Preparation method of hard carbon negative electrode material
Through high-temperature carbonization and pyrolysis treatment of plant materials and high-conductive carbon nanotubes, a hard carbon negative electrode material with high conductivity is formed, which solves the reversible capacity and specific surface area of hard carbon materials in sodium ion batteries and improves the battery rate performance and cycle stability.
Patent Information
- Application Number
- CN202411181424.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-15
- Publication Date
- 2024-11-29
AI Technical Summary
The reversible capacity of hard carbon materials in sodium ion batteries is low and the specific surface area is too large, resulting in low initial Coulomb efficiency and affecting long cycle performance.
By carbonizing plant materials at high temperature, mixing high-conductive carbon nanotubes and pyrolysis and calcining multiple times, a hard carbon negative electrode material with high conductivity is formed, and the rate performance is improved.
The ion storage site, conductivity and rate performance of hard carbon anode materials are improved, internal resistance is reduced, and long cycle performance of sodium ion batteries is enhanced.
Smart Images

Figure CN119038524A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery materials, and in particular to a method for preparing a hard carbon negative electrode material. Background Art
[0002] With the depletion of fossil fuels and the intensification of environmental pollution, the use of renewable clean energy such as wind power and solar energy has attracted more and more attention. However, these renewable energy sources are affected by the natural environment and are volatile and intermittent, making it difficult to achieve stable output to the power grid. Energy storage systems are crucial to achieving efficient use of renewable energy. Among the many energy storage technologies, lithium-ion batteries have fully occupied the market of portable electronic devices and new energy electric vehicles due to their advantages such as high energy density, high power density, and long cycle life. However, the limited reserves and uneven distribution of lithium have restricted the large-scale application of lithium-ion batteries in energy storage. Sodium, which has similar physical and chemical properties to lithium, is abundant in reserves, widely distributed, and low in cost, making sodium-ion batteries have broad application prospects in large-scale power grid energy storage.
[0003] At present, hard carbon materials have the advantages of abundant raw material resources, low cost, and good rate performance, and are promising candidates for commercialization of negative electrode materials for sodium-ion batteries. However, hard carbon materials have problems such as low reversible capacity and large specific surface area, which will lead to low initial coulombic efficiency and other problems that affect the long-cycle performance of sodium-ion batteries. Summary of the invention
[0004] This case is a divisional application of patent number 202210045379.2, patent name: A hard carbon negative electrode material and its preparation method, application date: January 15, 2022.
[0005] In view of this, an object of the present invention is to provide a method for preparing a hard carbon negative electrode material. The hard carbon negative electrode material provided by the present invention has high ion storage sites, good electrical conductivity, low internal resistance, and high rate performance.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a hard carbon negative electrode material, comprising the following steps:
[0008] 1) Carbonizing the plant material at high temperature to obtain a porous material;
[0009] 2) mixing the porous material obtained in step 1), the first organic matter and the highly conductive carbon nanotubes and performing a first high-temperature pyrolysis to obtain a primary pyrolysis material;
[0010] 3) mixing the primary pyrolysis material obtained in step 2), the second organic matter and the highly conductive carbon nanotubes, and then performing a second high-temperature pyrolysis to obtain a secondary pyrolysis material;
[0011] 4) The secondary pyrolysis material obtained in step 3) is subjected to high temperature calcination to obtain a hard carbon negative electrode material.
[0012] Preferably, the plant material in step 1) is at least one of corn stalks, corn cobs, grapefruit peels, rice husks, walnut shells, cotton, chestnut shells, coconut shells, peanut shells, apricot shells, peach shells and sugarcane bagasse.
[0013] Preferably, in step 1), the carbonization temperature is 50-1000° C., and the carbonization time is 1-10 h.
[0014] Preferably, in step 2), the first organic matter comprises at least one of a resin material or an asphalt material.
[0015] Preferably, in step 2), the mass ratio of the porous material, the first organic matter and the highly conductive carbon nanotubes is 9:1:1.
[0016] Preferably, the temperature of the first high-temperature pyrolysis in step 2) is 200-2000° C. and the time is 1-10 h.
[0017] Preferably, the second organic matter in step 3) includes at least one of a resin material or an asphalt material.
[0018] Preferably, in step 3), the mass ratio of the primary pyrolysis material, the second organic matter and the highly conductive carbon nanotubes is 9.5:0.5:0.5.
[0019] Preferably, the temperature of high temperature calcination in step 4) is 1000-3000°C.
[0020] The present invention also provides a hard carbon negative electrode material prepared by the above preparation method.
