-5 parts of isopropyl citrate, 2-4 parts of methyl acrylate, 2-4 parts of monoglycerol fatty acid ester, 1-3 parts of sodium hexametaphosphate, 0.5-2 parts of sodium secondary alkyl sulfonate, 2-5 parts of surfactant, 1.5-3 parts of thickener, 0-3 parts of bactericide and 70-85 parts of deionized water. The modified silicone defoamer obtained by the invention has good defoaming and anti-foaming properties, and the quality is stable for long-term storage and use. However, the application mainly achieves the composite effect by adding a variety of additives, and does not point out how to improve the preparation method to obtain a silicone defoamer with good stability and defoaming ability, and it can be seen from its examples that the defoaming ability of the defoamer of the application is still poor.
[0009] In summary, the above documents all mention silicone defoamers and their preparation methods. They often add agents with dispersing effects to make the defoamers more dispersible and stable during use. However, the improvement in dispersibility will also lead to poor defoaming effects. On the contrary, reducing the emulsifier will reduce the stability of the silicone defoamer in the form of an emulsion, and it is impossible to achieve both stability and defoaming power. Therefore, how to make the defoamer have a certain defoaming ability during the preparation of the silicone defoamer and avoid the decrease in emulsion stability during the emulsification process has become a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0010] In view of the problem that in organosilicon defoamers, it is difficult to balance stability and defoaming effectiveness due to the addition of emulsifiers during the preparation of emulsions, the first purpose of the present invention is to provide a composite organosilane defoamer, in which raw materials such as solid fillers and filler treatment agents are added to the formula to form a composite with siloxane compounds, so that the prepared defoamer has good dispersibility and stability.
[0011] The second object of the present invention is to provide a method for preparing a composite organosilane defoamer, which includes a filler heat treatment and a secondary emulsification process, so that the defoamer can have good defoaming effect and stability by generating new chemical bonds and forming a double emulsion.
[0012] The technical solution adopted by the present invention to solve its technical problem is:
[0013] A composite organosilicon defoamer, the raw materials of which include: siloxane compounds, dispersants, emulsifiers and thickeners, solid fillers, filler treatment agents, catalysts and additives; preferably, the mass ratio of the solid fillers to the siloxane compounds is less than or equal to 1:9; further, the solid fillers include: oxides of silicon, magnesium, zinc, aluminum, titanium and silicone resin, preferably: fumed silica and silicone resin, and the mass ratio of the two is 8-3:7-3.
[0014] The present application utilizes the characteristics of small particle size and large specific surface area of solid fillers, and adsorbs bubbles and impacts them to create weak points, so that the bubbles are broken under the action of the surface tension of the siloxane compound; and the surface of the solid filler has more than 5% to 10% hydroxyl groups, preferably fumed silica and silicone resin, both of which contain a certain amount of silanol bonds, which can form hydrogen bonds with water molecules in the water system, which is conducive to promoting the dispersion and stability of the defoamer. Furthermore, by controlling the mass ratio of fumed silica to silicone resin, the defoaming effect of the defoamer is better. Usually, exceeding the above ratio will cause the solid filler to be mixed for too long, and the incompletely mixed part will precipitate, while below this ratio will reduce the surface tension of the defoamer.
[0015] Preferably, the average particle size of the above solid fillers is ≤25 μm. When the solid fillers are fumed silica and silicone resin, the average particle size of the fumed silica is 5 to 25 μm, and the average particle size of the silicone resin is 3 to 20 μm.
[0016] Select appropriate solid filler particle size, preferably 5 to 15 μm, which can be dispersed to a high degree in the foaming liquid and have good stability, and form basic defoaming units with extremely small particles and a large number of particles between the foaming liquid, so that the defoamer can achieve the best defoaming effect.
[0017] Preferably, the mass of the filler treatment agent is 1-2.5% of the mass of the siloxane compound, and the filler treatment agent includes oleic acid. Adding the filler treatment agent to waterproof the solid filler can effectively prevent the solid filler from agglomerating, thereby improving the dispersion and uniformity of the mixture.
