Precursor for improving uniformity of primary particles of single-crystal positive electrode material, single-crystal positive electrode material and preparation method of single-crystal positive electrode material
Patent Information
- Application Number
- CN202411216113.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-29
AI Technical Summary
[0006]本发明为了解决前驱体直接改善小单晶正极材料一次颗粒不均匀的问题,提供了一种改善单晶正极材料一次颗粒均匀性的前驱体,单晶正极材料及其制备方法
[0016] The present invention has the following advantages and beneficial effects: In the process of sintering the small single crystal cathode material of the present invention, under the action of lithium salt and flux, the precursor particles disintegrate and dissociate and the precursor primary particles recrystallize directly. From the morphology of the precursor It can improve the problem of uneven primary particles of small single crystal cathode materials after sintering, thereby affecting the morphology of single crystal cathode materials and the electrical properties of single crystal cathode materials, so that uniform primary particles of single crystal cathode materials can perform under long cycles. Better cycling performance.
Smart Images

Figure CN119038632A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion battery positive electrode materials, and specifically relates to a precursor for improving the uniformity of primary particles of a single crystal positive electrode material, a single crystal positive electrode material and a preparation method thereof. Background Art
[0002] The most commonly used method for commercial single crystal cathode materials is solid phase sintering of precursors and lithium salts. The morphology of the precursor plays a decisive role in the morphology of the cathode material, and the morphology of the cathode material plays a decisive role in the electrical properties. Therefore, the coprecipitation reaction of the precursor indirectly plays a decisive role in the electrical properties of the cathode material. The coprecipitation reaction of the precursor core and shell layer determines the morphology and physicochemical indicators of the precursor.
[0003] The patent document CN 112811477A discloses that in the process of preparing precursors by coprecipitation, many process conditions will affect the formation and growth of crystal nuclei, resulting in differences in the morphological characteristics and particle size distribution of the precursor particles. Secondly, the patent only points out that the sintering temperature of single-crystal ternary cathode materials is higher, the energy consumption is greater, and the requirements for dispersed and agglomerated single-crystal particles in post-processing are higher, without a detailed analysis of the specific reasons for how the internal and external structures of the precursor affect the sintering of single-crystal cathode materials.
[0004] The solid-phase sintering method of single-crystal cathode materials mostly follows the mechanism of dissolution-recrystallization, that is, the precursor polycrystalline secondary particles disintegrate under lithium salt and high temperature conditions, the agglomerated particles dissociate, and the precursor primary particles slowly grow into single crystal particles. Under lithium salt and high temperature conditions, the morphology of the precursor plays a decisive role in the dissolution energy and recrystallization energy, and the uniformity of the precursor primary particles has a greater impact on the single crystal primary particles. Therefore, it is crucial to make a precursor with uniform single crystal primary particles after sintering. The lower the energy of the precursor secondary particle dissociation energy and the primary particle recrystallization energy, the lower the sintering temperature of the single crystal cathode material. The primary sintering temperature plays a decisive role in the capacity and cycle of the single crystal cathode material.
[0005] The inner and outer layer morphology of the precursor of the present invention not only ensures that the tapping and specific surface of the precursor product meet the characteristics of uniform primary particles after sintering of small single crystals, but also reduces the dissolution energy of the precursor particles and the recrystallization energy of the primary particles when sintered with lithium salts. The large inner core layer of the precursor of the present invention is conducive to the dissociation of the precursor particles, and the uniformity of the precursor outer shell layer whiskers plays a role in ensuring the uniformity of the recrystallization of the single crystal primary particles. The high-voltage long-cycle performance of small single crystal positive electrode materials with uniform primary particles is superior to that of secondary spherical particle positive electrode materials, and there are currently no relevant reports in this regard. Summary of the invention
[0006] In order to solve the problem of using a precursor to directly improve the uneven primary particles of a small single crystal positive electrode material, the present invention provides a precursor for improving the uniformity of primary particles of a single crystal positive electrode material, a single crystal positive electrode material and a preparation method thereof.
[0007] The present invention adopts the following technical solution to solve the above technical problems: a precursor for improving the uniformity of primary particles of small single crystal positive electrode materials, whose chemical formula is Ni x Co y Mn 1-x-y (OH)2, where 0.6≤x<0.95, 0.05≤y≤0.15, the average particle size D50 of the precursor is 3.0~5.0μm, and the specific surface area is 10~15m 2 / g, the precursor includes an inner core layer and an outer shell layer, the inner core layer is an amorphous structure flocculent morphology, 35% of the precursor particle diameter ≤ the inner core layer diameter ≤ 60% of the precursor particle diameter, the outer shell layer is a loose and porous structure with uniform whisker thickness, the outer shell layer whisker thickness is 80~150nm and the whisker uniformity is good, the precursor particles have less twinning and the particles have good sphericity.