[0021] Beneficial technical effects: The present invention provides a method for preparing a hard carbon negative electrode material, wherein a plant material is subjected to high-temperature carbonization to obtain a porous material, and organic pyrolysis carbon is embedded or attached to the inside or surface of the porous material through primary pyrolysis and secondary pyrolysis, and highly conductive carbon nanotubes are interspersed between the porous material and the pyrolysis carbon to form a good conductive network, and then calcined to form a partially parallel graphite structure with the highly conductive carbon nanotubes and the organic pyrolysis carbon, thereby improving the rate performance of the hard carbon negative electrode material. The carbon negative electrode material obtained by the preparation method of the present invention has high ion storage sites, good conductivity, low internal resistance, and high rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1This is the first charge and discharge curve of the button-type half-cell prepared in Example 1;
[0023] Figure 2 This is the pore size distribution diagram of the hard carbon negative electrode material prepared in Example 1. DETAILED DESCRIPTION
[0024] The present invention provides a method for preparing a hard carbon negative electrode material, comprising the following steps:
[0025] 1) Carbonizing the plant material at high temperature to obtain a porous material;
[0026] 2) mixing the porous material obtained in step 1), the first organic matter and the highly conductive carbon nanotubes and performing a first high-temperature pyrolysis to obtain a primary pyrolysis material;
[0027] 3) mixing the primary pyrolysis material obtained in step 2), the second organic matter and the highly conductive carbon nanotubes, and then performing a second high-temperature pyrolysis to obtain a secondary pyrolysis material;
[0028] 4) The secondary pyrolysis material obtained in step 3) is subjected to high temperature calcination to obtain a hard carbon negative electrode material.
[0029] The present invention carbonizes plant materials at high temperature to obtain porous materials.
[0030] In the present invention, the plant material is preferably at least one of corn stalks, corn cobs, grapefruit peels, rice husks, walnut shells, cotton, chestnut shells, coconut shells, peanut shells, apricot shells, peach shells and bagasse;
[0031] The high temperature carbonization atmosphere is preferably at least one of nitrogen, argon, hydrogen or oxygen;
[0032] The temperature of the high temperature carbonization is preferably 50 to 1000°C, more preferably 300 to 800°C, and most preferably 500 to 600°C;
[0033] The carbonization time is preferably 1 to 10 hours, more preferably 5 to 8 hours;
[0034] The high temperature carbonization equipment is preferably a tube furnace, a box furnace, a push plate furnace, a VCJ heating mixer, a tunnel furnace or a roller furnace;
[0035] The average pore diameter of the porous material is preferably 1 to 150 nm, more preferably 10 to 100 nm, and most preferably 50 to 80 nm;
[0036] The volume ratio of micropores, mesopores and macropores in the porous material is preferably 1: (50-100): (5-50), more preferably 1: (60-80): (20-30), and can be adjusted according to a specific process;
[0037] The BET specific surface area of the porous material is preferably 1 to 200 m2 / g, more preferably 50 to 150 m2 / g. 2 / g, most preferably 100m 2 / g;
[0038] The interlayer distance d002 value of the porous material is preferably 0.345 to 0.385, and more preferably 0.360 to 0.370.
[0039] After obtaining the porous material, the present invention mixes the obtained porous material, the first organic matter and the highly conductive carbon nanotubes and then performs a first high-temperature pyrolysis to obtain a primary pyrolysis material.
[0040] In the present invention, the first organic matter preferably includes at least one of a resin material or an asphalt material. The resin material of the present invention is preferably an epoxy resin, an acrylic resin, a polyester resin, a phenolic resin or an amino resin; the asphalt material is preferably petroleum asphalt or coal asphalt; the softening point of the asphalt material is preferably 80 to 280°C, more preferably 100 to 250°C, and most preferably 150 to 200°C. In the present invention, the particle size of the organic matter is preferably 1 to 500 nm, more preferably 50 to 400 nm, and most preferably 100 to 200 nm.
[0041] In the present invention, the mass ratio of the porous material, the first organic matter and the highly conductive carbon nanotubes is preferably 9:1:1.
[0042] In the present invention, the atmosphere of the first high-temperature pyrolysis is preferably nitrogen.
[0043] In the present invention, the temperature of the first high-temperature pyrolysis is preferably 200-2000°C, more preferably 500-1500°C, and most preferably 1000-1300°C; the equipment used for the first high-temperature pyrolysis is preferably a tubular furnace, a box furnace, a push plate furnace, a VCJ heating mixer, a tunnel furnace or a roller furnace.
[0044] The present invention uses the first high-temperature pyrolysis to embed or attach organic pyrolytic carbon into or on the surface of a porous material, and highly conductive carbon nanotubes are interspersed between the porous material and the pyrolytic carbon.
