Preparation method of halloysite-based low-concentration styrene adsorption material
Through the preparation method of low-concentration styrene adsorption materials of Elosite-based low-concentration styrene adsorption materials, the adsorption capacity and stability of the adsorbent are improved, and the low adsorption capacity of the adsorbent in the prior art is solved. The problem of poor circulation performance achieves efficient adsorption and cyclic regeneration of styrene.
Patent Information
- Application Number
- CN202411559261.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-04
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, honeycomb activated carbon adsorbent has low adsorption capacity to styrene during the fiberglass production process, short effective use time, needs to be replaced frequently, and is difficult to meet increasingly stringent emission standards, affecting the environment and workers' health.
The preparation method of Elosite-based low-concentration styrene adsorption material is adopted, and the adsorption capacity and selectivity of the adsorbent are improved through steps such as acid activation, alkalization, organic modification outside the tube and ion deposition inside the tube, and the adsorption capacity and selectivity of the adsorbent are formed to form a high adsorption amount. A new type of adsorbent with fast adsorption rate and strong stability.
It realizes efficient adsorption of styrene, with better circulation performance than activated carbon, moderate cost, and easy to regenerate in situ, meeting the absorption needs of low content, high flow styrene-containing waste gas.
Smart Images

Figure CN119034679A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of volatile organic pollution control, and in particular to a method for preparing an inorganic-organic composite modified halloysite-based adsorbent. Background Art
[0002] Styrene is the main volatile organic pollutant (VOCs) in the exhaust gas emitted by the FRP production process. Its chemical formula is C 8 H 8 , insoluble in water, soluble in most organic solvents such as ethanol and ether. During the production process of FRP, especially in the mixing, coating and curing stages, styrene will be volatilized to form waste gas emissions. The emission of styrene-containing waste gas not only pollutes the environment, but may also cause irreversible harm to the health of operators.
[0003] In order to reduce the generation of waste gas and its negative impact on the environment, a variety of measures have been taken in the production process of FRP, such as using styrene volatilization inhibitors to reduce the volatilization of styrene at the source, and adopting effective waste gas collection and treatment solutions to treat the released waste gas. However, styrene volatilization inhibitors will affect the performance of FRP products to a certain extent, and adsorbents based on activated carbon or zeolite are often increasingly difficult to meet increasingly stringent emission standards due to reasons such as pore blockage. The "National Technical Guidance Catalogue for Pollution Prevention and Control (2024, Restricted and Eliminated Categories)" lists VOCs honeycomb activated carbon adsorption and purification technology without an in-situ regeneration system as an eliminated category. This is mainly because honeycomb activated carbon has low adsorption capacity, short effective use time, and needs to be replaced frequently: honeycomb activated carbon has low strength, is easy to break, is disposable, and is difficult to regenerate off-site. Therefore, there is an urgent industrial demand to explore higher adsorption capacity and renewable adsorbents.
[0004] Halloysite (abbreviated as: HNTs) is a natural mineral with unique structure and excellent performance. It has the advantages of abundant reserves, environmental friendliness and low price. 2 Si 2 O 5 (OH) 4 ·nH 2 O chemical structure of nano hollow tubes. The tubular structure of halloysite is a multilayer structure with a diameter of about 20-50 nanometers and a length of tens to hundreds of nanometers. The nanoscale structure of halloysite has a large specific surface area, so it exhibits strong adsorption properties. In addition, given the chemical composition of halloysite, it also has good thermal stability under high temperature conditions.
[0005] The surface structure of halloysite gives it a high specific surface area and abundant pores, providing a large number of active sites for adsorption. During the adsorption process, halloysite can effectively adsorb various pollutants by physical adsorption and chemical adsorption. It has shown great potential in the field of adsorption. It can be used for the adsorption and removal of organic pollutants, heavy metal pollutants, etc. in gas and liquid environments, and can also be used in oil-water separation, catalyst carriers and other fields. For organic pollutants, halloysite can adsorb organic molecules on its surface or inside by virtue of its surface active sites and pore structure. Halloysite also performs well in the adsorption of heavy metal ions. It can firmly adsorb heavy metal ions such as lead, mercury, cadmium, etc. through ion exchange, surface complexation and other effects. This is of great significance for the treatment of environmental problems caused by heavy metal pollution. In addition, halloysite also has good stability and regeneration. After proper treatment, the adsorbent can be regenerated and reused, reducing the cost of use and environmental burden.