[0018] Preferably, the catalyst accounts for 1-3% of the weight of the solid filler, and the catalyst includes: hydrogen-containing silicone oil or silane coupling agent.
[0019] The catalyst is selected from hydrogen-containing silicone oil or silane coupling agent, the hydrophilic groups contained therein react with the hydroxyl groups in the solid filler, and can further enhance the bonding between the solid filler and the silicon oxide compound. The present invention makes the amount of hydrogen-containing silicone oil or silane coupling agent used be 1-2.5% of the above-mentioned solid filler. Generally, the smaller the filler particle size and the larger the surface area, the greater the amount of hydrogen-containing silicone oil or silane coupling agent used. However, using too much catalyst will lead to a decrease in economic efficiency, and too little catalyst will not have sufficient effect.
[0020] Preferably, the above dispersant is: a polyvinyl alcohol aqueous solution with an alkalinity of 54 to 89 mol%. Polyvinyl alcohol with a high alkalinity has a lower relative molecular mass and a higher hydroxyl functional group content, and has extremely strong treatability and biocompatibility. Polyvinyl alcohol with a low alkalinity has poorer treatability.
[0021] Preferably, the above-mentioned siloxane compound is polydimethylsiloxane. As a linear random polymer, polydimethylsiloxane is composed of repeated dimethylsiloxane units, has an unbranched structure, has excellent stability, electrical insulation and heat resistance, and can be used for a long time in the range of -50°C to 200°C.
[0022] A method for preparing a composite organosilicon defoamer comprises the following steps:
[0023] S1: Heat treatment of filler: add the above-mentioned siloxane compound and the above-mentioned solid filler into a reactor, heat the reactor to 150-180° C., stir for 4-7 hours, add the above-mentioned catalyst, heat to 180-185° C., react for 2-7 hours, and obtain a first mixed solution.
[0024] S2: Preparation of siloxane composite: Cool the first mixed solution to 60-70° C., add the filler treating agent, maintain the reactor temperature at 50-75° C., and continue stirring for 0.5-1 h to obtain a siloxane composite.
[0025] S3: Dispersion phase transition: add the above dispersant to the above siloxane complex, maintain the reactor temperature at 60-70°C, stir at a speed of 250-500 r / min, stir for 0.5 h to obtain a siloxane complex dispersion, add the above emulsifier and deionized water to the above siloxane complex dispersion in sequence, continue to maintain the reactor temperature at 60-70°C, stir at a speed of 10000-15000 r / min, stir for 0.5-1 h, and obtain a second mixed solution after phase transition.
[0026] S4: Secondary emulsification: Maintain the temperature of the second mixed liquid at 60-70°C. After the deionized water evaporates 5-10% of its mass fraction, add a corresponding amount of deionized water, maintain the reactor temperature at 60-70°C, and stir at a speed of 10000-15000 r / min for 0.5 h to obtain an emulsion.
[0027] S5: Cooling: adding the thickener and the additive to the emulsion, and cooling to room temperature to obtain the organosilicon defoaming agent.
[0028] On the surface of solid fillers before treatment, such as fumed silica and silicone resin, there are often two hydrophilic active groups, adjacent hydroxyl groups and isolated hydroxyl groups; the solid filler and the siloxane compound are heat-treated, and during the process, the isolated hydroxyl group is replaced by the siloxy group in the siloxane compound, and a chemical bond is generated between the solid filler and the siloxane compound. Since the solid filler has a small particle size and a large specific surface area, it can adsorb bubbles and impact the bubbles to create weak points, and promote the rupture of bubbles under the action of the surface tension of the siloxane compound. Furthermore, controlling the reaction temperature of the filler heat treatment at 180 to 185°C, preferably 180°C, can generate a more considerable number of chemical bonds between the solid filler and the siloxane compound, and at the same time, the hydrogen bonds between the hydroxyl groups and the siloxy groups are converted into chemical bonds, strengthening the bonding between the solid filler and the siloxane compound.