[0045] After obtaining the primary pyrolysis material, the present invention mixes the primary pyrolysis material, the second organic matter and the highly conductive carbon nanotubes and then performs a second high-temperature pyrolysis to obtain the secondary pyrolysis material.
[0046] In the present invention, the primary pyrolysis material is preferably crushed before mixing; the crushing equipment is preferably one or more of a jaw crusher, a hammer crusher, a toothed disc crusher, a double-roll crusher and a jet mill. The present invention has no particular limitation on the specific method of crushing, as long as the primary pyrolysis material can reach the desired particle size range.
[0047] In the present invention, the second organic matter preferably includes at least one of a resin material or an asphalt material. The resin material of the present invention is preferably at least one of an epoxy resin, an acrylic resin, a polyester resin, a phenolic resin and an amino resin; the asphalt material is preferably at least one of petroleum asphalt or coal asphalt; the softening point of the asphalt material is preferably 80 to 280°C, more preferably 100 to 250°C, and most preferably 150 to 200°C. In the present invention, the particle size of the organic matter is preferably 1 to 500nm, more preferably 50 to 400nm, and most preferably 100 to 200nm.
[0048] In the present invention, the mass ratio of the primary pyrolysis material, the second organic matter and the highly conductive carbon nanotubes is preferably 9.5:0.5:0.5.
[0049] In the present invention, the atmosphere of the second high-temperature pyrolysis is preferably nitrogen.
[0050] In the present invention, the temperature of the second high-temperature pyrolysis is preferably 200-2000°C, more preferably 500-1500°C, and most preferably 1000-1300°C; the equipment used for the second high-temperature pyrolysis is preferably a tubular furnace, a box furnace, a push plate furnace, a VCJ heating mixer, a tunnel furnace or a roller furnace.
[0051] After obtaining the secondary pyrolysis material, the present invention performs high-temperature calcination on the secondary pyrolysis material to obtain a hard carbon negative electrode material.
[0052] In the present invention, the calcination temperature is preferably 1000-3000°C, more preferably 1500-2500°C, and most preferably 2000-2300°C; the calcination time is preferably 1-10h, more preferably 5-8h; the calcination equipment is preferably a tube furnace, a box furnace, a push plate furnace, a tunnel furnace or a roller furnace; the calcination atmosphere is preferably nitrogen.
[0053] The invention uses calcination to form a partially parallel graphite structure with high-conductivity carbon nanotubes and organic pyrolysis carbon, thereby improving the rate performance of the hard carbon negative electrode material.
[0054] The present invention also provides a hard carbon negative electrode material prepared by the above preparation method.
[0055] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0056] Example 1
[0057] 1) Carbonizing the apricot shells at 500°C for 4 h in a N2 box furnace atmosphere furnace, introducing a nitrogen-oxygen mixed gas with a ratio of 5:1 when the temperature drops to 300°C, keeping the temperature for 1 h, and cooling naturally to obtain a porous carbonized material;
[0058] 2) The porous material is mixed with coal-based pitch with a softening point of 250°C and carbon nanotubes in a mass ratio of 9:1:1, pressed into blocks, and then pyrolyzed at 600°C for 2h in a N2 box atmosphere furnace and then naturally cooled to obtain a primary pyrolysis material;
[0059] 3) The primary pyrolysis material is crushed by a toothed disc crusher and a jet mill, and then mixed with coal-based asphalt with a softening point of 250°C and carbon nanotubes in a mass ratio of 9.5:0.5:0.5. After being carbonized at 600°C for 2 hours in a VCJ heating mixer filled with N2, the secondary pyrolysis material is naturally cooled.
[0060] 4) The secondary pyrolysis material is calcined at 1300° C. for 2 h in a N2 box atmosphere furnace, cooled naturally, and then sieved to obtain the high-capacity sodium ion battery hard carbon negative electrode material.
[0061] The negative electrode material prepared in Example 1 was prepared into a button-type half-cell. Figure 1 This is the first charge and discharge curve of the button-type half-cell prepared in Example 1. Figure 2 This is the pore size distribution diagram of the hard carbon negative electrode material prepared in Example 1.
[0062] Example 2
[0063] 1) Carbonizing the apricot shells at 1000°C for 1 hour in a N2 box furnace atmosphere furnace, introducing a nitrogen-oxygen mixed gas with a ratio of 5:1 when the temperature drops to 300°C, keeping the temperature for 1 hour, and cooling naturally to obtain a porous carbonized material;
[0064] 2) the porous material is mixed with coal-based pitch with a softening point of 280°C and carbon nanotubes in a mass ratio of 9:1:1, pressed into blocks, and then pyrolyzed at 2000°C for 1h in a N2 box atmosphere furnace and then naturally cooled to obtain a primary pyrolysis material;
[0065] 3) The primary pyrolysis material is crushed by a toothed disc crusher and a jet mill, and then mixed with coal-based asphalt with a softening point of 280°C and carbon nanotubes in a mass ratio of 9.5:0.5:0.5. After being carbonized at 2000°C for 1 hour in a VCJ heating mixer filled with N2, the secondary pyrolysis material is naturally cooled.