[0006] However, due to the inorganic properties of the halloysite surface, natural halloysite has limited ability to adsorb organic matter. In addition, halloysite can also increase its adsorption capacity by preferably adding transition metals and olefin π-bonds to form complexes. Finally, the mineralization environment of natural halloysite is relatively complex, and it often coexists with other clay minerals. It also contains a small amount of other metal elements, such as iron, copper, calcium, etc. In view of this, whether halloysite is used as an adsorbent or in the field of catalyst, it must undergo certain purification, functional group modification and other treatments. In view of this, it is entirely possible to optimize and screen out a new adsorption material based on halloysite that has high adsorption capacity, fast adsorption rate, strong stability, good cycle performance, and can be prepared on a large scale at low cost. Summary of the invention
[0007] In view of the shortcomings in the prior art, the present invention provides a method for preparing a halloysite-based low-concentration styrene adsorption material, which solves the problems of low adsorption capacity, short effective use time, frequent replacement, low strength, easy breakage, one-time use, and difficulty in regeneration in the existing absorption technology for low-content and high-flow styrene-containing waste gas; the adsorbent has a high adsorption capacity, moderate cost, and is easy to be regenerated and reused in situ; the adsorbent uses natural halloysite as a raw material, and based on its unique multi-layer hollow nanotube structure, improves the adsorption capacity and adsorption rate of the material, especially the selective adsorption performance for styrene, through modification methods such as in-situ activation of acids inside and outside the tubes, condensation of hydroxyls outside the tubes, and ion deposition inside the tubes.
[0008] The object of the present invention is achieved by: a method for preparing a halloysite-based low-concentration styrene adsorption material, comprising the following steps: S1: Activation, acid-activating the halloysite at a set pH value to remove impurities and open the halloysite nanotube pipeline that may be blocked, and obtain acid-treated halloysite; S2: Alkalization, washing the halloysite obtained in S1 with deionized water, further neutralizing with an alkaline solution to a slightly alkaline state, centrifuging, and drying; obtaining halloysite with increased unsaturated oxygen atom charge sites on the surface; S3: Organic modification of the outer surface of the halloysite tube, spraying a mixed solution of a set amount of ethanol, tetraethyl orthosilicate, ammonia water and vinyltrimethoxysilane into the halloysite obtained in S2 under a set temperature, nitrogen protection and stirring to obtain preliminary organically modified halloysite; S4: Heating and curing. After the spraying and adding of the product obtained in S3 outside the tube is completed, the temperature is raised and stirred until it is completely dry to obtain the final product; the organically modified and cured halloysite is obtained; S5: In-tube adsorption, the halloysite obtained in S4 is added with Ag + The ion solution is stirred for a period of time, centrifuged, repeatedly washed with distilled water and centrifuged, and the washed sample is dried to form particles of a certain size to obtain the finished adsorbent.
[0009] Furthermore, in S1, the acid concentration during the acid activation process is 1-6 mol / L, the acid is hydrochloric acid, nitric acid, or sulfuric acid, the reaction temperature is 25-50°C, the activation time is 3-6h, and the specific surface area of the acid-treated and washed halloysite is increased by more than 63% compared with the raw halloysite.
[0010] Furthermore, the halloysite in S2 is washed with deionized water and then neutralized with an alkaline solution to a slightly alkaline state; the alkaline solution is sodium hydroxide, potassium hydroxide, or ammonia solution, and the concentration of the solution is 1%-5%; the drying process requires stirring, and the temperature is controlled at 90-105°C, and the halloysite powder is sufficient when it has strong fluidity. The final adsorbent obtained by drying at a relatively low temperature is the best.
[0011] Furthermore, the halloysite in S3 is sprayed with a mixed solution of a set amount of ethanol, tetraethyl orthosilicate, ammonia water and vinyltrimethoxysilane under a set temperature, nitrogen protection and stirring. The selected temperature is 40-60°C, and the final adsorbent obtained at 50°C is the best.