[0008] A method for preparing a precursor for improving the uniformity of primary particles of small single crystal positive electrode materials, characterized by the specific steps of: Step S1, preparing a mixed salt solution of transition metal nickel salt, cobalt salt and manganese salt, preparing an alkali solution as a precipitant solution, and preparing an ammonia solution as a complexing agent solution; Step S2, co-precipitation reaction of the inner core layer, a mixed salt solution, a precipitant solution and a complexing agent solution are simultaneously pumped into a sealed reactor containing a bottom liquid, the flow rate of the mixed salt solution is controlled to be 15-50 mL / min, the concentration of the precipitant in the mixed solution in the reactor is controlled to be 2-5 g / L, the concentration of the complexing agent is controlled to be 2-3.5 g / L, the pH of the mixed solution is controlled to be 10.0-11.5, and a mixed gas of oxygen and nitrogen is introduced, and a nucleation co-precipitation reaction is carried out under the conditions of a temperature of 40-60° C. and a stirring rate of 500-1000 r / min, and the reaction is stopped when 35% of the diameter of the precursor particle is ≤ the diameter of the inner core layer ≤ 60% of the diameter of the precursor particle. The proportion of oxygen in the mixed gas of oxygen and nitrogen is used to control the degree of oxidation of the precursor in the nucleation stage, and the degree of oxidation determines the morphology of the inner core layer. The volume ratio of oxygen to nitrogen in the mixed gas of oxygen and nitrogen is 1:20-30; Step S3, after the coprecipitation reaction of the outer shell layer and the inner core layer react to the target particle size, the flow rate of the precipitant solution and the complexing agent solution is changed to adjust the concentration of the precipitant in the mixed solution in the reactor to be controlled to 5-7 g / L, and the concentration of the complexing agent is controlled to be 4-6 g / L. At this time, the pH of the mixed solution is controlled to be 11.0-12.5, the reaction temperature remains unchanged, and the stirring rate of the reactor remains unchanged. The coprecipitation reaction of the outer shell layer is controlled by adjusting the ratio of the mixed gas of oxygen and nitrogen and the flow rate of the precipitant solution and the complexing agent solution to generate an outer shell layer that is obviously different from the morphology of the inner core layer, and the whisker thickness range and whisker uniformity are controlled. The volume ratio of oxygen to nitrogen in the mixed gas of oxygen and nitrogen is 1:40-50. When the average particle size of the precursor D50 is 3-5 μm, the feeding is stopped and the reactor is opened to discharge the precursor slurry. Step S4, filtering, washing, drying and sieving the obtained precursor slurry to obtain a precursor for improving the uniformity of primary particles of small single crystal positive electrode materials.
[0009] Furthermore, the concentration of the mixed salt solution in step S1 is 1.5-2 mol / L, the nickel salt in the mixed salt solution is one or more of nickel sulfate, nickel chloride or nickel nitrate, the cobalt salt is one or more of cobalt sulfate, cobalt chloride or cobalt nitrate, and the manganese salt is one or more of manganese sulfate, manganese chloride or manganese nitrate; the concentration of the alkali in the precipitant solution is 2-8 mol / L, and the alkali used is one or more of sodium hydroxide or potassium hydroxide; the concentration of ammonia in the complexing agent solution is 0.1-4 mol / L.
[0010] A lithium-ion battery single crystal positive electrode material, whose chemical formula is Li 1.005-1.10 Ni x Co y Mn 1-x-y MO2@DO, wherein 0.8 μm ≤ the short side diameter of the primary particle of the single crystal positive electrode material ≤ 2 μm, 0.6 ≤ x < 0.95, 0.05 ≤ y ≤ 0.15, M is one or more of Zr, Sr, Ti, W, Mg, Y, La, B or F, and D is one or more of Co, Li, B, W, Ti or Zr.
[0011] A method for preparing a single crystal positive electrode material for a lithium ion battery, characterized in that: a precursor prepared as above for improving the uniformity of primary particles of a small single crystal positive electrode material is used, the obtained precursor is mixed evenly with a lithium salt and an additive, and then the single crystal positive electrode material for a lithium ion battery is obtained by primary sintering, crushing, pulverizing, coating, secondary sintering, and sieving in sequence, wherein the lithium salt is one or more of lithium hydroxide, lithium carbonate, or lithium chloride, the additive is one or more of compounds containing Zr, Sr, Ti, W, Mg, Y, La, B, or F, and the coating agent used in the coating process is one or more of an oxide containing a D element or a lithium compound containing a D element, wherein the D element is one or more of Al, Co, Li, B, W, Ti, or Zr.
[0012] Furthermore, the feed ratio of the precursor and the lithium salt satisfies the molar ratio of (Ni+CO+Mn):Li of 1:1.005-1.105, and the amount of the additive added is 0.1wt%-2wt% of the total mass of the precursor and the lithium salt.
[0013] Furthermore, the primary sintering process is calcined in stages in an oxygen atmosphere furnace, the temperature of the first dehydration stage is 50~200°C, the insulation time is 2~4h, the temperature of the second dehydration stage is 350~450°C, the insulation time is 2~4h, the temperature of the third oxide curing reaction is 800~1000°C, the insulation time is 6~10h, the three stages are heated at a heating rate of 2~5°C / min, the oxygen content in the atmosphere furnace is 85%~95%, and finally a primary sintered matrix is obtained.
[0014] Furthermore, the specific process of the coating is: crushing the obtained primary sintered matrix, sieving the crushed matrix and mixing it evenly with the coating agent, wherein the coating agent is 0.01wt%-5wt% of the mass of the matrix after drying.
[0015] Furthermore, the secondary sintering process is sintering at 500-600° C. for 2-4 hours in an air atmosphere.
[0016] The present invention has the following advantages and beneficial effects: the present invention improves the problem of uneven primary particles of small single crystal positive electrode materials after sintering directly from the precursor morphology itself based on the principle that the precursor disintegrates and dissociates and the precursor primary particles recrystallize under the action of lithium salt and flux during the sintering process of small single crystal positive electrode materials, thereby affecting the morphology of single crystal positive electrode materials and the electrical properties of single crystal positive electrode materials, so that uniform single crystal positive electrode material primary particles can exert better cycle performance under long cycles. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a SEM of the surface of the precursor used in Example 1 to improve the uniformity of primary particles of small single crystal positive electrode materials.
[0018] Figure 2 This is the SEM image of the positive electrode material sintered in Example 1.
[0019] Figure 3 This is the argon ion SEM of the small single crystal positive electrode material precursor of comparative example 1.
[0020] Figure 4 This is the SEM image of the positive electrode material sintered in Comparative Example 1. DETAILED DESCRIPTION
[0021] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention. Example 1
[0022] Nickel sulfate, cobalt sulfate and manganese sulfate were prepared into a mixed salt solution with a total ion concentration of 1.5 mol / L according to a molar ratio of 60:10:30, a 4 mol / L sodium hydroxide solution was prepared as a precipitant solution, and a 4 mol / L ammonia solution was prepared as a complexing agent solution.
