Efficient preparation method of silicon-carbon negative electrode material applied to lithium battery
Through the process of silicon particle nano-sizing, graphite sintering and carbon coating, the internal stress problem caused by volume expansion of silicon-based anode materials in lithium batteries is solved, and the preparation of silicon-carbon anode materials with high capacity and high circulation performance is achieved, simplifying the The process and reduce costs.
Patent Information
- Application Number
- CN202411095821.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-29
AI Technical Summary
The existing silicon-based negative electrode materials are internal stressed in lithium batteries due to volume expansion, resulting in rupture and SEI film rupture, reducing service life, and the preparation process is complex and costly, making it difficult to achieve high capacity, high first-time Coulomb efficiency and high cycle performance. .
By nano-sizing silicon particles and sintering them with graphite negative electrode material, and then carbon coating is carried out, silicon carbon negative electrode powder is prepared, carbon coating is achieved using fluoropolymer combustion synthesis reaction, silicon content and performance indicators are adjusted, and the process is simplified. and reduce costs.
The high capacity of silicon carbon negative electrode materials, the first Coulomb efficiency and the number of cycles have been improved, the process flow has been simplified, the production cost has been reduced, and the internal stress problems caused by volume changes have been solved, which has improved the stability and environmental protection of the material. sex.
Smart Images

Figure CN119038520A_ABST
Abstract
Description
Technical field:
[0001] The present invention belongs to the technical field of new energy lithium batteries, and specifically relates to a method for preparing a silicon-carbon negative electrode material. Background technology:
[0002] With the continuous expansion of new energy application fields, the demand for lithium batteries has increased by leaps and bounds. In the current large-scale commercial application of lithium battery materials, the negative electrode material is still mainly artificial graphite. The capacity of artificial graphite negative electrode materials can reach more than 360mAh / g, which is close to its theoretical capacity, but it cannot meet the application needs. The theoretical gram capacity of silicon material is 4200mAh / g, which is more than ten times that of graphite. With the demand for increasing battery energy density, especially the urgent need to improve the range of electric vehicles, silicon-based negative electrode materials with high gram capacity have always been favored by the industry.
[0003] In actual applications, the huge volume expansion of silicon materials during the lithium insertion process (expansion coefficient of about 300%) induces great internal stress, and the internal stress is released during the lithium removal process. This repeated process will cause the silicon particles to rupture or even pulverize. At the same time, the SEI film on the surface of the silicon negative electrode will rupture as the volume of silicon changes, causing the SEI film to rupture and generate cyclically during the subsequent charging and discharging process, resulting in a large loss of active lithium, thereby reducing the service life. There are also problems such as low initial coulomb efficiency and poor conductivity, which will affect the application of silicon negative electrode materials.
[0004] At present, silicon negative electrode materials are reduced by nano-siliconization, carbon coating of silicon or adding silicon oxide to reduce the negative impact of volume changes. Silicon-based negative electrode materials can be obtained through a variety of preparation methods, mainly including chemical vapor deposition, mechanical ball milling, sol-gel method, etc. At present, the preparation process of silicon-based negative electrode materials is complicated compared with graphite negative electrode materials, and there are certain difficulties in large-scale production. The cost remains high, and the production process of each enterprise is different, and the products are not standardized at present.
[0005] In summary, it is necessary to develop a silicon-based negative electrode material with high capacity, high first coulombic efficiency and high cycle performance. Summary of the invention:
[0006] The technical problem to be solved by the present invention is to provide an efficient preparation method for silicon-carbon negative electrode materials used in lithium batteries. In the preparation process of the silicon-carbon negative electrode materials, the silicon particles are nanosized (≤100nm) and sintered into one with the graphite negative electrode material, and then a carbon coating process is performed to improve the performance of the silicon-carbon negative electrode materials in multiple dimensions such as gram capacity, first efficiency, number of cycles, and rate. It has certain advantages in performance, cost and stability of product scale production, and can achieve upgrading of existing products.
[0007] The object of the present invention is achieved in that:
[0008] A silicon-carbon negative electrode powder, the powder has a particle size of D10 (3-9 μm), D50 (10-18 μm), and D90 (22-32 μm) (laser diffraction method).
[0009] The main components of the silicon-carbon negative electrode powder are: silicon and carbon; the silicon content is 2%-55wt%, and the carbon content is 98%-45wt%.
[0010] 2-8wt% of the carbon is a product of combustion synthesis of fluoropolymer and silicon, and is coated on the surface of the silicon-carbon powder.