[0012] Furthermore, the mixed solution of ethanol, tetraethyl orthosilicate, ammonia water and vinyltrimethoxysilane sprayed into S3 uses nitrogen as the carrier gas, and each 100 mL of the mixed solution contains 5-15 mL of vinyltrimethoxysilane, 5-10 mL of tetraethyl orthosilicate, and 20-50 mL of ammonia water, and the rest is supplemented with ethanol to make up 100 mL. The best ratio of vinyltrimethoxysilane, tetraethyl orthosilicate, ammonia water and ethanol is 3:1:4:12.
[0013] Furthermore, the injection speed in S3 is controlled at 20-60 minutes, the injection temperature is 40-60 degrees Celsius, and the final adsorbent prepared at 50 degrees Celsius is optimal.
[0014] Furthermore, the temperature used for the curing in S4 is 50-70 degrees Celsius, and the curing time is 1-3 hours, and the final adsorbent obtained after 3 hours is the best.
[0015] Further, in S5, the halloysite powder obtained in S4 is added with Ag + In the deionized water solution of ions, the solution reaches adsorption equilibrium under vigorous stirring, containing Ag + The ion aqueous solution is composed of AgNO 3 Prepared with deionized water, calculated by weight as Ag + The ion content is 0.1-2%, with 2% Ag + The final adsorbent obtained by the ion content is the best.
[0016] Furthermore, the reaction time in S5 is based on Ag + The final adsorbent obtained by controlling the adsorption time between 30 and 60 minutes and 30 minutes is the best due to the different ion concentrations and the amount of halloysite used.
[0017] Furthermore, the adsorbed Ag in S5 + The halloysite after ionization is further centrifuged and repeatedly centrifuged and washed with distilled water. The washed sample is dried at a temperature of 90-95°C under nitrogen protection until fluidity appears, and then further dried for 2 hours. The powder is cooled to room temperature under nitrogen protection, and the obtained powder is formed into 80-100 mesh particles to obtain the finished adsorbent.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: using the experimental device tested by the present invention, the adsorbent prepared by the present invention has an adsorption capacity of styrene of 0.058g / g~0.072g / g; this data is close to the widely used activated carbon adsorbent; in addition, the adsorbent prepared by the present invention has a cyclic adsorption capacity of 0.058g / g~0.071g / g, which is much higher than 0.031 g / g of activated carbon, and it can be seen that the cyclic performance is much higher than that of activated carbon adsorbent. Moreover, the activation conditions are low and the cyclic regeneration is easy; in view of this, the present invention is expected to replace the original adsorbent on a large scale and can be used for the adsorption of low-content and high-flow styrene-containing waste gas. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0020] Figure 1 Flowchart of the present invention. DETAILED DESCRIPTION
[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Embodiment 1: A method for preparing a halloysite-based adsorbent for absorbing styrene-containing waste gas comprises the following steps: S1: Acid activation: weigh 10g of commercial halloysite sieved through 200 mesh on a balance, add it to the reaction container, then add 500mL of the prepared 3mol / L hydrochloric acid solution, disperse it by ultrasonic under mechanical stirring, and then continue to stir and react at 50℃ for 1 hour. Stop heating, stir until it cools to room temperature, and continue to stir for 1 hour. After filtering to remove the acid solution containing impurities, add deionized water for washing several times, and measure the pH of the filtrate until the pH value is between 6.0-7.0.
[0023] S2: Alkalization; continue to filter the halloysite obtained in S1, dry it slightly, and then transfer it to an alkali solution. In Example 1, the alkali solution is an ammonia solution with a pH value of 11.0. During the alkalization process, pay attention to the change in pH value, add a small amount of ammonia water as appropriate, and keep the pH value at 11.0 when the reaction is stopped. Filter and air dry until the halloysite becomes fluid, then continue to dry at 105°C for 6 hours under stirring to obtain halloysite with surface oxygen anion enhancement.
[0024] S3: Organic modification of the outer surface of the halloysite tube; 10g of the halloysite obtained in S2 was sprayed with a certain amount of a mixed solution of vinyltrimethoxysilane, ammonia water and ethanol (in Example 1, the amounts of the four substances in the 20mL mixed solution were: 3ml vinyltrimethoxysilane A-171, 1mL tetraethyl orthosilicate, 4mL ammonia water, 12mL ethanol) at 50°C under nitrogen protection and stirring. The preliminary organically modified halloysite was obtained. The spraying time was about 60 minutes, and the halloysite always maintained fluidity during the spraying process.
