Preparation method of low-hydroxyl optical glass
Through high-purity raw materials and vacuum melting technology, combined with high-temperature degassing and annealing treatment, the problem of insufficient hydroxyl content and mechanical strength in the preparation of low-hydroxyl optical glass is solved, and the optical performance and stability are significantly improved, and it is suitable for high-precision optical applications.
Patent Information
- Application Number
- CN202411221985.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-29
AI Technical Summary
The hydroxyl content control in the existing low-hydroxy optical glass preparation technology is not accurate enough, and the mechanical strength and stability of the glass are insufficient, which affects the optical performance and application range.
High-purity raw materials are used for vacuum melting, protection with argon or nitrogen, and degassing and homogenizing are carried out at high temperatures. The molding is carried out by casting or die-casting, combined with optimized annealing treatment to eliminate internal stress of the glass.
It significantly reduces the hydroxyl content in the glass, improves optical transparency and mechanical strength, extends the service life of the glass, and is suitable for high-precision optical instruments.
Smart Images

Figure CN119038874A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass manufacturing, in particular to a method for preparing low-hydroxyl optical glass. Background Art
[0002] In the manufacture of modern optical devices, low hydroxyl optical glass is widely used in high-precision optical systems, such as astronomical telescopes, lasers, spectrometers and other optical instruments. The hydroxyl content has a crucial influence on the performance of optical glass. High hydroxyl content will cause the transmittance of optical glass to decrease in the infrared and ultraviolet spectrum range, and at the same time cause the instability of optical performance and even accelerate the aging of glass.
[0003] The existing low-hydroxyl optical glass preparation technology mainly relies on high-purity raw materials and vacuum melting process. However, the existing technology still has the following shortcomings:
[0004] Inaccurate control of hydroxyl content: Despite vacuum melting and argon protection, due to inaccurate control of temperature and time of degassing treatment, a certain amount of hydroxyl may still remain in the glass, affecting the optical properties.
[0005] Insufficient mechanical strength and stability of glass: The annealing treatment in the existing process fails to fully eliminate the stress inside the glass, resulting in poor mechanical strength and thermal stability of the finished glass, limiting its application in harsh environments.
[0006] To this end, those skilled in the art provide a method for preparing low-hydroxyl optical glass to solve the problems raised in the above background technology. Summary of the invention
[0007] In view of the deficiencies of the prior art, the present invention provides a method for preparing low-hydroxyl optical glass, which solves the problems in the prior art of inaccurate control of hydroxyl content and insufficient mechanical strength and stability of the glass.
[0008] To achieve the above objectives, the present invention is implemented through the following technical scheme: low hydroxyl optical glass, which is composed of the following components in mass percentage: 60-70% silicon dioxide, 10-15% boron oxide, 5-10% aluminum oxide, 2-5% magnesium oxide, 5-7% lanthanum oxide, 1-2% neodymium oxide, 1-3% cerium oxide, 0.5-2% titanium dioxide, 1-2% yttrium oxide, 0.5-1% phosphorus pentoxide, and 0.1-1% tungsten oxide.
[0009] The preparation method of low hydroxyl optical glass, used for low hydroxyl optical glass, comprises the following steps:
[0010] S1. Prepare silicon dioxide, boron oxide, aluminum oxide, magnesium oxide, lanthanum oxide, neodymium oxide, cerium oxide, titanium dioxide, yttrium oxide, phosphorus pentoxide, and tungsten oxide raw materials;
[0011] S2. Vacuum melt the processed raw materials, and add argon or nitrogen with a purity of not less than 99.99% as a protective gas during the melting process;
[0012] S3, degassing the molten glass;
[0013] S4, cooling the molten glass to 1200-1300° C. for homogenization and maintaining the temperature for 1-2 hours;
[0014] S5, forming the homogenized glass melt by tape casting or die casting, and continuously maintaining an inert gas environment for cooling and preventing water vapor from entering during the process;
[0015] S6. Annealing the formed glass to eliminate internal stress.
[0016] Preferably, in the step S1, the purity of the prepared silicon dioxide is not less than 99.99%, and all raw materials are placed in a drying furnace with an internal temperature of 110-150° C. for 120-480 min.
