Composite negative electrode material and preparation method thereof, negative electrode plate and sodium ion battery
By covering asphalt on the surface of activated carbon, closing the openings, and preparing composite negative electrode materials, the problem of poor performance of hard carbon and activated carbon materials in sodium ion batteries is solved, and the energy density and circulation performance of sodium ion batteries are improved.
Patent Information
- Application Number
- CN202411176342.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
The performance of existing sodium ion battery negative electrode materials is poor, especially the low first efficiency and low compaction of hard carbon, resulting in poor working performance, and the microporous structure of activated carbon leads to low Coulomb efficiency and large irreversible capacity.
The asphalt is coated on the surface of activated carbon by solid phase mixed coating, partial openings are closed, specific surface area is reduced, electrolyte contact sites are reduced, composite negative electrode materials are prepared, and applied to sodium ion batteries.
It improves the energy density and cycling performance of sodium ion batteries, inhibits irreversible sodium adsorption and electrolyte decomposition, and enhances the first-time Coulomb efficiency and reversible capacity.
Smart Images

Figure CN119038523A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a composite negative electrode material and a preparation method thereof, a negative electrode sheet and a sodium ion battery. Background Art
[0002] With the rapid development of renewable energy technology, the energy storage field is required to be more economical and safer; the widespread use of lithium-ion batteries has also led to an increasingly obvious problem of lithium resource scarcity, which will seriously restrict the development of the energy storage field in the future. Compared with lithium-ion batteries, sodium-ion batteries have the advantages of abundant reserves, wide distribution, and low cost, and are expected to become the mainstream in the future energy storage field, with more possibilities for development.
[0003] In terms of negative electrode materials for sodium-ion batteries, since the radius of sodium atoms is much larger than that of lithium atoms, the graphite structure originally suitable for the negative electrode of lithium-ion batteries is difficult to apply to the negative electrode of sodium-ion batteries. Amorphous carbon is considered to be a more suitable negative electrode material for sodium-ion batteries because of its good sodium storage capacity, high reversible specific capacity, good cycle performance, and obvious commercialization trend. Amorphous carbon can be divided into soft carbon and hard carbon. Soft carbon usually refers to carbon materials that can be graphitized after high-temperature treatment (above 2800°C). The disordered structure is easily eliminated, also known as easily graphitized carbon. Hard carbon usually refers to carbon that is difficult to completely graphitize even after high-temperature treatment (above 2800°C). Its disordered structure is difficult to eliminate at high temperatures, also known as difficult-to-graphitize carbon. Among them, hard carbon is currently the most widely selected negative electrode material for sodium-ion batteries due to its advantages such as good conductivity, high sodium storage capacity, small volume deformation after sodium insertion, environmental friendliness and low redox potential. However, the low initial efficiency and low compaction of hard carbon also limit its application. The working performance of sodium-ion batteries made of hard carbon is poor, so further regulation is needed.
[0004] Activated carbon has attracted much attention due to its high specific surface area, low cost, adjustable pore structure, good conductivity, electrochemical stability and thermal stability. However, there are a large number of micropores and mesopores inside activated carbon, with a specific surface area of 500-2000m 2 / g, directly using it as the negative electrode material of sodium ion batteries often has poor performance, and there are problems such as low first coulomb efficiency and large irreversible capacity during discharge. However, the microporous structure of activated carbon itself is conducive to sodium storage. Therefore, using activated carbon as a raw material to adjust the pore structure and prepare carbon materials through some methods can improve the sodium storage capacity of hard carbon negative electrodes. Summary of the invention
[0005] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a composite negative electrode material. The composite negative electrode material is obtained by coating a layer of asphalt on the surface of activated carbon through a solid phase mixed coating method, which can close some of the openings of the activated carbon, greatly reduce the specific surface area of the material, and reduce the active sites on the surface of the material that are in contact with the electrolyte. The composite negative electrode material is applied to a negative electrode plate, and the negative electrode plate is applied to a sodium ion battery. The sodium ion battery has high energy density and good cycle performance.
[0006] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0007] An embodiment of the first aspect of the present invention provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:
[0008] S101: After the activated carbon and asphalt are crushed separately, activated carbon fine powder and asphalt fine powder are prepared, and the activated carbon fine powder and asphalt fine powder are placed in a VC mixer for mixing to prepare a fine powder raw material;
[0009] S102: adding a cross-linking agent to the fine powder raw material, and then continuing to mix, and after the mixture is evenly mixed, performing a cross-linking reaction at a low temperature to prepare a precursor material;
[0010] S103: placing the precursor material in an inert gas atmosphere for high-temperature carbonization, and then cooling it to prepare a composite negative electrode material.