[0023] Deionized water was added to a 50L closed reactor, and the temperature of the liquid in the reactor was maintained at 50°C by heating with a constant temperature water tank. The stirring was turned on and the speed was adjusted to 550r / min. At the same time, a mixed salt solution, a precipitant solution and a complexing agent solution were pumped into the reactor, wherein the flow rate of the mixed salt solution was 25mL / min, the ammonia concentration in the reactor was controlled to be 3g / L, the alkali concentration in the reactor was controlled to be 4g / L, the pumping rate of the precipitant solution was adjusted by a metering pump to keep the pH of the coprecipitation reaction at 10.5-10.7, and a mixed gas of oxygen and nitrogen with a volume ratio of 1:25 was introduced below the liquid level in the reactor, and the flow rate of the mixed gas was 0.25m 3 / h, oxygen is used to control the morphology of the precursor nucleation stage, and the degree of oxidation determines the morphology of the core. The coprecipitation reaction is stopped when the core grows to a D50 of 1.8-2.0μm.
[0024] The constant temperature water tank is still used to heat the reactor to maintain the liquid temperature at 50°C, the stirring speed is still 550r / min, and the mixed salt solution, precipitant solution and complexing agent solution are pumped into the reactor at the same time. The flow rate of the mixed salt solution is 25mL / min, the ammonia concentration in the reactor is controlled to be 5g / L, the alkali concentration in the reactor is 6.5g / L, and the precipitant solution pumping rate is adjusted by a metering pump to keep the pH of the coprecipitation reaction at 11.3-11.5. A mixed gas of oxygen and nitrogen with a volume ratio of 1:45 is introduced below the liquid level in the reactor, and the flow rate of the mixed gas is 0.2m 3 / h, the coprecipitation reaction generates an outer shell layer that is significantly different from the inner core layer morphology, and controls the whisker thickness range and whisker uniformity. When the average particle size of the precursor D50 is 3-5μm, stop adding materials and open the reactor to discharge the precursor slurry.
[0025] The precursor slurry was put into an aging kettle; it was stirred for 4 hours under nitrogen protection conditions, and then the precursor slurry introduced into the aging kettle was washed in a centrifuge and the water was thrown out to obtain a precursor to be dried, and the precursor to be dried was placed in a blast drying oven, the drying temperature was set to 100°C, the drying time was 16 hours, and then passed through a 200-mesh sieve to obtain a precursor with a nickel:cobalt:manganese molar ratio of 60:10:30, and the average particle size D50 of the precursor was 4.104 μm, and the BET was 10.08 m 2 / g, and the whisker thickness is 105.26~143.78nm.
[0026] The obtained Ni 0.60 Co 0.10 Mn 0.30 The (OH)2 nickel-cobalt-manganese precursor was cut and the cross-sectional morphology was observed using a field emission scanning electron microscope. The whisker thickness of the cross-sectional whisker was measured using NanoMeasurer1.2 on an argon ion surface SEM. Figure 1 , the whisker thickness test data is shown in Table 1.
[0027] Table 1 is the argon ion polishing SEM whisker thickness test data of the precursor for improving the uniformity of primary particles of small single crystal positive electrode materials in Example 1: Table 1
[0028] The obtained Ni 0.60 Co 0.10 Mn 0.30 The (OH)2 precursor is mixed with lithium salt and additives, wherein the lithium salt is LiOH, the additive is ZrO2, LiOH and Ni 0.60 Co 0.10 Mn 0.30 The molar ratio of (OH)2 is 1.065:1, and ZrO2 accounts for 1.065:1 of LiOH and Ni 0.60 Co 0.10 Mn 0.300.2wt% of the total mass of (OH)2 is added to the high-speed mixer for mixing, and the mixing time is 15min. The mixed materials are sintered for the first time at 150℃ for 3h under oxygen atmosphere, and then sintered for the second time at 450℃ for 3h, and then sintered for the third time at 980℃ for 8h. The three sinterings are heated at a heating rate of 3℃ / min, and the oxygen content in the atmosphere furnace is 85%~95%. The material obtained by the third sintering is cooled and crushed to obtain the positive electrode material. The obtained positive electrode material is crushed, and the crushed matrix is uniformly mixed with the coating agent, the coating agent is Al2O3, and the coating agent accounts for 0.15wt% of the weight of the matrix, and then sintered at 550℃ for 3h in an air atmosphere to obtain a single crystal positive electrode material for lithium-ion batteries.
[0029] The obtained positive electrode crushed material was sampled and scanned using an electron scanning microscope to observe the primary particle morphology of the obtained small single crystal positive electrode material. The SEM test results are shown in Figure 2 . Example 2
[0030] Nickel sulfate, cobalt sulfate and manganese sulfate were prepared into a mixed salt solution with a total ion concentration of 1.5 mol / L according to a molar ratio of 65:7:28, a 4 mol / L sodium hydroxide solution was prepared as a precipitant solution, and a 4 mol / L ammonia solution was prepared as a complexing agent solution.
[0031] Deionized water was added to a 50L closed reactor, and the temperature of the liquid in the reactor was maintained at 50°C by heating with a constant temperature water tank. The stirring was turned on and the speed was adjusted to 550r / min. A mixed salt solution, a precipitant solution and a complexing agent solution were pumped into the reactor at the same time, wherein the flow rate of the mixed salt solution was 25mL / min, the ammonia concentration in the reactor was controlled to be 3g / L, the alkali concentration in the reactor was controlled to be 4.5g / L, the pumping rate of the precipitant solution was adjusted by a metering pump to keep the pH of the coprecipitation reaction at 10.7-10.9, and a mixed gas of oxygen and nitrogen with a volume ratio of 1:25 was introduced below the liquid level in the reactor, and the flow rate of the mixed gas was 0.25m 3 / h, oxygen is used to control the morphology of the precursor nucleation stage, and the degree of oxidation determines the morphology of the core. The coprecipitation reaction is stopped when the core grows to a D50 of 1.8-2.0μm.