[0025] S4: Heating and curing; after the product obtained in S3 is sprayed and added, the temperature is raised to 60° C. and stirred until completely dry, and then the temperature is maintained for more than 30 minutes to obtain organically modified halloysite.
[0026] S5: In-tube adsorption: 10 g of the halloysite obtained in S4 was added with 50 ml of Ag-containing + ions in a solution (in Example 1, the solution used contained 0.2% Ag +ions), react at 25-30℃ with stirring for 60 minutes, centrifuge, wash repeatedly with deionized water and centrifuge, and vacuum dry the washed sample. The obtained powder sample is made into 80-100 mesh particles to obtain the adsorbent to be measured.
[0027] The adsorbent obtained in this example is marked as 3A171-HNTs -1% Ag-a, and 1g of the adsorbent is placed in the experimental adsorption device; high-purity nitrogen is used as the carrier gas, and the gas flow is controlled to pass through the styrene ethanol solution at a constant temperature to simulate the gas flow containing a certain styrene concentration, and the styrene concentration is determined by gas chromatograph. In this example, a 195ppm styrene gas flow is passed through the prepared adsorbent at a flow rate of 30mL / min. After the tail gas is stable, the tail gas styrene concentration is measured to be less than 5ppm. The styrene concentration in the tail gas is detected at intervals of hours, and the experiment is stopped when the styrene concentration is greater than 10ppm. This time is greater than 100h. Nitrogen is introduced, heated to 65°C for desorption, and activated in situ at the same time. The weight is reduced by 0.069g compared with before absorption and activation. This part of the weight can be regarded as the amount of styrene adsorbed by 1g of adsorbent. After in-situ heating activation, the operation is repeated three times, and the adsorption amount reaches 0.068g, indicating that the adsorbent has strong stability and good cycle performance.
[0028] Embodiment 2: A method for preparing a halloysite-based adsorbent for absorbing styrene-containing waste gas comprises the following steps: S1: Acid activation. Weigh 10g of commercial halloysite sieved through 200 mesh on a balance, add it to the reaction vessel, then add 500mL of the prepared 6mol / L hydrochloric acid solution, disperse it ultrasonically under mechanical stirring, and then continue to stir and react at 50°C for 1 hour. Stop heating, stir until it cools to room temperature, and continue stirring for 1 hour. After filtering to remove the acid solution containing impurities, add deionized water for washing several times, and measure the pH of the filtrate until the pH value is between 6.0-7.0.
[0029] The remaining S2-S5 processes are the same as those in Example 1.
[0030] The adsorbent obtained in this example is marked as 3A171-HNTs -1% Ag-b, and 1g of the adsorbent is taken and placed in the experimental adsorption device. Using high-purity nitrogen as the carrier gas, the gas flow is controlled to pass through the styrene ethanol solution at a constant temperature to simulate the gas flow containing a certain styrene concentration, and the styrene concentration is determined by gas chromatograph. In this example, a 195ppm styrene gas flow is passed through the prepared adsorbent at a flow rate of 30mL / min. After the tail gas is stabilized, the tail gas styrene concentration is measured to be less than 5ppm. The styrene concentration in the tail gas is detected at intervals of hours, and the experiment is stopped when the styrene concentration is greater than 10ppm. This time is greater than 100h. Nitrogen is introduced, heated to 65°C for desorption, and activated in situ at the same time. The weight is reduced by 0.063g compared with before absorption and activation. This part of the weight can be regarded as the amount of styrene adsorbed by 1g of adsorbent. After in-situ heating activation, the operation is repeated three times, and the adsorption amount reaches 0.060g, indicating that the adsorbent has strong stability and good cycle performance.
[0031] Embodiment 3: A method for preparing a halloysite-based adsorbent for absorbing styrene-containing waste gas comprises the following steps: S1: Acid activation. Same as Example 1.