[0011] Furthermore, the activated carbon is any one or more of wood activated carbon, coal activated carbon, coconut shell activated carbon, and fruit shell activated carbon mixed in any proportion;
[0012] The asphalt is any one or more of petroleum asphalt, coal asphalt, and natural asphalt mixed in any proportion;
[0013] The cross-linking agent is any one of p-toluenesulfonic acid and terephthalaldehyde;
[0014] The inert gas is any one or more of nitrogen, helium and argon mixed in any proportion.
[0015] Further, the D50 of the activated carbon fine powder is not greater than 5 μm;
[0016] The D50 of the asphalt fine powder is not greater than 3 μm.
[0017] Furthermore, in step S101, in the fine powder raw material, the mass ratio of activated carbon fine powder to asphalt fine powder is (2-4):1.
[0018] Furthermore, in step S102, the mass ratio of the fine powder raw material to the cross-linking agent is 2:1.
[0019] Furthermore, in step S102, the cross-linking reaction temperature is 120-280°C, and the cross-linking reaction time is 2-10h.
[0020] Furthermore, in step S103, the high temperature carbonization temperature is 1200-1500°C, and the high temperature carbonization time is 2-5h.
[0021] An embodiment of the second aspect of the present invention provides a composite negative electrode material, which is prepared by the preparation method of the composite negative electrode material provided by the embodiment of the first aspect of the present invention.
[0022] The embodiment of the third aspect of the present invention provides a negative electrode sheet, which comprises, by mass percentage: 70-90% of composite negative electrode material and 10-30% of Super P-PVDF;
[0023] The composite negative electrode material is prepared by the preparation method of the composite negative electrode material provided by the embodiment of the first aspect of the present invention;
[0024] The Super P-PVDF is prepared by mixing ultrafine conductive carbon black and polyvinylidene fluoride in a mass ratio of 1:1.
[0025] An embodiment of the fourth aspect of the present invention provides a sodium ion battery, comprising the negative electrode plate provided by the embodiment of the third aspect of the present invention.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The present invention provides a composite negative electrode material, which is prepared by crushing activated carbon and asphalt into a certain size, mixing them, adding a cross-linking agent after mixing, mixing and cross-linking at a certain temperature to obtain a precursor material, and then carbonizing the precursor material at a high temperature to prepare a composite negative electrode material.
[0028] 2. The composite negative electrode material provided by the present invention is a composite negative electrode material in which a layer of asphalt is coated on the surface of activated carbon by a solid phase mixed coating method, which can close some of the openings of the activated carbon, greatly reduce the specific surface area of the material, and reduce the active sites on the surface of the material in contact with the electrolyte. The composite negative electrode material is applied to a negative electrode plate, and the negative electrode plate is applied to a sodium ion battery. The sodium ion battery has high energy density and good cycle performance.
[0029] 3. In the present invention, since asphalt coating on the surface of activated carbon can seal part of the open pores, the active sites on the surface of the material in contact with the electrolyte are reduced, thereby hindering part of the irreversible sodium adsorption, inhibiting the decomposition of the electrolyte, and reducing the occurrence of side reactions; in addition, after sealing a large number of open pores and turning them into closed pores, it is more conducive to the storage of sodium ions, thereby improving the initial coulombic efficiency and reversible capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0031] Figure 1 This is a schematic diagram of the first charge and discharge of a sodium ion battery prepared using the composite negative electrode material provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] An embodiment of the first aspect of the present invention provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:
[0034] S101: crushing the activated carbon and the asphalt respectively to prepare activated carbon fine powder and asphalt fine powder, wherein the D50 of the activated carbon fine powder is not greater than 5 μm, and the D50 of the asphalt fine powder is not greater than 3 μm;
[0035] Then, the activated carbon fine powder and the asphalt fine powder are placed in a VC mixer in a mass ratio of (2-4):1 to mix and prepare a fine powder raw material;
[0036] The activated carbon is any one or more of wood activated carbon, coal activated carbon, coconut shell activated carbon, and fruit shell activated carbon mixed in any proportion;
[0037] The asphalt is any one or more of petroleum asphalt, coal asphalt and natural asphalt mixed in any proportion;
[0038] S102: adding a crosslinking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the crosslinking agent is 2:1, and continuing to mix, after mixing evenly, performing a crosslinking reaction at 120-280° C. for 2-10 hours to prepare a precursor material;
[0039] Wherein, the cross-linking agent is any one of p-toluenesulfonic acid and terephthalaldehyde;
[0040] S103: placing the precursor material in an inert gas atmosphere for high-temperature carbonization, wherein the inert gas is any one or more of nitrogen, helium, and argon mixed in any proportion, the high-temperature carbonization temperature is 1200-1500°C, the high-temperature carbonization time is 2-5h, and after high-temperature carbonization, it is cooled to prepare a composite negative electrode material.