[0017] Preferably, the vacuum melting in step S2 is maintained at a vacuum degree equal to or lower than 10 -5 Under the condition of 200-1200°C, the temperature is melted to 1500-1600°C and maintained for 120-480 minutes.
[0018] Preferably, in the step S2, a high-purity quartz crucible is used as the melting container.
[0019] Preferably, the degassing treatment in the step S3 is carried out by slowly raising and lowering the temperature within the range of 1400-1600° C., and the treatment time is maintained at 120-480 min.
[0020] Preferably, the inert gas in step S6 includes but is not limited to krypton, helium and nitrogen.
[0021] Preferably, the annealing treatment in step S7 includes placing the glass melt in a box-type annealing furnace, gradually reducing the temperature to 500-600° C. and maintaining it for at least 240 minutes.
[0022] Preferably, the degassing treatment in step S3 uses a vacuum degassing furnace at a vacuum degree of less than 10 -6 Torr, and the temperature is controlled in the range of 1400-1600°C.
[0023] Preferably, phosphorus pentoxide is added during the degassing process and a stirrer is used to ensure its uniform distribution in the glass melt.
[0024] The present invention provides a method for preparing low-hydroxyl optical glass, which has the following beneficial effects:
[0025] 1. The present invention significantly reduces the hydroxyl content in the glass by adopting high-purity raw materials, vacuum melting, argon or helium protection and high-temperature degassing treatment, ensuring the high optical transparency and low impurity content of the glass, and effectively improving the optical properties of the glass, especially the transmittance in the visible light and infrared spectrum range is higher, and is suitable for high-precision optical instruments.
[0026] 2. The present invention successfully eliminates the stress inside the glass through homogenization and optimized annealing process, and enhances the mechanical strength and long-term thermal stability of the finished glass. Whether in high temperature environment or in long-term use, the glass can maintain its excellent optical and physical properties, prolonging the service life of the product and meeting the application scenarios with high requirements for optical glass performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the method steps of the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1: Standard process
[0030] step:
[0031] S1: Silica purity 99.99%, all raw materials were dried at 150°C for 300 minutes.
[0032] S2: Vacuum melting at 10 -5 The melting temperature was 1550°C for 240 minutes and the protective gas was argon.
[0033] S3: Degassing treatment was performed at 1400°C for 240 minutes using a vacuum degassing furnace.
[0034] S4: Homogenization treatment was performed at 1250° C. for 120 minutes.
[0035] S5: The molding is completed by the casting method, and argon gas is used to protect the film from water vapor.
[0036] S6: Annealing treatment is carried out in a box-type annealing furnace, and the temperature is gradually reduced to 550° C. for 300 minutes.
[0037] Summary: This standard process example aims to provide a stable and repeatable low-hydroxyl optical glass preparation process. The following are several key points of the process:
[0038] Raw material processing: High temperature drying effectively removes moisture and volatile impurities in the raw materials, ensuring that no additional hydroxyl groups are introduced during the subsequent melting process. Raw material purity control (such as SiO 2 99.99% purity) lays the foundation for the production of high-quality optical glass.
[0039] Vacuum melting: melting process under vacuum conditions (10 -5 Torr) can significantly reduce bubbles and oxide impurities in the glass melt, ensuring the purity and optical uniformity of the glass melt. By using argon as a protective gas, the melt is further prevented from reacting with impurities in the air.
[0040] Degassing: Degassing is carried out at 1400°C, and a vacuum degassing furnace is used to effectively remove residual bubbles and dissolved gases in the melt. The temperature and time during the degassing process are controlled to ensure that the bubbles can fully float up and escape from the melt, greatly improving the optical transparency and uniformity of the glass.
[0041] Homogenization: Homogenization makes the composition and temperature of the glass melt more uniform and eliminates possible stress concentration points. This step is crucial to ensure the optical properties of the finished glass, especially in the application of optical devices, where uniformity directly affects the transmission and scattering of light.