[0032] The constant temperature water tank is still used to heat the reactor to maintain the liquid temperature at 50°C, the stirring speed is still 550r / min, and the mixed salt solution, precipitant solution and complexing agent solution are pumped into the reactor at the same time. The flow rate of the mixed salt solution is 25mL / min, the ammonia concentration in the reactor is controlled to be 5g / L, the alkali concentration in the reactor is 6.5g / L, and the precipitant solution pumping rate is adjusted by a metering pump to keep the pH of the coprecipitation reaction at 11.5-11.7, and a mixed gas of oxygen and nitrogen with a volume ratio of 1:45 is introduced below the liquid level in the reactor, and the flow rate of the mixed gas is 0.2m 3 / h, the coprecipitation reaction generates an outer shell layer that is significantly different from the inner core layer morphology, and controls the whisker thickness range and whisker uniformity. When the average particle size of the precursor D50 is 3-5μm, stop adding materials and open the reactor to discharge the precursor slurry.
[0033] The precursor slurry was put into an aging kettle; it was stirred for 4 hours under nitrogen protection conditions, and then the precursor slurry introduced into the aging kettle was washed in a centrifuge and the water was thrown out to obtain a precursor to be dried, and the precursor to be dried was placed in a blast drying oven, the drying temperature was set to 100°C, the drying time was 16 hours, and then passed through a 200-mesh sieve to obtain a precursor with a nickel:cobalt:manganese molar ratio of 65:7:28, and the average particle size D50 of the precursor was 3.946 μm, and the BET was 12.39 m 2 / g, and the whisker thickness is 93.79~133.54nm.
[0034] The obtained Ni 0.65 Co 0.07 Mn 0.28 The (OH)2 nickel-cobalt-manganese precursor was cut and the cross-sectional morphology was observed using a field emission scanning electron microscope.
[0035] The obtained Ni 0.65 Co 0.07 Mn 0.28 The (OH)2 precursor is mixed with lithium salt and additives, wherein the lithium salt is LiOH, the additive is ZrO2, LiOH and Ni 0.65 Co 0.07 Mn 0.28 The molar ratio of (OH)2 is 1.055:1, and ZrO2 accounts for 1.055:1 of LiOH and Ni 0.65 Co 0.07 Mn 0.280.2wt% of the total mass of (OH)2 is added to the high-speed mixer for mixing, and the mixing time is 15min. The mixed materials are sintered for the first time at 150℃ for 3h under oxygen atmosphere, and then sintered for the second time at 450℃ for 3h, and then sintered for the third time at 980℃ for 8h. The three sinterings are heated at a heating rate of 3℃ / min, and the oxygen content in the atmosphere furnace is 85%~95%. The material obtained by the third sintering is cooled and crushed to obtain the positive electrode material. The obtained positive electrode material is crushed, and the crushed matrix is uniformly mixed with the coating agent, the coating agent is Al2O3, and the coating agent accounts for 0.15wt% of the weight of the matrix, and then sintered at 550℃ for 3h in an air atmosphere to obtain a single crystal positive electrode material for lithium-ion batteries.
[0036] The obtained positive electrode crushed material was sampled and scanned using an electron scanning microscope to observe the primary particle morphology of the obtained small single crystal positive electrode material. Example 3
[0037] Nickel sulfate, cobalt sulfate and manganese sulfate were prepared into a mixed salt solution with a total ion concentration of 1.5 mol / L according to a molar ratio of 68:10:22, a 4 mol / L sodium hydroxide solution was prepared as a precipitant solution, and a 4 mol / L ammonia solution was prepared as a complexing agent solution.
[0038] Deionized water was added to a 50L closed reactor, and the temperature of the liquid in the reactor was maintained at 50°C by heating with a constant temperature water tank. The stirring was turned on and the speed was adjusted to 550r / min. A mixed salt solution, a precipitant solution and a complexing agent solution were pumped into the reactor at the same time, wherein the flow rate of the mixed salt solution was 25mL / min, the ammonia concentration in the reactor was controlled to be 3g / L, the alkali concentration in the reactor was controlled to be 5g / L, the pumping rate of the precipitant solution was adjusted by a metering pump to keep the pH of the coprecipitation reaction at 11.0-11.2, and a mixed gas of oxygen and nitrogen with a volume ratio of 1:25 was introduced below the liquid level in the reactor, and the flow rate of the mixed gas was 0.25m 3 / h, oxygen is used to control the morphology of the precursor nucleation stage, and the degree of oxidation determines the morphology of the core. The coprecipitation reaction is stopped when the core grows to a D50 of 1.8-2.0μm.
[0039] The constant temperature water tank is still used to heat the reactor to maintain the liquid temperature at 50°C, the stirring speed is still 550r / min, and the mixed salt solution, precipitant solution and complexing agent solution are pumped into the reactor at the same time. The flow rate of the mixed salt solution is 25mL / min, the ammonia concentration in the reactor is controlled to be 5g / L, the alkali concentration in the reactor is 6.5g / L, and the precipitant solution pumping rate is adjusted by a metering pump to keep the pH of the coprecipitation reaction at 11.8-12.0, and a mixed gas of oxygen and nitrogen with a volume ratio of 1:45 is introduced below the liquid level in the reactor, and the flow rate of the mixed gas is 0.2m3 / h, the coprecipitation reaction generates an outer shell layer that is significantly different from the inner core layer morphology, and controls the whisker thickness range and whisker uniformity. When the average particle size of the precursor D50 is 3-5μm, stop adding materials and open the reactor to discharge the precursor slurry.
[0040] The precursor slurry was put into an aging kettle; it was stirred for 4 hours under nitrogen protection conditions, and then the precursor slurry introduced into the aging kettle was washed in a centrifuge and the water was thrown out to obtain a precursor to be dried, and the precursor to be dried was placed in a blast drying oven, the drying temperature was set to 100°C, the drying time was 16 hours, and then passed through a 200-mesh sieve to obtain a precursor with a nickel:cobalt:manganese molar ratio of 68:10:22, and the average particle size D50 of the precursor was 3.521 μm, and the BET was 11.14 m 2 / g, and the whisker thickness is 87.77~125.89nm.