[0029] After preparing the siloxane compound and the solid filler to obtain the siloxane complex, the dispersion phase transfer and the first emulsification are first carried out, and the aqueous solution is encapsulated in the oil phase to form an oil-in-water primary emulsion, i.e., the second mixed solution. The second mixed solution is then subjected to a secondary emulsification. It should be clear that "secondary emulsification" does not simply refer to the second emulsification process, and the present invention does not limit the number of secondary emulsifications in the system. In this process, the substance is encapsulated by multiple emulsifications, and the emulsion is converted from an oil-in-water state to a water-in-oil state. The primary emulsion is encapsulated in the water phase under the action of high-speed shearing, evaporation, and continuous emulsification by adding water, thereby obtaining a double emulsion structure that takes into account both stability and defoaming effectiveness, which is suitable for defoaming in a water system and can be dispersed more evenly.
[0030] Preferably, in S3, when the main component of the emulsifier is polyvinyl alcohol, it is first mixed with the deionized water at a concentration of 5% to prepare an emulsifier aqueous solution, and then the siloxane complex dispersion is added. The emulsifier is prepared as an aqueous solution in advance to avoid dehydration and etherification of the solid and loss of solubility, which can better protect the colloid and promote the emulsification and secondary emulsification process.
[0031] Compared with the prior art, the embodiments of the present invention have at least the following beneficial effects:
[0032] 1. In the preparation of the siloxane composite, the present invention adds a solid filler and a filler treatment agent, which can make the polydimethylsiloxane dispersed stably on the surface of the foaming system for a long time, and improve the continuity and stability of the defoaming effect while maintaining the defoaming performance.
[0033] 2. The present invention performs heat treatment on the filler before preparing the silicone composite, and utilizes high temperature to promote the formation of chemical bonds between the silicone compound and the solid filler, and the conversion of hydrogen bonds to chemical bonds occurs, which can effectively improve the defoaming effect and the emulsion stability during the phase transition process.
[0034] 3. The present invention adopts a secondary emulsification method, and the prepared defoamer has a double emulsion structure. When used for defoaming, it is evenly dispersed in the water system, and can take into account both stability and defoaming effectiveness; and the structure is stable, which significantly improves the storage time and heating stability of the defoamer. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0036] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other. The present invention will be described in detail below with reference to specific embodiments.
[0037] A composite organosilicon defoamer and a preparation method thereof, comprising the following steps:
[0038] S1: Heat treatment of filler: Add siloxane compound and solid filler into the reactor, heat the reactor to 150-180°C, stir for 4-7h, add catalyst, heat to 180-185°C, react for 2-7h to obtain the first mixed solution.
[0039] In this step, the catalyst includes: hydrogen-containing silicone oil or silane coupling agent. The catalyst is added after the stirring is completed to further enhance the bonding between the solid filler and the siloxane compound; further, the average particle size of the solid filler is limited to ≤25μm, preferably 5-15μm, the solid filler particle size is appropriate, the degree of dispersion in the foaming liquid is high, the stability is good, and it can form a basic defoaming unit with extremely small particles and a large number in the foaming liquid, so that the defoaming agent can achieve the best defoaming effect.
[0040] Furthermore, the siloxane compound is polydimethylsiloxane, and the mass ratio of the solid filler to the polydimethylsiloxane is less than or equal to 1:9, preferably 3:37, 1:9 or 1:24, which can improve the defoaming effect and reduce precipitation.
[0041] Furthermore, the solid filler is: fumed silica and silicone resin, and the mass ratio between the two is 8-3:7-3. Since both contain silanol bonds, the mass ratio of the two is limited to form a suitable number of hydrogen bonds with water molecules. When applied in a water system, it can promote the dispersion and stability of the first mixed liquid; and under the action of the solid filler and the filler treatment agent, under the premise of not changing the quality, the viscosity of the polydimethylsiloxane in the formula can be adjusted, or polydimethylsiloxanes of different single viscosities or two polydimethylsiloxanes with different viscosities can be used for compounding, so that the defoamer is not limited by the viscosity and temperature of the foaming system during use, so as to reduce the influence of the environment on the performance of the defoamer.
[0042] S2: Preparation of siloxane composite: Cool the first mixed solution to 60-70° C., add a filler treatment agent, maintain the reactor temperature at 50-75° C., and continue stirring for 0.5-1 h to obtain a siloxane composite.