[0032] S2: Alkalization. The halloysite obtained in S1 is further filtered and slightly dried, and then transferred to an alkali solution. In Example 1, the alkali solution is an ammonia solution with a pH value of 13.0. During the alkalization process, pay attention to the change in pH value, appropriately add a small amount of ammonia water, and keep the pH value at 13.0 when the reaction is stopped. Filter and air dry until the halloysite becomes fluid, then continue drying at 105°C for 6 hours under stirring to obtain halloysite with surface oxygen anion enhanced.
[0033] The remaining S3-S5 processes are the same as those in Example 1.
[0034] The adsorbent obtained in this example is marked as 3A171-HNTs -1% Ag-c, and 1g of the adsorbent is taken and placed in the experimental adsorption device. Using high-purity nitrogen as the carrier gas, the gas flow is controlled to pass through the styrene ethanol solution at a constant temperature to simulate the gas flow containing a certain styrene concentration, and the styrene concentration is determined by gas chromatograph. In this example, a 195ppm styrene gas flow is passed through the prepared adsorbent at a flow rate of 30mL / min. After the tail gas is stable, the tail gas styrene concentration is measured to be less than 5ppm. The styrene concentration in the tail gas is detected at intervals of hours, and the experiment is stopped when the styrene concentration is greater than 10ppm. This time is greater than 100h. Nitrogen is introduced, heated to 65°C for desorption, and activated in situ at the same time. The weight is reduced by 0.064g compared with before absorption and activation. This part of the weight can be regarded as the amount of styrene adsorbed by 1g of adsorbent. After in-situ heating activation, the operation is repeated three times, and the adsorption amount reaches 0.062g, indicating that the adsorbent has strong stability and good cycle performance.
[0035] Embodiment 4: A method for preparing a halloysite-based adsorbent for absorbing styrene-containing waste gas comprises the following steps: S1: Acid activation. Same as Example 1.
[0036] S2: Alkalization. The halloysite obtained in S1 is further filtered and slightly dried, and then transferred to an alkali solution. In Example 1, the alkali solution is a NaOH solution with a pH value of 11.0. During the alkalization process, pay attention to the change in pH value, appropriately add a small amount of NaOH solution, and when the reaction is stopped, the pH value is maintained at 11.0. Filter and air dry until the halloysite becomes fluid, then continue drying at 105°C for 6 hours with stirring to obtain halloysite with surface oxygen anion enhanced.
[0037] S3-S5: The process is the same as that in Example 1.
[0038] The adsorbent obtained in this example is marked as 3A171-HNTs -1% Ag-d, and 1g of the adsorbent is taken and placed in the experimental adsorption device. Using high-purity nitrogen as the carrier gas, the gas flow is controlled to pass through the styrene ethanol solution at a constant temperature to simulate the gas flow containing a certain styrene concentration, and the styrene concentration is determined by gas chromatograph. In this example, a 195ppm styrene gas flow is passed through the prepared adsorbent at a flow rate of 30mL / min. After the tail gas is stable, the tail gas styrene concentration is measured to be less than 5ppm. The styrene concentration in the tail gas is detected at intervals of hours, and the experiment is stopped when the styrene concentration is greater than 10ppm. This time is greater than 100h. Nitrogen is introduced, heated to 65°C for desorption, and activated in situ at the same time. The weight is reduced by 0.058g compared to before absorption and activation. This part of the weight can be regarded as the amount of styrene adsorbed by 1g of adsorbent. After in-situ heating activation, the operation is repeated three times, and the adsorption amount reaches 0.058g, indicating that the adsorbent has strong stability and good cycle performance.
[0039] Embodiment 5: A method for preparing a halloysite-based adsorbent for absorbing styrene-containing waste gas comprises the following steps: S1-S2: The process is the same as in Example 1.
[0040] S3: Organic modification of the outer surface of the halloysite tube. 10g of the halloysite obtained in S2 was sprayed with a certain amount of a mixed solution of vinyltrimethoxysilane, ammonia water and ethanol (in Example 5, the amounts of the four substances in the 20mL mixed solution were: 4ml vinyltrimethoxysilane A-171, 1mL tetraethyl orthosilicate, 4mL ammonia water, 11mL ethanol) at 50°C under nitrogen protection and stirring. The preliminary organically modified halloysite was obtained. The spraying time was about 60 minutes, and the halloysite always maintained fluidity during the spraying process.
[0041] S4-S5: The process is the same as in Example 1.