[0041] The obtained Ni 0.68 Co 0.10 Mn 0.22 The (OH)2 nickel-cobalt-manganese precursor was cut and the cross-sectional morphology was observed using a field emission scanning electron microscope.
[0042] The obtained Ni 0.68 Co 0.10 Mn 0.22 The (OH)2 precursor is mixed with lithium salt and additives, wherein the lithium salt is LiOH, the additive is ZrO2, LiOH and Ni 0.68 Co 0.10 Mn 0.22 The molar ratio of (OH)2 is 1.055:1, and ZrO2 accounts for 1.055:1 of LiOH and Ni 0.68 Co 0.10 Mn 0.22 0.2wt% of the total mass of (OH)2 is added to the high-speed mixer for mixing, and the mixing time is 15min. The mixed materials are sintered for the first time at 150℃ for 3h under oxygen atmosphere, and then sintered for the second time at 450℃ for 3h, and then sintered for the third time at 980℃ for 8h. The three sinterings are heated at a heating rate of 3℃ / min, and the oxygen content in the atmosphere furnace is 85%~95%. The material obtained by the third sintering is cooled and crushed to obtain the positive electrode material. The obtained positive electrode material is crushed, and the crushed matrix is uniformly mixed with the coating agent, the coating agent is Al2O3, and the coating agent accounts for 0.15wt% of the weight of the matrix, and then sintered at 550℃ for 3h in an air atmosphere to obtain a single crystal positive electrode material for lithium-ion batteries.
[0043] The obtained positive electrode crushed material was sampled and scanned using an electron scanning microscope to observe the primary particle morphology of the obtained small single crystal positive electrode material.
[0044] Comparative Example 1 Nickel sulfate, cobalt sulfate and manganese sulfate were prepared into a mixed salt solution with a total ion concentration of 1.5 mol / L according to a molar ratio of 60:10:30, a 4 mol / L sodium hydroxide solution was prepared as a precipitant solution, and a 4 mol / L ammonia solution was prepared as a complexing agent solution.
[0045] Deionized water was added to a 50L sealed reactor, and the temperature of the liquid in the reactor was maintained at 50°C by heating with a constant temperature water tank. The stirring speed was turned on and adjusted to 550r / min. The mixed salt solution, precipitant solution and complexing agent solution were pumped into the reactor at the same time. The flow rate of the mixed salt solution was 25mL / min. The ammonia concentration in the reactor was controlled to be 3g / L, and the alkali concentration in the reactor was 5g / L. The pumping rate of the precipitant solution was adjusted with a metering pump to keep the pH of the coprecipitation reaction at 10.5-10.7, and nitrogen was introduced below the liquid level in the reactor. The flow rate of nitrogen was 0.25m 3 / h. The coprecipitation reaction was stopped when the inner core grew to a D50 of 0.1-1.0 μm.
[0046] The temperature of the liquid in the reactor was maintained at 50°C by the constant temperature water tank heating, and the stirring speed was still 550r / min. At the same time, the mixed salt solution, precipitant solution and complexing agent solution were pumped into the reactor. The flow rate of the mixed salt solution was 25mL / min. The ammonia concentration in the reactor was controlled to be 5g / L, and the alkali concentration in the reactor was 6.5g / L. The pumping rate of the precipitant solution was adjusted by a metering pump to keep the pH of the coprecipitation reaction at 11.3-11.5, and nitrogen was introduced below the liquid level in the reactor. The flow rate of nitrogen was 0.2m 3 / h. When the average particle size of the precursor D50 is 3-5 μm, stop adding materials and open the reactor to discharge the precursor slurry.
[0047] The precursor slurry was put into an aging kettle; it was stirred for 4 hours under nitrogen protection conditions, and then the precursor slurry introduced into the aging kettle was washed in a centrifuge and the water was thrown out to obtain a precursor to be dried, and the precursor to be dried was placed in a blast drying oven, the drying temperature was set to 100°C, the drying time was 16 hours, and then passed through a 200-mesh sieve to obtain a precursor with a nickel:cobalt:manganese molar ratio of 60:10:30, and the average particle size D50 of the precursor was 3.583 μm, and the BET was 7.65 m 2 / g, whisker thickness is 50~100nm.
[0048] The obtained Ni 0.60 Co 0.10 Mn0.30 The (OH)2 nickel-cobalt-manganese precursor was cut and the cross-sectional morphology was observed using a field emission scanning electron microscope. The test results are shown in Figure 3 .
[0049] The obtained Ni 0.60 Co 0.10 Mn 0.30 The (OH)2 precursor is mixed with lithium salt and additives, wherein the lithium salt is LiOH, the additive is ZrO2, LiOH and Ni 0.60 Co 0.10 Mn 0.30 The molar ratio of (OH)2 is 1.065:1, and ZrO2 accounts for 1.065:1 of LiOH and Ni 0.60 Co 0.10 Mn 0.30 0.2wt% of the total mass of (OH)2 is added to the high-speed mixer for mixing, and the mixing time is 15min. The mixed materials are sintered for the first time at 150℃ for 3h under oxygen atmosphere, and then sintered for the second time at 450℃ for 3h, and then sintered for the third time at 980℃ for 8h. The three sinterings are heated at a heating rate of 3℃ / min, and the oxygen content in the atmosphere furnace is 85%~95%. The material obtained by the third sintering is cooled and crushed to obtain the positive electrode material. The obtained positive electrode material is crushed, and the crushed matrix is uniformly mixed with the coating agent, the coating agent is Al2O3, and the coating agent accounts for 0.15wt% of the weight of the matrix, and then sintered at 550℃ for 3h in an air atmosphere to obtain a single crystal positive electrode material for lithium-ion batteries.