[0041] An embodiment of the second aspect of the present invention provides a composite negative electrode material, which is prepared by a preparation method of a composite negative electrode material provided by an embodiment of the first aspect of the present invention.
[0042] The embodiment of the third aspect of the present invention provides a negative electrode plate, which comprises, by mass percentage: 70-90% of composite negative electrode material and 10-30% of Super P-PVDF;
[0043] Wherein, the composite negative electrode material is prepared by the preparation method of the composite negative electrode material provided by the embodiment of the first aspect of the present invention;
[0044] Super P-PVDF is a mixture of ultrafine conductive carbon black and polyvinylidene fluoride in a mass ratio of 1:1.
[0045] The embodiment of the fourth aspect of the present invention further provides a sodium ion battery, comprising the negative electrode sheet provided by the embodiment of the third aspect of the present invention;
[0046] The sodium ion battery also includes an electrolyte, a separator and a positive electrode plate;
[0047] Specifically, the electrolyte uses EC (ethylene carbonate) and DEC (diethyl carbonate) as solvents and sodium hexafluorophosphate as solute. In the electrolyte, the volume ratio of EC and DEC is 1:1, and the concentration of sodium hexafluorophosphate is 1 mol / L.
[0048] The diaphragm is made of glass fiber;
[0049] The positive electrode is a sodium plate.
[0050] The following are specific examples. In the following examples, unless otherwise specified, all raw materials can be obtained from commercial sources.
[0051] In the following examples, the activated carbon is wood activated carbon, the asphalt is natural asphalt, the cross-linking agent is p-toluenesulfonic acid, and the inert gas is nitrogen.
[0052] Example 1
[0053] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:
[0054] S101: crushing the activated carbon and the asphalt respectively to prepare activated carbon fine powder and asphalt fine powder, wherein the D50 of the activated carbon fine powder is 5 μm, and the D50 of the asphalt fine powder is 3 μm;
[0055] Then, the activated carbon fine powder and the asphalt fine powder are placed in a VC mixer in a mass ratio of 3:1 to mix to prepare a fine powder raw material;
[0056] S102: adding a cross-linking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the cross-linking agent is 2:1, and continuing to mix, after being evenly mixed, heating to 160° C. at a rate of 2° C. / min, and keeping the temperature for 5 hours to complete the cross-linking reaction, thereby preparing a precursor material;
[0057] S103: placing the precursor material in an inert gas atmosphere, heating it to 1400°C at a heating rate of 5°C / min, keeping the temperature for reaction for 2 hours, completing high-temperature carbonization, and then cooling it to prepare a composite negative electrode material.
[0058] Example 2
[0059] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:
[0060] S101: crushing the activated carbon and the asphalt respectively to prepare activated carbon fine powder and asphalt fine powder, wherein the D50 of the activated carbon fine powder is 5 μm, and the D50 of the asphalt fine powder is 3 μm;
[0061] Then, the activated carbon fine powder and the asphalt fine powder are placed in a VC mixer in a mass ratio of 3:1 to mix to prepare a fine powder raw material;
[0062] S102: adding a cross-linking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the cross-linking agent is 2:1, and continuing to mix, after mixing evenly, heating to 120° C. at a rate of 2° C. / min, and keeping the temperature for 5 hours to complete the cross-linking reaction, thereby preparing a precursor material;
[0063] S103: placing the precursor material in an inert gas atmosphere, heating it to 900°C at a heating rate of 5°C / min, keeping the temperature for reaction for 3 hours, completing high-temperature carbonization, and then cooling it to prepare a composite negative electrode material.