[0011] The raw materials of silicon-carbon negative electrode powder are: silicon powder (D50≤2.0μm, purity≥5N), graphite negative electrode powder (particle size D50≤15±μm), fluorine-containing polymer (particle size D50≤3.5μm); the molar ratio of silicon powder to fluorine-containing polymer is 1:1.2-6. The amount of graphite negative electrode powder is: the weight ratio of (silicon powder+fluorine-containing polymer) to graphite negative electrode powder is 1:0.5-3.
[0012] The above raw materials can be purchased directly in the market.
[0013] The fluorine-containing polymer powder is one or any combination of polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), polyvinyl fluoride (PVF), perfluoroalkyl (PFA), and perfluoroethylene propylene copolymer (FEP) (when it is any combination, it can be in any proportion).
[0014] The preparation method of the above-mentioned silicon-carbon negative electrode powder comprises the following steps: after mixing silicon powder, fluorine-containing polymer and graphite negative electrode powder uniformly by ball milling in the above-mentioned proportion, placing the mixture in a reaction container, evacuating (≤1Pa) to remove the air, passing argon gas (0.5-1.5MPa), adjusting the ventilation pressure according to the volume of the reaction materials, the ratio of the volume of the reaction materials to the volume of the reactor is 1:6-2, the ventilation pressure changes with the material ratio, and the pressure is arbitrarily adjusted between a maximum of 1.5MPa and a minimum of 0.5MPa, igniting the local mixed powder to initiate a combustion synthesis reaction.
[0015] For example, polytetrafluoroethylene (PTEF) and silicon powder react:
[0016]
[0017] Adding excess silicon powder and graphite negative electrode powder during the reaction process can obtain silicon-carbon composite powder, and the carbon generated by the reaction is coated on the surface of the silicon-carbon composite powder;
[0018]
[0019] After the reaction is completed, the gas in the reactor is introduced into a NaOH aqueous solution to remove the SiF4 gas.
[0020] SiF4↑+6NaOH=NasiO3+4NaF+3H2O
[0021] The silicon content in the reactants is measured, and the proportion of silicon in the powder is adjusted by adding graphite negative electrode powder to make the silicon content reach 2%-55wt%, thereby adjusting the gram capacity, first efficiency, tap density, specific surface area and other technical indicators of the silicon-carbon negative electrode material to meet the standards for commercial applications.
[0022] Silicon powder, fluorine-containing polymer powder and graphite negative electrode powder are placed in a planetary mixer for mixing according to the above-mentioned proportion range. The mixing medium is zirconia balls with a diameter of 3 to 10 mm. The mass ratio of zirconia balls to materials is 2:1 (or 1.5:1, 2.5:1, 3:1, etc.). The mixer speed is controlled to 800 rpm and the mixing time is 2 hours.
[0023] The gas phase conditions of the self-propagation synthesis reaction can be any atmosphere and any gas pressure; for example, the atmosphere can be argon gas with a gas pressure of 1 MPa.
[0024] Preferably, a tungsten wire is used to partially ignite the mixed raw materials to induce a combustion reaction, and the current is 10 to 50A.
[0025] The present invention has the following beneficial effects:
[0026] 1. The present invention uses micron silicon powder, fluorine-containing polymer and graphite negative electrode powder to achieve nano-scale silicon powder remaining from the reaction through combustion synthesis reaction.
[0027] 2. The high temperature generated during the reaction process can nano-size the silicon powder deposited on the graphite powder and sinter the two into a silicon-carbon composite powder.
[0028] 3. The carbon reduced from polytetrafluoroethylene is coated on the surface of the silicon-carbon composite powder to increase its conductivity.
[0029] 4. The silicon-carbon negative electrode material prepared by the present invention has excellent performance, simple process flow, short cycle, high efficiency, easy to obtain raw materials and easy to mass produce.
[0030] 5. The recovery of SiF4 gas by NaOH aqueous solution can solve the emission of harmful gases and achieve environmental protection and resource recycling. Description of the drawings:
[0031] Figure 1 is the XRD characterization result of the combustion synthesis product in Example 1 of the present invention;
[0032] Figure 2 This is the SEM characterization result of the combustion synthesis product in Example 1 of the present invention;
[0033] Figure 3 is the characterization result of the combustion synthesis product in Example 1 of the present invention;
[0034] Figure 4 These are the performance results of the first effect and cycle performance tests of the silicon-carbon negative electrode in Example 1 of the present invention;
[0035] Figure 5 is the XRD characterization result of the combustion synthesis product in Example 2 of the present invention;
[0036] Figure 6 This is the SEM characterization result of the product in Example 2 of the present invention;
[0037] Figure 7 This is the TEM characterization result of the product in Example 2 of the present invention;
[0038] Figure 8 These are the performance results of the first efficiency and cycle performance tests of the silicon-carbon negative electrode in Example 2 of the present invention. Specific implementation method:
[0039] In order to explain the present invention more clearly, the following is a preferred embodiment and the attached drawings. Figure 1-8 To further illustrate this description, it should be particularly noted that the following examples are only auxiliary explanations of the present invention and should not be used to limit the scope of protection of the present invention.