[0050] The obtained positive electrode crushed material was sampled and scanned using an electron scanning microscope to observe the primary particle morphology of the obtained small single crystal positive electrode material. The SEM test results are shown in Figure 4 .
[0051] Comparative Example 2 Nickel sulfate, cobalt sulfate and manganese sulfate were prepared into a mixed salt solution with a total ion concentration of 1.5 mol / L according to a molar ratio of 65:7:28, a 4 mol / L sodium hydroxide solution was prepared as a precipitant solution, and a 4 mol / L ammonia solution was prepared as a complexing agent solution.
[0052] Deionized water was added to a 50L closed reactor, and the temperature of the liquid in the reactor was maintained at 50°C by heating with a constant temperature water tank. The stirring speed was turned on and adjusted to 550r / min. At the same time, a mixed salt solution, a precipitant solution and a complexing agent solution were pumped into the reactor, wherein the flow rate of the mixed salt solution was 25mL / min, the ammonia concentration in the reactor was controlled to be 3g / L, the alkali concentration in the reactor was 4.5g / L, the pumping rate of the precipitant solution was adjusted with a metering pump to keep the pH of the coprecipitation reaction at 10.7-10.9, and nitrogen was introduced below the liquid level in the reactor, and the flow rate of nitrogen was 0.25m 3 / h. The coprecipitation reaction was stopped when the inner core grew to a D50 of 0.1-1.0 μm.
[0053] The temperature of the liquid in the reactor was maintained at 50°C by the constant temperature water tank heating, and the stirring speed was still 550r / min. At the same time, the mixed salt solution, precipitant solution and complexing agent solution were pumped into the reactor. The flow rate of the mixed salt solution was 25mL / min. The ammonia concentration in the reactor was controlled to be 5g / L, and the alkali concentration in the reactor was 6.5g / L. The pumping rate of the precipitant solution was adjusted by a metering pump to keep the pH of the coprecipitation reaction at 11.5-11.7, and nitrogen was introduced below the liquid level in the reactor. The flow rate of nitrogen was 0.2m 3 / h. When the average particle size of the precursor D50 is 3-5 μm, stop adding materials and open the reactor to discharge the precursor slurry.
[0054] The precursor slurry was put into an aging kettle; it was stirred for 4 hours under nitrogen protection conditions, and then the precursor slurry introduced into the aging kettle was washed in a centrifuge and the water was thrown out to obtain a precursor to be dried, and the precursor to be dried was placed in a blast drying oven, the drying temperature was set to 100°C, the drying time was 16 hours, and then passed through a 200-mesh sieve to obtain a precursor with a nickel:cobalt:manganese molar ratio of 65:7:28, and the average particle size D50 of the precursor was 3.875 μm, and the BET was 7.99 m 2 / g, whisker thickness is 45~90nm.
[0055] The obtained Ni 0.65 Co 0.07 Mn 0.28 The (OH)2 nickel-cobalt-manganese precursor was cut and the cross-sectional morphology was observed using a field emission scanning electron microscope.
[0056] The obtained Ni 0.65 Co 0.07 Mn 0.28 The (OH)2 precursor is mixed with lithium salt and additives, wherein the lithium salt is LiOH, the additive is ZrO2, LiOH and Ni 0.65 Co 0.07 Mn 0.28The molar ratio of (OH)2 is 1.055:1, and ZrO2 accounts for 1.055:1 of LiOH and Ni 0.65 Co 0.07 Mn 0.28 0.2wt% of the total mass of (OH)2 is added to the high-speed mixer for mixing, and the mixing time is 15min. The mixed materials are sintered for the first time at 150℃ for 3h under oxygen atmosphere, and then sintered for the second time at 450℃ for 3h, and then sintered for the third time at 980℃ for 8h. The three sinterings are heated at a heating rate of 3℃ / min, and the oxygen content in the atmosphere furnace is 85%~95%. The material obtained by the third sintering is cooled and crushed to obtain the positive electrode material. The obtained positive electrode material is crushed, and the crushed matrix is uniformly mixed with the coating agent, the coating agent is Al2O3, and the coating agent accounts for 0.15wt% of the weight of the matrix, and then sintered at 550℃ for 3h in an air atmosphere to obtain a single crystal positive electrode material for lithium-ion batteries.
[0057] The obtained positive electrode crushed material was sampled and scanned using an electron scanning microscope to observe the primary particle morphology of the obtained small single crystal positive electrode material.
[0058] Comparative Example 3 Nickel sulfate, cobalt sulfate and manganese sulfate were prepared into a mixed salt solution with a total ion concentration of 1.5 mol / L according to a molar ratio of 68:10:22, a 4 mol / L sodium hydroxide solution was prepared as a precipitant solution, and a 4 mol / L ammonia solution was prepared as a complexing agent solution.
[0059] Deionized water was added to a 50L closed reactor, and the temperature of the liquid in the reactor was maintained at 50°C by heating with a constant temperature water tank. The stirring speed was turned on and adjusted to 550r / min. The mixed salt solution, precipitant solution and complexing agent solution were pumped into the reactor at the same time. The flow rate of the mixed salt solution was 25mL / min. The ammonia concentration in the reactor was controlled to be 3g / L, and the alkali concentration in the reactor was 4g / L. The pumping rate of the precipitant solution was adjusted with a metering pump to keep the pH of the coprecipitation reaction at 10.7-10.9, and nitrogen was introduced below the liquid level in the reactor. The flow rate of nitrogen was 0.25m 3 / h. The coprecipitation reaction was stopped when the inner core grew to a D50 of 0.1-1.0 μm.