[0064] Example 3
[0065] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:
[0066] S101: crushing the activated carbon and the asphalt respectively to prepare activated carbon fine powder and asphalt fine powder, wherein the D50 of the activated carbon fine powder is 5 μm, and the D50 of the asphalt fine powder is 3 μm;
[0067] Then, the activated carbon fine powder and the asphalt fine powder are placed in a VC mixer in a mass ratio of 3:1 to mix to prepare a fine powder raw material;
[0068] S102: adding a cross-linking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the cross-linking agent is 2:1, and then continuing to mix. After the mixture is evenly mixed, the mixture is heated to 280° C. at a rate of 2° C. / min, and kept at this temperature for 2 hours to complete the cross-linking reaction, thereby preparing a precursor material;
[0069] S103: placing the precursor material in an inert gas atmosphere, heating it to 1000°C at a heating rate of 5°C / min, keeping the temperature for reaction for 2 hours, completing high-temperature carbonization, and then cooling it to prepare a composite negative electrode material.
[0070] Example 4
[0071] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:
[0072] S101: crushing the activated carbon and the asphalt respectively to prepare activated carbon fine powder and asphalt fine powder, wherein the D50 of the activated carbon fine powder is 5 μm, and the D50 of the asphalt fine powder is 3 μm;
[0073] Then, the activated carbon fine powder and the asphalt fine powder are placed in a VC mixer in a mass ratio of 3:1 to mix to prepare a fine powder raw material;
[0074] S102: adding a cross-linking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the cross-linking agent is 2:1, and continuing to mix, after being evenly mixed, heating to 160° C. at a rate of 2° C. / min, and keeping the temperature for 5 hours to complete the cross-linking reaction, thereby preparing a precursor material;
[0075] S103: placing the precursor material in an inert gas atmosphere, heating it to 1100°C at a heating rate of 5°C / min, keeping the temperature for reaction for 2 hours, completing high-temperature carbonization, and then cooling it to prepare a composite negative electrode material.
[0076] Example 5
[0077] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:
[0078] S101: crushing the activated carbon and the asphalt respectively to prepare activated carbon fine powder and asphalt fine powder, wherein the D50 of the activated carbon fine powder is 5 μm, and the D50 of the asphalt fine powder is 3 μm;
[0079] Then, the activated carbon fine powder and the asphalt fine powder are placed in a VC mixer in a mass ratio of 3:1 to mix to prepare a fine powder raw material;
[0080] S102: adding a cross-linking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the cross-linking agent is 2:1, and continuing to mix, after mixing evenly, heating to 120° C. at a rate of 2° C. / min, and keeping the temperature for 5 hours to complete the cross-linking reaction, thereby preparing a precursor material;
[0081] S103: placing the precursor material in an inert gas atmosphere, heating it to 1200°C at a heating rate of 5°C / min, keeping the temperature for reaction for 2 hours, completing high-temperature carbonization, and then cooling it to prepare a composite negative electrode material.
[0082] Example 6
[0083] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:
[0084] S101: crushing the activated carbon and the asphalt respectively to prepare activated carbon fine powder and asphalt fine powder, wherein the D50 of the activated carbon fine powder is 5 μm, and the D50 of the asphalt fine powder is 3 μm;
[0085] Then, the activated carbon fine powder and the asphalt fine powder are placed in a VC mixer in a mass ratio of 3:1 to mix to prepare a fine powder raw material;
[0086] S102: adding a cross-linking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the cross-linking agent is 2:1, and continuing to mix, after being evenly mixed, heating to 160° C. at a rate of 2° C. / min, and keeping the temperature for 5 hours to complete the cross-linking reaction, thereby preparing a precursor material;
[0087] S103: placing the precursor material in an inert gas atmosphere, heating it to 1300°C at a heating rate of 5°C / min, keeping the temperature for reaction for 2 hours, completing high-temperature carbonization, and then cooling it to prepare a composite negative electrode material.
[0088] Example 7
[0089] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:
[0090] S101: crushing the activated carbon and the asphalt respectively to prepare activated carbon fine powder and asphalt fine powder, wherein the D50 of the activated carbon fine powder is 5 μm, and the D50 of the asphalt fine powder is 3 μm;
[0091] Then, the activated carbon fine powder and the asphalt fine powder are placed in a VC mixer in a mass ratio of 3:1 to mix to prepare a fine powder raw material;
[0092] S102: adding a cross-linking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the cross-linking agent is 2:1, and then continuing to mix. After the mixture is evenly mixed, the mixture is heated to 280° C. at a rate of 2° C. / min, and kept at this temperature for 2 hours to complete the cross-linking reaction, thereby preparing a precursor material;
[0093] S103: placing the precursor material in an inert gas atmosphere, heating it to 1500°C at a heating rate of 5°C / min, keeping the temperature for reaction for 2 hours, completing high-temperature carbonization, and then cooling it to prepare a composite negative electrode material.