[0043] In this step, the filler treating agent includes: oleic acid, low relative molecular weight linear polysiloxane or low relative molecular weight cyclic polysiloxane. Preferably, the mass of the filler treating agent is 1-2% of the mass of the above-mentioned siloxane compound, and can effectively prevent the filler from agglomerating when combined with the solid filler. Preferably, after adding the above-mentioned filler treating agent, the reactor temperature is maintained at 60-70°C for reaction, and the emulsification performance can be maintained at this temperature. A lower emulsification temperature may make emulsification difficult, while a higher emulsification temperature may cause the formed emulsion to break.
[0044] S3: Dispersion phase inversion: Add a dispersant to the above siloxane complex, wherein the above dispersant is: polyvinyl alcohol with a basicity of 54-89 mol%, preferably 86.0 mol%, maintain the reactor temperature at 60-70°C, stir at a speed of 250-500 r / min, stir for 0.5 h, and obtain a siloxane complex dispersion. Add an emulsifier and deionized water to the above siloxane complex dispersion in sequence, continue to maintain the reactor temperature at 60-70°C, stir at a speed of 10000-15000 r / min, stir for 0.5-1 h, and obtain a second mixed solution after phase inversion.
[0045] In this step, the emulsifier can be: a low concentration of polyvinyl alcohol aqueous solution, glycerol monostearate, tributyl phosphate, polyether or nonionic surfactant, wherein the nonionic surfactant includes: at least one of sorbitan fatty acid ester and polyoxyethylene sorbitan fatty acid ester, which can reduce the interfacial tension and help the droplet dispersion, thereby reducing the increase in interfacial area caused by emulsification, and further stabilizing the emulsion. And after adding the emulsifier and deionized water, reacting at 60-70°C can make the emulsifier better contact with the oil and water components, and the emulsification effect is better. At the same time, it can also destroy the cell structure of organic matter and accelerate the mixing effect; but too high a temperature will cause the liquid to deteriorate and affect the product quality.
[0046] Preferably, the emulsifier and deionized water can be prepared at a concentration of 5% to prepare an emulsifier aqueous solution and then add the above-mentioned siloxane complex dispersion, so that the emulsifier has good film-forming and emulsifying properties and can be used as a protective colloid during polymer emulsification. Since the glass transition temperature of the emulsifier (taking polyvinyl alcohol as an example) is 75-85°C, in actual application, if it is directly added in solid form, dehydration and etherification may occur, loss of solubility, etc.
[0047] S4: Secondary emulsification: Maintain the temperature of the second mixed liquid at 60-70°C. After the deionized water evaporates 5-10% of its mass fraction, add a corresponding amount of deionized water, maintain the reactor temperature at 60-70°C, and stir at a speed of 10000-15000 r / min for 0.5 h to obtain an emulsion.
[0048] In this step, the secondary emulsification realizes material encapsulation through multiple emulsifications. The first emulsification is to encapsulate the aqueous solution in the oil phase to form a primary emulsion. The multiple emulsifications are carried out by high-speed shearing, evaporation and adding water to make the emulsification continue. The primary emulsion is encapsulated in the water phase and converted from an oil-in-water state to a water-in-oil state, thereby obtaining a double emulsion that takes into account both stability and defoaming effect.
[0049] S5: Cooling: adding a thickener and additives to the emulsion, and cooling to room temperature to obtain an organosilicon defoaming agent.
[0050] In this step, the thickener may be: a high concentration of polyvinyl alcohol aqueous solution, carboxymethyl cellulose or methyl cellulose, which can increase the viscosity of the material system and keep the material system in a uniform and stable state; the additives include: mold growth inhibitors and antioxidants, which play a role in inhibiting fungi, antibacterial and antioxidant effects.
[0051] Example 1
[0052] S1: Add 9.6 g of polydimethylsiloxane, 0.28 g of fumed silica and 0.12 g of silicone resin into the reactor, heat the reactor to 180°C and stir for 2 h. During this process, add 0.01 g of silane coupling agent, heat to 180°C and react for 2 h.