[0042] The adsorbent obtained in this example is marked as 4A171-HNTs -1% Ag-e, and 1g of the adsorbent is taken and placed in the experimental adsorption device. High-purity nitrogen is used as the carrier gas, and the gas flow is controlled to pass through the styrene ethanol solution at a constant temperature to simulate the gas flow containing a certain styrene concentration, and the styrene concentration is determined by gas chromatograph. In this example, a 195ppm styrene gas flow is passed through the prepared adsorbent at a flow rate of 30mL / min. After the tail gas is stable, the tail gas styrene concentration is measured to be less than 5ppm. The styrene concentration in the tail gas is detected at intervals of hours, and the experiment is stopped when the styrene concentration is greater than 10ppm. This time is greater than 100h. Nitrogen is introduced, heated to 65°C for desorption, and activated in situ at the same time. The weight is reduced by 0.065g compared with before absorption and activation. This part of the weight can be regarded as the amount of styrene adsorbed by 1g of adsorbent. After in-situ heating activation, the operation is repeated three times, and the adsorption amount reaches 0.064g, indicating that the adsorbent has strong stability and good cycle performance.
[0043] Embodiment 6: A method for preparing a halloysite-based adsorbent for absorbing styrene-containing waste gas comprises the following steps: S1-S4: The process is the same as in Example 1.
[0044] S5: In-tube adsorption. 10 g of the halloysite obtained in S4 was added with 50 ml of Ag-containing + ions in a solution (in Example 1, the solution used contained 0.4% Ag + ions), react at 25-30℃ with stirring for 60 minutes, centrifuge, wash repeatedly with deionized water and centrifuge, and vacuum dry the washed sample. The obtained powder sample is made into 80-100 mesh particles to obtain the adsorbent to be measured.
[0045] The adsorbent obtained in this example is marked as 3A171-HNTs -1%Ag-f, and 1g of the adsorbent is taken and placed in the experimental adsorption device. Using high-purity nitrogen as the carrier gas, the gas flow is controlled to pass through the styrene ethanol solution at a constant temperature to simulate the gas flow containing a certain styrene concentration, and the styrene concentration is determined by gas chromatograph. In this example, a 195ppm styrene gas flow is passed through the prepared adsorbent at a flow rate of 30mL / min. After the tail gas is stable, the tail gas styrene concentration is measured to be less than 5ppm. The styrene concentration in the tail gas is detected at intervals of hours, and the experiment is stopped when the styrene concentration is greater than 10ppm. This time is greater than 100h. Nitrogen is introduced, heated to 65°C for desorption, and activated in situ at the same time. The weight is reduced by 0.072g compared with before absorption and activation. This part of the weight can be regarded as the amount of styrene adsorbed by 1g of adsorbent. After in-situ heating activation, the operation is repeated three times, and the adsorption amount reaches 0.071g, indicating that the adsorbent has strong stability and good cycle performance.
[0046] Table 1 below shows the differences in various conditions and reagent amounts when optimizing the prepared adsorbent.
[0047]
[0048] Comparative Example 1: Directly use activated carbon with similar specific surface area as adsorbent to conduct adsorption and regeneration experiments.
[0049] Take 1g activated carbon (specific surface area 296m 2 / g) adsorbent is placed in the experimental adsorption device. Using high-purity nitrogen as the carrier gas, the gas flow is controlled to pass through the styrene ethanol solution at a constant temperature to simulate the gas flow containing a certain styrene concentration, and the styrene concentration is determined by gas chromatograph. In this example, a 195ppm styrene gas flow is passed through the activated carbon at a flow rate of 30mL / min. After the tail gas is stabilized, the tail gas styrene concentration is measured to be less than 5ppm. The styrene concentration in the tail gas is detected at intervals of hours, and the experiment is stopped when the styrene concentration is greater than 10ppm. This time is greater than 100h. Nitrogen is introduced and heated to 200℃ for desorption, and the desorption weight is 0.081g; this weight can be regarded as the amount of styrene adsorbed by 1g of activated carbon, but it is obvious that the desorption conditions are much more stringent than the embodiment. After heating and activation, the adsorption and desorption operations were repeated three times, and the adsorption amount was only 0.031g, indicating that the stability and cyclicity of the activated carbon adsorbent are relatively poor.