[0040] A silicon-carbon negative electrode powder, the powder has a particle size of D10 (3-9 μm), D50 (10-18 μm), and D90 (22-32 μm) (laser diffraction method).
[0041] The main components of silicon-carbon negative electrode powder are silicon and carbon, with silicon content of 2%-55wt% and carbon content of 98%-45wt%. 2-8wt% of the carbon is a product of combustion synthesis of fluoropolymer and silicon, which is coated on the surface of silicon-carbon powder.
[0042] The raw materials of silicon-carbon negative electrode powder are: silicon powder (D50≤2.0μm, purity≥5N), graphite negative electrode powder (particle size D50≤15±μm), fluorine-containing polymer (particle size D50≤3.5μm); the molar ratio of silicon powder to fluorine-containing polymer is 1:1.2-6. The amount of graphite negative electrode powder is: the weight ratio of (silicon powder+fluorine-containing polymer) to graphite negative electrode powder is 1:0.5-3.
[0043] The molar ratio of the silicon powder to the fluorine-containing polymer is 1:1.2 or 1:1.8 or 1:2.5 or 1:3 or 1:3.6 or 1:4.2 or 1:4.8 or 1:5 or 1:1.53 or 1:6.
[0044] The amount of graphite negative electrode powder used is: the weight ratio of (silicon powder + fluorine-containing polymer) to graphite negative electrode powder is 1:0.5 or 1:0.8 or 1:1.2 or 1:1.8 or 1:2.2 or 1:2.6 or 1:3.
[0045] The fluorine-containing polymer powder is one or any combination of polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), polyvinyl fluoride (PVF), perfluoroalkyl (PFA), and perfluoroethylene propylene copolymer (FEP) (when it is any combination, it can be in any proportion).
[0046] The preparation method of the above-mentioned silicon-carbon negative electrode powder comprises the following steps: after mixing silicon powder, fluorine-containing polymer and graphite negative electrode powder uniformly by ball milling in the above-mentioned proportion, placing the mixture in a reaction container, evacuating (≤1Pa) to remove the air, passing argon gas (0.5-1.5MPa), adjusting the ventilation pressure according to the volume of the reaction materials, the ratio of the volume of the reaction materials to the volume of the reactor is 1:6-2, the ventilation pressure changes with the material ratio, and the pressure is arbitrarily adjusted between a maximum of 1.5MPa and a minimum of 0.5MPa, igniting the local mixed powder to initiate a combustion synthesis reaction.
[0047] For example, polytetrafluoroethylene (PTEF) and silicon powder react:
[0048]
[0049] Adding excess silicon powder and graphite negative electrode powder during the reaction process can obtain silicon-carbon composite powder, and the carbon generated by the reaction is coated on the surface of the silicon-carbon composite powder;
[0050]
[0051] After the reaction is completed, the gas in the reactor is passed into a NaOH aqueous solution to remove the SiF4 gas;
[0052] SiF4↑+6NaOH=NasiO3+4NaF+3H2O
[0053] The silicon content in the reactants is measured, and the proportion of silicon in the powder is adjusted by adding graphite negative electrode powder to make the silicon content reach 2%-55wt%, thereby adjusting the gram capacity, first efficiency, tap density, specific surface area and other technical indicators of the silicon-carbon negative electrode material to meet the standards for commercial applications.
[0054] Silicon powder, fluorine-containing polymer powder and graphite negative electrode powder are placed in a planetary mixer for mixing according to the above-mentioned proportion range. The mixing medium is zirconia balls with a diameter of 3 to 10 mm. The mass ratio of zirconia balls to materials is 2:1 (or 1.5:1, 2.5:1, 3:1, etc.). The mixer speed is controlled to 800 rpm and the mixing time is 2 hours.
[0055] The gas phase conditions of the self-propagation synthesis reaction can be any atmosphere and any gas pressure; for example, the atmosphere can be argon gas with a gas pressure of 1 MPa.
[0056] Preferably, a tungsten wire is used to partially ignite the mixed raw materials to induce a combustion reaction, and the current is 10 to 50A.