[0053] S2: Cool the contents of the reactor to 90° C., add 0.2 g of oleic acid to the mixture after the filler heat treatment, maintain the reactor temperature at 90° C., and continue stirring for 0.5 h to obtain a siloxane composite.
[0054] S3: After adding the dispersant to the siloxane complex, maintain the reactor temperature at 70°C, the stirring speed at 15000 r / min, stir for 0.5 h, add 1.6 g of emulsifier (Span80: Tween80 = 3:2), slowly add 83 g of deionized water at 50°C, maintain the reactor temperature at 70°C, the stirring speed at 15000 r / min, and continue for 0.5 h.
[0055] S4: Maintain the temperature of the mixture system at 70°C, stir at a low speed for 10 minutes, and after volatilizing part of the water, add an equal amount of 50°C deionized water to the system, maintain the reactor temperature at 70°C, and stir at a speed of 15000 r / min for 0.5 hours to obtain an emulsion.
[0056] S5: Add 2 g of thickener and 0.1 g of mold growth inhibitor to the above emulsion, cool to room temperature, and obtain an organosilicon defoaming agent.
[0057] Embodiments 2 to 8
[0058] Embodiments 2 to 8 of the present invention are basically the same as Embodiment 1, and are implemented according to the technical scheme of the above specific implementation mode. The implementation conditions are shown in Table 1:
[0059] Table 1 Specific implementation conditions of Examples 1 to 8
[0060]
[0061]
[0062] Comparative Example 1
[0063] The implementation of Comparative Example 1 is basically the same as that of Example 1, except that the mass ratio of the solid filler to the polydimethylsiloxane in the raw materials is greater than 1:9, and the emulsification process is a single emulsification. The specific raw materials and proportions are shown in Table 2.
[0064] Comparative Example 2
[0065] The implementation of Comparative Example 2 is basically the same as that of Example 1, except that no catalyst and filler treatment agent are added, and the emulsification process is a single emulsification. The specific raw materials and proportions are shown in Table 2.
[0066] Comparative Example 3
[0067] The implementation of Comparative Example 3 is basically the same as that of Example 1, except that no solid filler is added. The specific raw materials and proportions are shown in Table 2.
[0068] Comparative Example 4
[0069] The implementation of Comparative Example 4 is substantially the same as that of Example 1, except that no heat treatment of the filler is performed.
[0070] The specific implementation conditions of Comparative Examples 1 to 2 are shown in Table 2:
[0071] Table 2 Specific implementation conditions of comparative examples 1 to 4
[0072]
[0073] Experimental example
[0074] Defoamer performance test method:
[0075] (1) The effectiveness of the defoamer was evaluated by foaming a 0.1% fatty alcohol sulfate solution.
[0076] Calculate the defoaming value:
[0077] Defoaming value = 100-(100∑h t / 4h a )
[0078] in:
[0079] ∑h t —The sum of the foam heights after 1 minute, 5 minutes, 15 minutes and 30 minutes;
[0080] h a —Foam height when bubbling stops (i.e. 0 min).
[0081] (2) A 0.1% aqueous solution of a polyoxyethylene derivative of sorbitan monooleate (Tween-80) was used as a standard foaming solution. 100 mL of the standard foaming solution was placed in a 250 mL bottle. One drop of defoaming agent was added and the bottle was covered and shaken for 10 minutes. The time it took for the foam to burst was measured.
[0082] The performance test results of the organosilane defoamers prepared in Examples 1 to 7 and Comparative Examples 1 to 2 are shown in Table 3:
[0083] Table 3 Performance test results of organosilane defoamers of Examples 1 to 8 and Comparative Examples 1 to 4
[0084]
[0085]
[0086] From the above, it can be seen that the defoaming agent prepared by the present invention has good stability and dispersibility while maintaining a good defoaming effect.
[0087] The embodiments described above are part of the embodiments of the present invention, rather than all of the embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the application claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
Claims
1. A composite organosilicon defoamer, the raw materials comprising: Silicone compounds, dispersants, emulsifiers and thickeners, characterized in that the raw materials also include: solid fillers, filler treatment agents, catalysts and additives.