[0050] Comparative Example 2: Untreated halloysite was directly used as adsorbent, and adsorption and regeneration experiments were carried out under the same conditions.
[0051] Take 1g of halloysite adsorbent and put it into the experimental adsorption device. Use high-purity nitrogen as the carrier gas, control the gas flow rate through the styrene ethanol solution at a constant temperature, simulate the gas flow containing a certain styrene concentration, and use a gas chromatograph to determine the styrene concentration. In this case, a 195ppm styrene gas flow is passed through the activated carbon at a flow rate of 30mL / min. After the tail gas is stable, the tail gas styrene concentration is measured to be less than 5ppm. The styrene concentration in the tail gas is detected at intervals of hours, and the experiment is stopped when the styrene concentration is greater than 10ppm. This time is about 85h. Nitrogen is passed in, heated to 65℃ for desorption, and the desorption weight is 0.032g; this weight can be regarded as the amount of styrene adsorbed by 1g of halloysite, which is much less than. After heating and activation, the adsorption and desorption operations are repeated three times, and the adsorption amount is only 0.025g, indicating that the adsorption effect of halloysite as an adsorbent is poor without modification.
[0052] The following Table 2 illustrates the difference in the use effects of the products obtained by the preferred adsorbent preparation methods in combination with comparative adsorbents.
[0053]
[0054] Under the test conditions of the device used in the present invention, the adsorption amount of styrene by the prepared adsorbent is between 0.058g / g and 0.072g / g. This data is similar to that of the widely used activated carbon adsorbent, and is much higher than that of the halloysite raw material that has not been modified by organic-inorganic composite. In addition, the adsorbent prepared by the present invention far exceeds the activated carbon adsorbent in terms of cycle performance, and its cycle adsorption amount is in the range of 0.058g / g to 0.071g / g. After three cycles of use, the adsorption amount can be regarded as completely retained. After three cycles, the adsorption amount of activated carbon is only 0.031g / g, which is only 38% of the initial value. Furthermore, the activation conditions of the adsorbent prepared by the present invention are low, and the cycle regeneration is easy. It can be seen that the adsorbent prepared by the present invention is far superior to the activated carbon adsorbent used for styrene adsorption in terms of performance.
[0055] The organic-inorganic composite modified halloysite-based styrene adsorption material of the present invention can well solve the problems of adsorption activity and recycling when using activated carbon to adsorb low-concentration styrene. The present invention uses alkaline substances to change the charge composed of Si-OH on the inner and outer surfaces of the halloysite nanotubes from the original basic balance to the presence of more O negatively charged unsaturated sites, thereby enhancing the ability of the outer wall of the halloysite nanotube to react with the silane coupling agent vinyltrimethylsilane. The silane coupling agent reacts and solidifies on the halloysite surface by spraying, and the resulting halloysite surface contains a certain number of vinyl groups, thereby utilizing the affinity between organic matter and the interaction between olefin π bonds to facilitate the rapid adsorption of styrene on the halloysite surface. In the subsequent step of inorganic modification, Ag⁺ is deposited in the halloysite lumen. Ag + The outer empty orbital of the ion is easy to combine with the π orbital of the olefin in terms of energy and symmetry to form a π complex, which further enhances the adsorption performance of the adsorbent of the present invention on styrene. In view of this, the new adsorbent material prepared by the present invention based on halloysite with moderate adsorption amount, fast adsorption rate, strong stability and good cycle performance is reasonable in principle.
[0056] The above principles and embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a halloysite-based low-concentration styrene adsorption material, characterized in that: The following steps are involved: S1: Activation, acid-activating the halloysite at a set pH value to remove impurities and open the halloysite nanotube pipeline that may be blocked, thereby obtaining acid-treated halloysite; S2: Alkalization, washing the halloysite obtained in S1 with deionized water, further neutralizing with an alkaline solution to a slightly alkaline state, centrifuging, and drying; obtaining halloysite with increased unsaturated oxygen atom charge sites on the surface; S3: Organic modification of the outer surface of the halloysite tube, spraying a mixed solution of a set amount of ethanol, tetraethyl orthosilicate, ammonia water and vinyltrimethoxysilane into the halloysite obtained in S2 under a set temperature, nitrogen protection and stirring to obtain preliminary organically modified halloysite; S4: Heating and curing, after the product obtained in S3 is sprayed and added, heating and stirring until it is completely dry to obtain organically modified and cured halloysite; S5: In-tube adsorption, the halloysite obtained in S4 is added with Ag + The ion solution is stirred for a period of time, centrifuged, repeatedly washed with distilled water and centrifuged, and the washed sample is dried to form particles of a certain size to obtain the finished adsorbent.