[0066] 4) The secondary pyrolysis material is calcined at 2000° C. for 2 h in a N2 box atmosphere furnace, cooled naturally, and then sieved to obtain the high-capacity sodium ion battery hard carbon negative electrode material.
[0067] Example 3
[0068] 1) Carbonizing the apricot shell at 8000°C for 3 h in a N2 box furnace atmosphere furnace, introducing a nitrogen-oxygen mixed gas with a ratio of 5:1 when the temperature drops to 300°C, keeping the temperature for 1 h, and cooling naturally to obtain a porous carbonized material;
[0069] 2) The porous material is mixed with coal-based pitch with a softening point of 150°C and carbon nanotubes in a mass ratio of 9:1:1, pressed into blocks, and then pyrolyzed at 800°C for 10 hours in a N2 box atmosphere furnace and then naturally cooled to obtain a primary pyrolysis material;
[0070] 3) The primary pyrolysis material is crushed by a toothed disc crusher and a jet mill, and then mixed with coal-based asphalt with a softening point of 280°C and carbon nanotubes in a mass ratio of 9.5:0.5:0.5. After being carbonized at 800°C for 10 hours in a VCJ heating mixer filled with N2, the secondary pyrolysis material is naturally cooled.
[0071] 4) The secondary pyrolysis material is calcined at 3000° C. for 1 h in a N2 box atmosphere furnace, cooled naturally, and then sieved to obtain the high-capacity sodium ion battery hard carbon negative electrode material.
[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a hard carbon negative electrode material, characterized in that: The following steps are involved: 1) Carbonizing the plant material at high temperature to obtain a porous material, wherein the average pore diameter of the porous material is 50-80 nm, wherein the volume ratio of micropores, mesopores and macropores in the porous material is 1:60-80:20-30, and the BET specific surface area of the porous material is 100 m 2 / g; the interlayer spacing d of the porous material 002 The value is preferably 0.360 to 0.
370. ; 2) mixing the porous material obtained in step 1), the first organic matter and the highly conductive carbon nanotubes and performing a first high-temperature pyrolysis to obtain a primary pyrolysis material; 3) mixing the primary pyrolysis material obtained in step 2), the second organic matter and the highly conductive carbon nanotubes, and then performing a second high-temperature pyrolysis to obtain a secondary pyrolysis material; 4) The secondary pyrolysis material obtained in step 3) is subjected to high temperature calcination to obtain a hard carbon negative electrode material.
2. The preparation method according to claim 1, characterized in that: In the step 1), the plant material is at least one of corn stalks, corn cobs, grapefruit peels, rice husks, walnut shells, cotton, chestnut shells, coconut shells, peanut shells, apricot shells, peach shells and sugarcane bagasse.
3. The preparation method according to claim 1, characterized in that: In the step 1), the carbonization temperature is 500-600° C., and the carbonization time is 5-8 hours.
4. The preparation method according to claim 1, characterized in that: In the step 2), the first organic matter includes at least one of a resin material or an asphalt material.
5. The preparation method according to claim 1, characterized in that: In the step 2), the mass ratio of the porous material, the first organic matter and the highly conductive carbon nanotubes is 9:1:
1.
6. The preparation method according to claim 1, characterized in that: The temperature of the first high temperature pyrolysis in step 2) is 200-2000° C. and the time is 1-10 hours.
7. The preparation method according to claim 1, characterized in that: In the step 3), the second organic matter includes at least one of a resin material or an asphalt material, and the temperature of the second high-temperature pyrolysis is preferably 1000-1300°C.
8. The preparation method according to claim 1, characterized in that: In the step 3), the mass ratio of the primary pyrolysis material, the second organic matter and the highly conductive carbon nanotubes is 9.5:0.5:0.
5.
9. The preparation method according to claim 1, characterized in that: The temperature of the high temperature calcination in step 4) is 2000-2300° C.; the calcination time is 5-8 hours.
Citation Information
Patent Citations
High-capacity sodium ion battery hard carbon negative electrode material and preparation method thereof
CN116207260A
Cited By
Hard carbon negative electrode material and preparation method thereof
CN120698442A
Hard carbon negative electrode material and preparation method thereof
CN120698442B