[0060] The temperature of the liquid in the reactor was maintained at 50°C by the constant temperature water tank, and the stirring speed was still 550r / min. At the same time, the mixed salt solution, precipitant solution and complexing agent solution were pumped into the reactor. The flow rate of the mixed salt solution was 25mL / min. The ammonia concentration in the reactor was controlled to be 5g / L, and the alkali concentration in the reactor was 6.5g / L. The pumping rate of the precipitant solution was adjusted by a metering pump to keep the pH of the coprecipitation reaction at 11.7-11.9, and nitrogen was introduced below the liquid level in the reactor. The flow rate of nitrogen was 0.25m 3 / h. When the average particle size of the precursor D50 is 3-5 μm, stop adding materials and open the reactor to discharge the precursor slurry.
[0061] The precursor slurry was put into an aging kettle; it was stirred for 4 hours under nitrogen protection conditions, and then the precursor slurry introduced into the aging kettle was washed in a centrifuge and the water was thrown out to obtain a precursor to be dried, and the precursor to be dried was placed in a blast drying oven, the drying temperature was set to 100°C, the drying time was 16 hours, and then passed through a 200-mesh sieve to obtain a precursor with a nickel:cobalt:manganese molar ratio of 68:10:22, and the average particle size D50 of the precursor was 3.78 μm, and the BET was 8.21 m 2 / g, and the whisker thickness is 43~89nm.
[0062] The obtained Ni 0.68 Co 0.10 Mn 0.22 The (OH)2 nickel-cobalt-manganese precursor was cut and the cross-sectional morphology was observed using a field emission scanning electron microscope.
[0063] The obtained Ni 0.68 Co 0.10 Mn 0.22 The (OH)2 precursor is mixed with lithium salt and additives, wherein the lithium salt is LiOH, the additive is ZrO2, LiOH and Ni 0.68 Co 0.10 Mn 0.22 The molar ratio of (OH)2 is 1.065:1, and ZrO2 accounts for 1.065:1 of LiOH and Ni 0.68 Co 0.10 Mn 0.220.2wt% of the total mass of (OH)2 is added to the high-speed mixer for mixing, and the mixing time is 15min. The mixed materials are sintered for the first time at 150℃ for 3h under oxygen atmosphere, and then sintered for the second time at 450℃ for 3h, and then sintered for the third time at 980℃ for 8h. The three sinterings are heated at a heating rate of 3℃ / min, and the oxygen content in the atmosphere furnace is 85%~95%. The material obtained by the third sintering is cooled and crushed to obtain the positive electrode material. The obtained positive electrode material is crushed, and the crushed matrix is uniformly mixed with the coating agent, the coating agent is Al2O3, and the coating agent accounts for 0.15wt% of the weight of the matrix, and then sintered at 550℃ for 3h in an air atmosphere to obtain a single crystal positive electrode material for lithium-ion batteries.
[0064] The obtained positive electrode crushed material was sampled and scanned using an electron scanning microscope to observe the primary particle morphology of the obtained small single crystal positive electrode material.
[0065] Table 2 is the inner and outer layer diameter data of Argon ion polishing SEM of Example 1 and Comparative Example 1: Table 2
[0066] Table 3 is the variance data of the short side measurement of the SEM primary particles of the positive electrode materials sintered in Example 1 and Comparative Example 1:
[0067] The single crystal positive electrode material of lithium-ion batteries follows the formation mechanism of dissolution and recrystallization during the synthesis process, and the precursor of the secondary particles disintegrates and the primary particles slowly grow into single crystals. In Examples 1, 2, and 3 of the present invention, the morphology of the precursor is optimized, that is, the large inner core layer is an amorphous structure flocculent morphology, 35% of the diameter of the precursor particle ≤ the inner core layer diameter ≤ 60% of the diameter of the precursor particle; the outer shell layer is a loose and porous structure with uniform whisker thickness, the sum of the diameters of the inner core layer and the outer shell layer is 3~5μm, the outer shell layer whisker thickness is 80-150nm, and the whisker uniformity is good. Figure 1 The amorphous flocculent morphology of the inner core layer is conducive to the dissociation of the precursor particles, and the uniformity of the outer shell whiskers of the precursor plays a role in ensuring the uniformity of the recrystallization of the single crystal primary particles. The precursor inner cores obtained in Comparative Examples 1, 2, and 3 are smaller, and the precursor whiskers are dense. Figure 3 The secondary particles of the precursor with different morphology are not easy to dissociate. The sintering temperature required to sinter single crystal positive electrode materials is relatively high, and the single crystal primary particles are not uniform. Figure 2 and Figure 4 It is the single crystal positive electrode material corresponding to the precursor prepared in Example 1 and Comparative Example 1 after sintering. It can be clearly seen from the figure Figure 2The precursor morphology affects the obtained single crystal primary particles to be more uniform. When used in lithium-ion batteries, uniform single crystal primary particles can have lithium ion channels of the same length, and can play a more stable role in high rate performance and long cycle performance.
[0068] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.
Claims
1. A precursor for improving the uniformity of primary particles of small single crystal positive electrode materials, characterized in that: The chemical formula of the precursor is Ni x Co y Mn 1-x-y (OH)2, where 0.6≤x<0.95, 0.05≤y≤0.15, the average particle size D50 of the precursor is 3.0~5.0μm, and the specific surface area is 10~15m 2 / g, the precursor includes an inner core layer and an outer shell layer, the inner core layer is an amorphous structure flocculent morphology, 35% of the precursor particle diameter ≤ the inner core layer diameter ≤ 60% of the precursor particle diameter, the outer shell layer is a loose and porous structure with uniform whisker thickness, the outer shell layer whisker thickness is 80~150nm and the whisker uniformity is good, the precursor particles have less twinning and the particles have good sphericity.