2. The method for preparing a halloysite-based low-concentration styrene adsorption material according to claim 1, characterized in that: In S1, during the acid activation process, the acid concentration is 1-6 mol / L, the acid is hydrochloric acid, nitric acid, or sulfuric acid, the reaction temperature is 25-50° C., and the activation time is 3-6 h.
3. The method for preparing a halloysite-based low-concentration styrene adsorption material according to claim 1 or 2, characterized in that: The halloysite in S2 is washed with deionized water and then neutralized with an alkaline solution to be slightly alkaline; the alkaline solution is sodium hydroxide, potassium hydroxide, or ammonia solution, and the solution concentration is 1%-5%; the drying process requires stirring and the temperature is controlled at 90-105°C until the halloysite powder has strong fluidity.
4. The method for preparing a halloysite-based low-concentration styrene adsorption material according to claim 1 or 2, characterized in that: The halloysite in S3 is sprayed with a mixed solution of a set amount of ethanol, tetraethyl orthosilicate, ammonia water and vinyltrimethoxysilane under a set temperature, nitrogen protection and stirring, and the selected temperature is 40-60°C.
5. The method for preparing a halloysite-based low-concentration styrene adsorption material according to claim 1 or 2, characterized in that: The mixed solution of ethanol, tetraethyl orthosilicate, ammonia water and vinyl trimethoxysilane sprayed into S3 uses nitrogen as carrier gas. Every 100 mL of the mixed solution contains 5-15 mL of vinyl trimethoxysilane, 5-10 mL of tetraethyl orthosilicate, and 20-50 mL of ammonia water, and the rest is supplemented with ethanol to 100 mL.
6. The method for preparing a halloysite-based low-concentration styrene adsorption material according to claim 1 or 2, characterized in that: The injection speed in S3 is controlled at 20-60 minutes, and the injection temperature is 40-60 degrees Celsius.
7. The method for preparing a halloysite-based low-concentration styrene adsorption material according to claim 1 or 2, characterized in that: The temperature used for the heating and curing in S4 is 50-70 degrees Celsius, and the curing time is 1-3 hours.
8. The method for preparing a halloysite-based low-concentration styrene adsorption material according to claim 1 or 2, characterized in that: In S5, the halloysite powder obtained in S4 is added with Ag + In the deionized water solution of ions, the solution reaches adsorption equilibrium under vigorous stirring, containing Ag + The ionized aqueous solution is prepared by AgNO3 and deionized water, and the weight is Ag. + The ion content is 0.1-2%.
9. The method for preparing a halloysite-based low-concentration styrene adsorption material according to claim 1 or 2, characterized in that: The reaction time in S5 is based on Ag + The difference in ion concentration and the amount of halloysite used is controlled within 30-60 minutes.
10. The method for preparing a halloysite-based low-concentration styrene adsorption material according to claim 1 or 2, characterized in that: The adsorbed Ag in S5 + The halloysite after ionization is further centrifuged and repeatedly centrifuged and washed with distilled water. The washed sample is dried at a temperature of 90-95°C under nitrogen protection until fluidity appears, and then further dried for 2 hours. The powder is cooled to room temperature under nitrogen protection, and the obtained powder is formed into 80-100 mesh particles to obtain the finished adsorbent.
Citation Information
Patent Citations
Preparation method of chelating type ion exchange resin with natural halloysite nanotube (HNT) as matrix
CN102250347A
Modified halloysite, composite coating based on modified halloysite and preparation methods of modified halloysite and composite coating
CN111607283A
Deodorant, gas-permeable deodorized film and method of manufacturing the same
WO1994023764A1
Cited By
A production process of ammonium molybdate
CN119774659A
Carbon monoxide adsorbent and preparation method thereof
CN120618440A