[0094] Example 8
[0095] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:
[0096] S101: crushing the activated carbon and the asphalt respectively to prepare activated carbon fine powder and asphalt fine powder, wherein the D50 of the activated carbon fine powder is 5 μm, and the D50 of the asphalt fine powder is 3 μm;
[0097] Then, the activated carbon fine powder and the asphalt fine powder are placed in a VC mixer in a mass ratio of 2:1 to mix to prepare a fine powder raw material;
[0098] S102: adding a cross-linking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the cross-linking agent is 2:1, and continuing to mix, after being evenly mixed, heating to 160° C. at a rate of 2° C. / min, and keeping the temperature for 5 hours to complete the cross-linking reaction, thereby preparing a precursor material;
[0099] S103: placing the precursor material in an inert gas atmosphere, heating it to 1400°C at a heating rate of 5°C / min, keeping the temperature for reaction for 2 hours, completing high-temperature carbonization, and then cooling it to prepare a composite negative electrode material.
[0100] Example 9
[0101] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:
[0102] S101: crushing the activated carbon and the asphalt respectively to prepare activated carbon fine powder and asphalt fine powder, wherein the D50 of the activated carbon fine powder is 5 μm, and the D50 of the asphalt fine powder is 3 μm;
[0103] Then, the activated carbon fine powder and the asphalt fine powder are placed in a VC mixer in a mass ratio of 4:1 to mix to prepare a fine powder raw material;
[0104] S102: adding a cross-linking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the cross-linking agent is 2:1, and continuing to mix, after being evenly mixed, heating to 160° C. at a rate of 2° C. / min, and keeping the temperature for 5 hours to complete the cross-linking reaction, thereby preparing a precursor material;
[0105] S103: placing the precursor material in an inert gas atmosphere, heating it to 1400°C at a heating rate of 5°C / min, keeping the temperature for reaction for 2 hours, completing high-temperature carbonization, and then cooling it to prepare a composite negative electrode material.
[0106] Comparative Example 1
[0107] This comparative example provides a method for preparing a composite negative electrode material, which comprises the following steps:
[0108] The activated carbon was crushed to prepare activated carbon fine powder, wherein the D50 of the activated carbon fine powder was 5 μm; the activated carbon fine powder was heated to 1400°C at a heating rate of 5°C / min in a tubular furnace under a nitrogen atmosphere, and kept warm for reaction for 2 hours. After the reaction was completed, it was cooled to room temperature to prepare a negative electrode material.
[0109] The experimental conditions in Examples 1-9 and Comparative Example 1 are shown in Table 1.
[0110] Table 1
[0111]
[0112]
[0113] Performance Testing
[0114] The composite negative electrode materials prepared in Examples 1-9 and the negative electrode material prepared in Comparative Example 1 were used in a sodium ion battery, specifically:
[0115] The sodium ion battery comprises a negative electrode plate, an electrolyte, a separator and a positive electrode plate;
[0116] The composite negative electrode materials prepared in Examples 1 to 9 and the negative electrode materials prepared in Comparative Example 1 were mixed with SuperP-PVDF respectively to prepare a variety of mixed materials, wherein the mixed materials included 80% of the composite negative electrode materials and 20% of Super P-PVDF in terms of mass percentage, and the mixed materials were sheeted to prepare negative electrode sheets;
[0117] Super P-PVDF is made of ultrafine conductive carbon black and polyvinylidene fluoride mixed in a mass ratio of 1:1;
[0118] The electrolyte uses EC (ethylene carbonate) and DEC (diethyl carbonate) as solvents and sodium hexafluorophosphate as solute. In the electrolyte, the volume ratio of EC and DEC is 1:1, and the concentration of sodium hexafluorophosphate is 1 mol / L.