2. A composite organosilicon defoamer according to claim 1, characterized in that: The mass ratio of the solid filler to the siloxane compound is less than or equal to 1:
9.
3. A composite organosilicon defoamer according to claim 1 or 2, characterized in that: The solid filler includes oxides of silicon, magnesium, zinc, aluminum, titanium and silicone resin.
4. A composite organosilicon defoamer according to claim 3, characterized in that: The solid filler is: fumed silica and silicone resin, and the mass ratio of the fumed silica to the silicone resin is 8-3:7-3.
5. A composite organosilicon defoamer according to claim 1 or 2, characterized in that: The average particle size of the solid filler is ≤25 μm.
6. The composite organosilicon defoamer according to claim 4, characterized in that: The average particle size of the fumed silica is 5 to 25 μm, and the average particle size of the silicone resin is 3 to 20 μm.
7. The composite organosilicon defoamer according to claim 1, characterized in that: The mass of the filler treatment agent is 1 to 3% of the mass of the siloxane compound.
8. A composite organosilicon defoamer according to claim 1 or 7, characterized in that: The filler treating agent includes: oleic acid.
9. The composite organosilicon defoamer according to claim 1, characterized in that: The catalyst accounts for 1-2.5% of the weight of the solid filler.
10. A composite organosilicon defoamer according to claim 1 or 9, characterized in that: The catalyst includes: hydrogen-containing silicone oil or a silane coupling agent.
11. The composite organosilicon defoamer according to claim 1, characterized in that: The dispersant is: a polyvinyl alcohol aqueous solution with a basicity of 54 to 89 mol%.
12. The composite organosilicon defoamer according to claim 1, characterized in that: The silicone compound is polydimethylsiloxane.
13. A method for preparing the composite organosilicon defoamer according to any one of claims 1 to 12, comprising emulsification, characterized in that: The solid filler is heat-treated, and the emulsification is secondary emulsification.
14. The method for preparing a composite organosilicon defoamer according to claim 13, characterized in that: The following steps are involved: S1: Heat treatment of filler: add the siloxane compound and the solid filler into the reactor, heat the reactor to 150-180° C., stir for 4-7 hours, add the catalyst, heat to 180-185° C., react for 2-7 hours, and obtain a first mixed solution; S2: preparing a siloxane composite: cooling the first mixed solution to 60-70° C., adding the filler treatment agent, maintaining the reactor temperature at 50-75° C., and continuously stirring for 0.5-1 h to obtain a siloxane composite; S3: Dispersion phase inversion: After adding the dispersant to the siloxane complex, maintain the reactor temperature at 60-70°C, stir at 250-500 r / min, stir for 0.5 h, and obtain a siloxane complex dispersion; sequentially add the emulsifier and deionized water to the siloxane complex dispersion; continue to maintain the reactor temperature at 60-70°C, stir at 10000-15000 r / min, stir for 0.5-1 h, and obtain a second mixed solution after phase inversion; S4: Secondary emulsification: maintaining the temperature of the second mixed liquid at 60-70° C., after the deionized water evaporates 5-10% of its mass fraction, adding a corresponding amount of deionized water, maintaining the reactor temperature at 60-70° C., stirring at a speed of 10000-15000 r / min, and continuing for 0.5 h to obtain an emulsion; S5: Cooling: adding the thickener and the additive to the emulsion, and cooling to room temperature to obtain the organosilicon defoaming agent.
15. The method for preparing a composite organosilicon defoamer according to claim 14, characterized in that: In S3: the emulsifier and the deionized water are mixed at a concentration of 5% to prepare an emulsifier aqueous solution, and then the siloxane complex dispersion is added thereto.
Citation Information
Patent Citations
Organic silicon emulsion defoaming agent
CN113491886A
Fluorosilicone powder defoaming agent and preparation method thereof
CN117753062A
High-temperature and strong alkali organic silicon antifoamer emulsion composition and preparing method thereof
CN1583212A
Organic silicon defoaming agent emulsifying device
CN217910161U