[0057] Embodiment 1:
[0058] raw material:
[0059] Silica powder, D50≤2.0 micron, purity≥5N;
[0060] Polytetrafluoroethylene powder (D50≤3.5μm);
[0061] Graphite anode powder (D50 15±1.0μm, tap density ≥1.0g / cm 3 , specific surface area 1.±0.3 (㎡ / g));
[0062] Weigh 100 grams of polytetrafluoroethylene powder, 70 grams of silicon powder, and 230 grams of graphite negative electrode powder as raw material powder. The raw material powder and zirconia balls are placed in a drum mixer at a mass ratio of 1:2 and mixed for 2 hours. The mixed materials are poured into a porous stainless steel mold covered with carbon felt, and the mold is placed in a reactor. The reactor is evacuated to ≥1Pa, and then 1MPa argon is introduced. The local material is ignited by an energized tungsten wire to initiate a combustion synthesis reaction. During the reaction, the temperature rises, causing the pressure in the kettle to rise, up to 4MPa or more. After 90 seconds, the pressure drops to 1-1.5MPa, and the reaction process ends. Open the vent valve to pass the gas in the kettle into the sodium hydroxide aqueous solution, recover the SiF4 gas, and after the pressure in the kettle is balanced with the external pressure, close the vent valve, open the air inlet valve, pass compressed air to 0.5-1MPa, then close the air inlet valve, and open the vent valve to vent. Repeat this process 2-3 times, exhaust the SiF4 gas in the kettle, and then open the kettle door to take out the solid product of the reaction.
[0063]
[0064] Based on this calculation, the content of solid powder is:
[0065]
[0066] The drawings in the specification Figure 1 The XRD characterization results of the combustion synthesis products of this system in this embodiment are shown. According to the figure, the products contain carbon, silicon and a very small amount of silicon carbide. Figure 2 ) and TEM( Figure 3 ) characterization results show that silicon is mainly nano-scale spherical particles, which are coated on the graphite negative electrode material powder. And through SEM surface composition analysis, the surface of nano-scale silicon particles is coated with carbon, and through TEM characterization, it can be seen that the carbon coating state is in the form of floccules.
[0067] The above product was made into a lithium battery negative electrode and used in a half-button lithium battery for performance testing, and the following results were obtained:
[0068] Lithium battery model: CR2032;
[0069] Electrolyte: 1M LiPF6 in EC / DEC (VOL.=1:1) With 5% FEC;
[0070] Counter electrode: lithium sheet;
[0071] Working electrode: The amount of active material is 90 mg, CMC2200 is 6 mg, and conductive carbon black is 4 mg.
[0072]
[0073] Sample 2305-1 was taken as component A, and graphite negative electrode material was taken as component B, with A:B (weight ratio) = 42:58. They were mixed in a drum ball mill to form a silicon-carbon negative electrode material with a Si content of 6%. The negative electrode of the lithium battery was prepared and used for performance testing of a half-button lithium battery. The results are as follows:
[0074]
[0075] Embodiment 2:
[0076] raw material:
[0077] Silica powder, D50≤2.0, purity≥5N;
[0078] Polytetrafluoroethylene powder (D50≤3.5μm);
[0079] Graphite anode powder (D50 15±1.0μm, tap density ≥1.0(g / cm 3 ), specific surface area 13±0.3 (㎡ / g));
[0080] Weigh 100 grams of polytetrafluoroethylene powder, 150 grams of silicon powder, and 230 grams of graphite negative electrode powder as raw material powder. Place the raw material powder and zirconium oxide balls in a mass ratio of 1:2 in a drum mixer and mix for 2 hours. Pour the mixed materials into a porous stainless steel mold covered with carbon felt, and place the mold in a reactor. Evacuate the reactor to ≥1Pa, then introduce 1MPa argon gas, and use an energized tungsten wire to ignite local materials to initiate a combustion synthesis reaction. During the reaction, the temperature rises, causing the pressure in the kettle to rise, up to 4mPa or more. After 90 seconds, the pressure will reach 1-1.5mPa, and the reaction process is over. Open the vent valve to pass the gas in the kettle into the sodium hydroxide aqueous solution, recover the SiF4 gas, and after the pressure in the kettle is balanced with the external pressure, close the vent valve, open the air inlet valve, pass compressed air to 0.5-1mPa, then close the air inlet valve, and open the vent valve to vent. Repeat this process 2-3 times, exhaust the SiF4 gas in the kettle, and then open the kettle door to take out the solid product of the reaction.