[0119] The diaphragm is made of glass fiber;
[0120] The positive electrode is a sodium plate;
[0121] The components of the above sodium ion battery: negative electrode plate, electrolyte, separator and positive electrode plate, were processed into CR2032 button batteries, and their performance was tested. The test conditions were: first 0.1C rate discharge, then 0.02mA constant current discharge, and then 0.1C rate charge test. The test results are shown in Table 1;
[0122] Table 1
[0123]
[0124]
[0125] It can be seen from the data in Table 1 that, compared with Comparative Example 1, the sodium ion batteries prepared using the composite negative electrode materials provided in Examples 1-9 have better reversible capacity and first efficiency (first efficiency) than those of the comparative example.
[0126] Figure 1 Schematic diagram of the first charge and discharge of a sodium ion battery prepared using the composite negative electrode material provided in Example 1.
[0127] The composite negative electrode material provided by the present invention is prepared by crushing activated carbon and asphalt into a certain size, mixing them, adding a cross-linking agent after mixing, mixing and cross-linking at a certain temperature to obtain a precursor material, and then carbonizing the precursor material at a high temperature to obtain a composite negative electrode material; the composite negative electrode material is applied to a negative electrode plate, and the negative electrode plate is applied to a sodium ion battery, and the prepared sodium ion battery has high energy density and good cycle performance.
[0128] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0129] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A method for preparing a composite negative electrode material, characterized in that: The preparation method comprises the following steps: S101: After the activated carbon and asphalt are crushed separately, activated carbon fine powder and asphalt fine powder are prepared, and the activated carbon fine powder and asphalt fine powder are placed in a VC mixer for mixing to prepare a fine powder raw material; S102: adding a cross-linking agent to the fine powder raw material, and then continuing to mix, and after the mixture is evenly mixed, performing a cross-linking reaction at a low temperature to prepare a precursor material; S103: placing the precursor material in an inert gas atmosphere for high-temperature carbonization, and then cooling it to prepare a composite negative electrode material.
2. The method for preparing a composite negative electrode material according to claim 1, characterized in that: The activated carbon is any one or more of wood activated carbon, coal activated carbon, coconut shell activated carbon, and fruit shell activated carbon mixed in any proportion; The asphalt is any one or more of petroleum asphalt, coal asphalt, and natural asphalt mixed in any proportion; The cross-linking agent is any one of p-toluenesulfonic acid and terephthalaldehyde; The inert gas is any one or more of nitrogen, helium and argon mixed in any proportion.
3. The method for preparing a composite negative electrode material according to claim 1, characterized in that: The D50 of the activated carbon fine powder is not greater than 5 μm; The D50 of the asphalt fine powder is not greater than 3 μm.
4. The method for preparing a composite negative electrode material according to claim 1, characterized in that: In step S101, in the fine powder raw material, the mass ratio of activated carbon fine powder to asphalt fine powder is (2-4):
1.
5. The method for preparing a composite negative electrode material according to claim 1, characterized in that: In step S102, the mass ratio of the fine powder raw material to the cross-linking agent is 2:
1.
6. The method for preparing a composite negative electrode material according to claim 1, characterized in that: In step S102, the cross-linking reaction temperature is 120-280°C, and the cross-linking reaction time is 2-10 hours.
7. The method for preparing a composite negative electrode material according to claim 1, characterized in that: In step S103, the high temperature carbonization temperature is 1200-1500°C, and the high temperature carbonization time is 2-5h.
8. A composite negative electrode material, characterized in that: The composite negative electrode material is prepared by the preparation method of the composite negative electrode material according to any one of claims 1 to 7.
9. A negative electrode plate, characterized in that: According to the mass percentage, it includes: composite negative electrode material 70-90%, SuperP-PVDF 10-30%; The composite negative electrode material is prepared by the preparation method of the composite negative electrode material according to any one of claims 1 to 7; The Super P-PVDF is prepared by mixing ultrafine conductive carbon black and polyvinylidene fluoride in a mass ratio of 1:
1.
10. A sodium ion battery, characterized in that: Including the negative electrode sheet as described in claim 9.
Citation Information
Patent Citations
Lignin-based carbon foams and composites and related methods
CA3005011A1
Sodium ion battery negative electrode material based on carbon material and pitch and preparation method and application thereof
CN109148838A
Oxidized asphalt-based hard carbon negative electrode material for sodium-ion battery and preparation method of oxidized asphalt-based hard carbon negative electrode material
CN115991467A
Sodium-ion battery carbon negative electrode material composite particle and preparation method and device thereof
CN116565199A