[0042] Molding and annealing: Casting by tape casting combined with argon protection can prevent external moisture from entering the interior of the glass and maintain the low hydroxyl properties of the glass. Annealing treatment eliminates stress inside the glass by slowly cooling it down, ensuring its high mechanical strength and long-term stability. The choice of annealing temperature and time (550°C and 300 minutes) has been optimized to balance stress release and glass structural stability.
[0043] Example 2: Increasing the degassing temperature
[0044] step:
[0045] S1: Silica purity 99.99%, all raw materials were dried at 120°C for 400 minutes.
[0046] S2: Vacuum melting at 10 -5 The melting temperature was 1600°C for 300 min and the protective gas was argon.
[0047] S3: Degassing treatment was performed at 1600°C for 180 minutes using a vacuum degassing furnace.
[0048] S4: Homogenization treatment was performed at 1280°C for 150 minutes.
[0049] S5: Molding is done by die casting, with argon protection.
[0050] S6: Annealing treatment is carried out in a box-type annealing furnace, and the temperature is gradually reduced to 600° C. for 240 minutes.
[0051] In summary: Increasing the degassing temperature is expected to more effectively remove bubbles from the melt and improve optical uniformity.
[0052] Example 3: Using helium as shielding gas
[0053] step:
[0054] S1: Silica purity 99.99%, all raw materials were dried at 150°C for 120 minutes.
[0055] S2: Vacuum melting at 10 -5 The melting temperature was 1500°C for 240 minutes and the protective gas was helium.
[0056] S3: Degassing treatment was performed at 1500°C for 240 minutes using a vacuum degassing furnace.
[0057] S4: Homogenization treatment was performed at 1270°C for 180 minutes.
[0058] S5: Molding is done by tape casting, with helium protection.
[0059] S6: Annealing treatment is carried out in a box-type annealing furnace, and the temperature is gradually reduced to 560° C. for 300 minutes.
[0060] Summary: Using helium as a shielding gas can help further reduce the introduction of impurities and may improve optical clarity.
[0061] Example 4: Adding phosphorus pentoxide and stirring
[0062] step:
[0063] S1: Silica purity 99.99%, all raw materials were dried at 110°C for 480 minutes.
[0064] S2: Vacuum melting at 10 -5 The melting temperature was 1550°C for 240 minutes and the protective gas was argon.
[0065] S3: Degassing treatment was performed at 1400° C. for 240 minutes, and phosphorus pentoxide was added and stirred.
[0066] S4: Homogenization treatment is performed at 1200° C. for 120 minutes.
[0067] S5: Molding is done by die casting, with argon protection.
[0068] S6: Annealing treatment is carried out in a box-type annealing furnace, and the temperature is gradually reduced to 580° C. for 300 minutes.
[0069] Summary: Adding phosphorus pentoxide and stirring during the degassing process is expected to dehydrate more effectively and further reduce the hydroxyl content.
[0070] Example 5: Using different annealing gases
[0071] step:
[0072] S1: Silica purity 99.99%, all raw materials were dried at 130°C for 240 minutes.
[0073] S2: Vacuum melting at 10 -5 The melting temperature was 1570°C for 240 minutes and the protective gas was argon.
[0074] S3: Degassing treatment was performed at 1500°C for 240 minutes using a vacuum degassing furnace.
[0075] S4: Homogenization treatment was performed at 1300° C. for 120 minutes.
[0076] S5: Molding is done by die casting, nitrogen protection.
[0077] S6: Annealing treatment is performed in a box-type annealing furnace, the temperature is gradually reduced to 550° C., krypton gas is used, and the time is 240 minutes.
[0078] Summary: Changing the gas during the annealing process, by using different inert gases (such as krypton), studies its effect on glass stress relief and optical properties.
[0079] Summary of Examples
[0080] Each example focuses on different process variables, including raw material processing, degassing temperature, protective gas type, stirring treatment and annealing gas selection. Through the combination of these different variables, the preparation process of low hydroxyl optical glass can be more comprehensively optimized to achieve the best optical performance, mechanical strength and durability.
[0081] Test experiment
[0082] Assume that we conduct the following test experiments, focusing on evaluating the optical transmittance, mechanical strength and hydroxyl content of each embodiment:
[0083] Optical transmittance: The transmittance from 200nm to 2000nm was measured by a spectrophotometer.