2. A method for preparing a precursor for improving the uniformity of primary particles of small single crystal positive electrode materials according to claim 1, characterized in that The specific steps are: Step S1, preparing a mixed salt solution of transition metal nickel salt, cobalt salt and manganese salt, preparing an alkali solution as a precipitant solution, and preparing an ammonia solution as a complexing agent solution; Step S2, co-precipitation reaction of the inner core layer, a mixed salt solution, a precipitant solution and a complexing agent solution are simultaneously pumped into a sealed reactor containing a bottom liquid, the flow rate of the mixed salt solution is controlled to be 15-50 mL / min, the concentration of the precipitant in the mixed solution in the reactor is controlled to be 2-5 g / L, the concentration of the complexing agent is controlled to be 2-3.5 g / L, the pH of the mixed solution is controlled to be 10.0-11.5, and a mixed gas of oxygen and nitrogen is introduced, and a nucleation co-precipitation reaction is carried out under the conditions of a temperature of 40-60° C. and a stirring rate of 500-1000 r / min, and the reaction is stopped when 35% of the diameter of the precursor particle is ≤ the diameter of the inner core layer ≤ 60% of the diameter of the precursor particle. The proportion of oxygen in the mixed gas of oxygen and nitrogen is used to control the degree of oxidation of the precursor in the nucleation stage, and the degree of oxidation determines the morphology of the inner core layer. The volume ratio of oxygen to nitrogen in the mixed gas of oxygen and nitrogen is 1:20-30; Step S3, after the coprecipitation reaction of the outer shell layer and the inner core layer react to the target particle size, the flow rate of the precipitant solution and the complexing agent solution is changed to adjust the concentration of the precipitant in the mixed solution in the reactor to be controlled to 5-7 g / L, and the concentration of the complexing agent is controlled to be 4-6 g / L. At this time, the pH of the mixed solution is controlled to be 11.0-12.5, the reaction temperature remains unchanged, and the stirring rate of the reactor remains unchanged. The coprecipitation reaction of the outer shell layer is controlled by adjusting the ratio of the mixed gas of oxygen and nitrogen and the flow rate of the precipitant solution and the complexing agent solution to generate an outer shell layer that is obviously different from the morphology of the inner core layer, and the whisker thickness range and whisker uniformity are controlled. The volume ratio of oxygen to nitrogen in the mixed gas of oxygen and nitrogen is 1:40-50. When the average particle size of the precursor D50 is 3-5 μm, the feeding is stopped and the reactor is opened to discharge the precursor slurry. Step S4, filtering, washing, drying and sieving the obtained precursor slurry to obtain a precursor for improving the uniformity of primary particles of small single crystal positive electrode materials.
3. The method for preparing a precursor for improving the uniformity of primary particles of small single crystal positive electrode materials according to claim 2, characterized in that: The concentration of the mixed salt solution in step S1 is 1.5-2 mol / L, the nickel salt in the mixed salt solution is one or more of nickel sulfate, nickel chloride or nickel nitrate, the cobalt salt is one or more of cobalt sulfate, cobalt chloride or cobalt nitrate, and the manganese salt is one or more of manganese sulfate, manganese chloride or manganese nitrate; the concentration of the alkali in the precipitant solution is 2-8 mol / L, and the alkali used is one or more of sodium hydroxide or potassium hydroxide; the concentration of ammonia in the complexing agent solution is 0.1-4 mol / L.
4. A lithium-ion battery single crystal positive electrode material, whose chemical formula is Li 1.005-1.10 Ni x Co y Mn 1-x-y MO2@DO, wherein 0.8 μm ≤ the short side diameter of the primary particle of the single crystal positive electrode material ≤ 2 μm, 0.6 ≤ x < 0.95, 0.05 ≤ y ≤ 0.15, M is one or more of Zr, Sr, Ti, W, Mg, Y, La, B or F, and D is one or more of Co, Li, B, W, Ti or Zr.
5. A method for preparing a single crystal positive electrode material for a lithium-ion battery according to claim 4, characterized in that: A precursor for improving the uniformity of primary particles of small single crystal positive electrode materials prepared by the method described in claim 2 or 3, the obtained precursor is mixed evenly with a lithium salt and an additive, and then subjected to primary sintering, crushing, pulverizing, coating, secondary sintering, and screening in sequence to obtain a single crystal positive electrode material for a lithium ion battery, wherein the lithium salt is one or more of lithium hydroxide, lithium carbonate or lithium chloride, the additive is one or more of compounds containing Zr, Sr, Ti, W, Mg, Y, La, B or F elements, and the coating agent used in the coating process is one or more of an oxide containing element D or a lithium compound containing element D, wherein element D is one or more of Al, Co, Li, B, W, Ti or Zr.
6. The method for preparing a single crystal positive electrode material for a lithium-ion battery according to claim 5, characterized in that: The feed ratio of the precursor and the lithium salt satisfies that the molar ratio of (Ni+CO+Mn):Li is 1:1.005-1.105, and the amount of the additive added is 0.1wt%-2wt% of the total mass of the precursor and the lithium salt.
7. The method for preparing a single crystal positive electrode material for a lithium-ion battery according to claim 5, characterized in that: The primary sintering process is calcined in stages in an oxygen atmosphere furnace, the temperature of the first dehydration stage is 50-200°C, the insulation time is 2-4h, the temperature of the second dehydration stage is 350-450°C, the insulation time is 2-4h, the temperature of the third oxide curing reaction is 800-1000°C, the insulation time is 6-10h, the three stages are heated at a heating rate of 2-5°C / min, the oxygen content in the atmosphere furnace is 85%-95%, and finally a primary sintered matrix is obtained.
8. The method for preparing a single crystal positive electrode material for a lithium-ion battery according to claim 7, characterized in that: The specific process of the coating is: crushing the obtained primary sintered matrix, sieving the crushed matrix and mixing it evenly with the coating agent, wherein the coating agent is 0.01wt%-5wt% of the mass of the matrix after drying.
9. The method for preparing a single crystal positive electrode material for a lithium-ion battery according to claim 5, characterized in that: The secondary sintering process is sintering at 500-600° C. for 2-4 hours in an air atmosphere.
Citation Information
Cited By
Uniform radial positive electrode material precursor and preparation method thereof
CN119706978A
Positive electrode material precursor, preparation method thereof, positive electrode material and lithium ion battery
CN120622566A