[0081]
[0082] Based on this calculation, the content of solid powder is:
[0083]
[0084] Figure 5 The XRD characterization results of the combustion synthesis products of the system in this example are shown. Figure 6 This is the SEM characterization result of the product in this example. Figure 7 This is the TEM characterization result of the product in this example.
[0085] The above product was made into a lithium battery negative electrode and used in a half-button lithium battery for performance testing, and the following results were obtained:
[0086] Lithium battery model: CR2032;
[0087] Electrolyte: 1M LiPF6 in EC / DEC (VOL.=1:1) With 5% FEC;
[0088] Counter electrode: lithium sheet;
[0089] Working electrode: The amount of active material is 90 mg, CMC2200 is 6 mg, and conductive carbon black is 4 mg.
[0090]
[0091] Take sample 2305-2 as component A, and use graphite negative electrode material as component B, A:B (weight ratio) = 24.7:75.3, mix them in a drum ball mill to form a silicon-carbon negative electrode material with a Si content of 8%, prepare a lithium battery negative electrode, and use it for half-button lithium battery performance testing. The results are as follows:
[0092]
[0093] The above embodiments are provided to illustrate the technical feasibility of the present invention, and are not intended to limit the actual methods of the present invention. For those skilled in the art, other different forms of components and process variations can be made based on the above embodiments. It is not possible to cite all implementation schemes here, and all changes or modifications derived from the technical solutions of the present invention are still within the scope of protection of the present invention.
Claims
1. An efficient preparation method for silicon-carbon negative electrode materials used in lithium batteries, characterized in that: The raw materials used are: silicon powder, graphite negative electrode powder, and fluorine-containing polymer; Silicon powder, fluorine-containing polymer and graphite negative electrode powder are mixed uniformly by ball milling according to the above proportions, and then placed in a reaction container. After evacuation to remove air, argon gas is passed through, and the ventilation pressure is adjusted according to the volume of the reaction materials. The ventilation pressure changes with the material ratio, and the pressure is arbitrarily adjusted between a maximum of 1.5 MPa and a minimum of 0.5 MPa. The local mixed powder is ignited to initiate a combustion synthesis reaction; Adding excess silicon powder and graphite negative electrode powder during the reaction process can obtain silicon-carbon composite powder, and the carbon generated by the reaction is coated on the surface of the silicon-carbon composite powder; After the reaction is completed, the gas in the reactor is passed into a NaOH aqueous solution to remove the SiF4 gas; The silicon content in the reactants is measured, and the proportion of silicon in the powder is adjusted by adding graphite negative electrode powder so that the silicon content reaches 2%-55wt%.
2. The method for efficiently preparing silicon-carbon negative electrode materials for lithium batteries according to claim 1, characterized in that: The main components of silicon-carbon negative electrode powder are: silicon and carbon; the silicon content is 2%-55wt%, and the carbon content is 98%-45wt%; 2-8wt% of the carbon is the product of combustion synthesis of fluoropolymer and silicon, which is coated on the surface of the silicon-carbon powder.
3. The method for efficiently preparing silicon-carbon negative electrode materials for lithium batteries according to claim 1, characterized in that: The molar ratio of the silicon powder to the fluorine-containing polymer is 1:1.2-6; The amount of graphite negative electrode powder used is: the weight ratio of (silicon powder + fluorine-containing polymer) to graphite negative electrode powder is 1:0.5-3.
4. The method for efficiently preparing a silicon-carbon negative electrode material for a lithium battery according to claim 1 or 3, characterized in that: The fluorine-containing polymer powder is one or any combination of polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), polyvinyl fluoride (PVF), perfluoroalkyl (PFA), and perfluoroethylene propylene copolymer (FEP). When it is any combination, it can be in any proportion.
5. The method for efficiently preparing silicon-carbon negative electrode materials for lithium batteries according to claim 1 or 3, characterized in that: The gas phase conditions of the self-propagation synthesis reaction may be any atmosphere and any gas pressure.
6. The method for efficiently preparing silicon-carbon negative electrode materials for lithium batteries according to claim 1 or 3, characterized in that: A tungsten wire is used to ignite a portion of the mixed raw materials to induce a combustion reaction, with a current of 10 to 50A.
7. The method for efficiently preparing silicon-carbon negative electrode materials for lithium batteries according to claim 1, characterized in that: The ratio of the volume of the reaction material to the volume of the reactor is 1:6-2.
Citation Information
Patent Citations
Method for synthesizing high pure and ultra-fine beta-SiC powder by self-spread burning
CN101104516A
Method for synthesizing homogeneous nano silicon carbide powder by burning
CN101125653A
Preparation method of coated carbon-silicon negative electrode material
CN111960421A