[0084] Mechanical Strength: The flexural strength of glass samples was measured using a three-point bending test.
[0085] Hydroxyl content: Fourier transform infrared spectroscopy (FTIR) was used to measure the hydroxyl absorption peak intensity in the glass.
[0086] Experimental data table:
[0087]
[0088] Comparative experiment
[0089] Comparative experiment 1: Effect of different degassing temperatures on performance
[0090] Experimental design: All other conditions were kept unchanged, only the degassing temperature was changed (1400°C, 1500°C, 1600°C).
[0091] Measurement parameters: optical transmittance, mechanical strength, hydroxyl content.
[0092] Comparative experiment 2: Effects of using different protective gases on glass performance
[0093] Experimental design: Argon, helium and nitrogen were used as protective gases, and other conditions remained unchanged.
[0094] Measurement parameters: optical transmittance, mechanical strength, hydroxyl content.
[0095] Comparative experiment 3: Effects of different annealing gases on glass stress and optical properties
[0096] Experimental design: Krypton, argon and nitrogen were used as annealing gases, and other conditions remained unchanged.
[0097] Measurement parameters: optical transmittance, stress distribution (by polarization test), hydroxyl content.
[0098] Comparative experimental data table:
[0099]
[0100]
[0101] Next, the preparation method is compared with the existing conventional low-hydroxyl optical glass preparation method from several key indicators such as optical properties, mechanical strength, hydroxyl content and durability (such as thermal stability):
[0102] Purpose
[0103] Through comparative tests, the advantages of the preparation method of the present invention in the following aspects are verified:
[0104] Optical transmittance: High optical transmittance indicates that the glass has higher purity and uniformity, and lower impurity and bubble content.
[0105] Mechanical Strength: Higher mechanical strength indicates that the glass has less internal stress and is more structurally stable.
[0106] Hydroxyl content: Low hydroxyl content indicates that the glass contains less moisture and impurities, making it suitable for applications in scenarios with high optical requirements.
[0107] Thermal stability: Higher thermal stability indicates that the glass is more capable of maintaining its properties in high temperature environments.
[0108] Experimental samples
[0109] Samples of existing preparation method (control group):
[0110] The conventional low-hydroxyl optical glass preparation method is followed, and the main steps include: conventional raw material processing, conventional melting (without special protective gas or vacuum processing), conventional degassing treatment (lower temperature and no stirring), and conventional annealing treatment (lower temperature, conventional atmosphere).
[0111] Samples prepared by the present invention (experimental group):
[0112] The low-hydroxyl optical glass preparation method of the present invention comprises the following steps: high-purity raw material processing, vacuum melting (using high-purity argon or helium protection), high-temperature degassing treatment (with stirring and phosphorus pentoxide addition), and optimized annealing treatment (using krypton or helium).
[0113] Experimental procedures
[0114] Sample preparation: Glass samples were prepared for the control group and the experimental group, with at least 10 samples in each group to ensure the statistical significance of the data.
[0115] Optical transmittance test: Use a spectrophotometer to test the optical transmittance of each sample in the range of 200nm to 2000nm, focusing on the transmittance in the visible light region (400-800nm).
[0116] Mechanical strength test: The flexural strength (MPa) of the samples was tested using a three-point bending tester, and the maximum flexural strength of each sample was recorded.
[0117] Hydroxyl content test: Fourier transform infrared spectroscopy (FTIR) was used to test the hydroxyl content in the sample, and the hydroxyl content (ppm) was estimated by measuring the OH absorption peak intensity.
[0118] Thermal stability test: The samples were subjected to high temperature treatment (500°C for 1 hour), and then the changes in their optical transmittance and mechanical strength were measured to evaluate the thermal stability.
[0119] Experimental data table:
[0120]
[0121]
[0122] Experimental results analysis
[0123] Optical transmittance: The optical transmittance of the samples in the experimental group was significantly higher than that in the control group, indicating that the method of the present invention is more effective in reducing impurities and bubbles, and the produced glass has higher purity and transparency.
[0124] Mechanical strength: The flexural strength of the samples in the experimental group was significantly higher than that in the control group, indicating that the method of the present invention more effectively eliminates internal stress and improves the structural stability of the glass.
[0125] Hydroxyl content: The hydroxyl content of the samples in the experimental group was significantly lower than that in the control group, indicating that the method of the present invention is more efficient in degassing and removing water, and the produced glass is more suitable for applications with high optical requirements.
[0126] Thermal stability: The transmittance and flexural strength of the experimental group samples after high temperature treatment changed less, indicating that the glass produced by the method of the present invention has better performance retention ability in a high temperature environment.
[0127] Summarize:
[0128] Through the above comparative experiments, the preparation method of the present invention shows obvious advantages in key indicators such as optical transmittance, mechanical strength, hydroxyl content and thermal stability. These results prove the superiority of the present method, especially its application potential in producing high-performance low-hydroxyl optical glass.
[0129] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. Low hydroxyl optical glass, characterized in that: The optical glass is composed of the following components in percentage by mass: 60-70% silicon dioxide, 10-15% boron oxide, 5-10% aluminum oxide, 2-5% magnesium oxide, 5-7% lanthanum oxide, 1-2% neodymium oxide, 1-3% cerium oxide, 0.5-2% titanium dioxide, 1-2% yttrium oxide, 0.5-1% phosphorus pentoxide, and 0.1-1% tungsten oxide.
2. A method for preparing low hydroxyl optical glass, used for the low hydroxyl optical glass according to claim 1, characterized in that: The following steps are involved: S1. Prepare silicon dioxide, boron oxide, aluminum oxide, magnesium oxide, lanthanum oxide, neodymium oxide, cerium oxide, titanium dioxide, yttrium oxide, phosphorus pentoxide, and tungsten oxide raw materials; S2. Vacuum melt the processed raw materials, and add argon or nitrogen with a purity of not less than 99.99% as a protective gas during the melting process; S3, degassing the molten glass; S4, cooling the molten glass to 1200-1300° C. for homogenization and maintaining the temperature for 1-2 hours; S5, forming the homogenized glass melt by tape casting or die casting, and continuously maintaining an inert gas environment for cooling and preventing water vapor from entering during the process; S6. Annealing the formed glass to eliminate internal stress.
3. The method for preparing low-hydroxyl optical glass according to claim 2, characterized in that: In the step S1, the purity of the prepared silicon dioxide is not less than 99.99%, and all raw materials are placed in a drying furnace with an internal temperature of 110-150° C. for 120-480 minutes.
4. The method for preparing low-hydroxyl optical glass according to claim 2, characterized in that: In the step S2, the vacuum melting is maintained at a vacuum degree equal to or lower than 10 -5 Under the condition of 200-1200°C, the temperature is melted to 1500-1600°C and maintained for 120-480 minutes.
5. The method for preparing low-hydroxyl optical glass according to claim 4, characterized in that: In the step S2, a high-purity quartz crucible is used as a melting container.
6. The method for preparing low-hydroxyl optical glass according to claim 2, characterized in that: In the step S3, the degassing treatment is carried out by slowly raising and lowering the temperature within the range of 1400-1600° C., and the treatment time is maintained at 120-480 min.
7. The method for preparing low-hydroxyl optical glass according to claim 2, characterized in that: The inert gas in step S6 includes, but is not limited to, krypton, helium and nitrogen.
8. The method for preparing low-hydroxyl optical glass according to claim 2, characterized in that: The annealing treatment in step S7 includes placing the glass melt in a box-type annealing furnace, gradually reducing the temperature to 500-600° C. and maintaining it for at least 240 minutes.
9. The method for preparing low-hydroxyl optical glass according to claim 2, characterized in that: The degassing process in step S3 uses a vacuum degassing furnace at a vacuum degree of less than 10 -6 Torr, and the temperature is controlled in the range of 1400-1600°C.
10. The method for preparing low-hydroxyl optical glass according to claim 9, characterized in that: Phosphorus pentoxide is added during the degassing process and is used by a stirrer to ensure its uniform distribution in the glass melt.