Preparation method of aerogel surface anti-scouring protective coating

Through thermal spraying technology, the anti-shrink protective coating is deposited on the surface of the aerogel material, which solves the problem of easy falling off in high temperature environments, and achieves a coating with high cohesive strength and excellent anti-shrink performance, maintaining the material Lightweight thermal insulation properties.

CN119038951APending Publication Date: 2024-11-29AVIC BEIJING AERONAUTICAL MFG TECH RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410320851.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Due to its low cohesive strength, aerogel materials are easily washed away by airflow in high temperature environments. The existing anti-solution protective coating process has problems such as low coating strength, long process cycle, obvious weight gain and easy cracking.

Method used

Thermal spraying process is used to deposit anti-shrink protective coating on the surface of the aerogel material. By adjusting the spraying process parameters such as power, speed and distance, selecting alloy or ceramic material as coating material, performing preheating and fully melting state spraying, and controlling coating Layer thickness and cohesion strength.

Benefits of technology

A high-quality, evenly distributed anti-shrink protective coating is achieved, which significantly improves the cohesive strength and anti-shrink performance of the coating, extends the service life of the aerogel material, and maintains its lightweight thermal insulation properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038951A_ABST
    Figure CN119038951A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of thermal spraying, and particularly relates to a preparation method of an aerogel surface anti-scouring protective coating. The method comprises the following steps: selecting an aerogel material as a sprayed body; selecting a coating material according to a use environment and a temperature-resistant range of the aerogel material; a thermal spraying process is adopted, the anti-scouring protective coating is prepared on the surface of the aerogel material through spraying deposition by setting spraying process parameters, and the spraying process parameters include that the spraying power is set between 25 KW and 50 KW, the spraying speed is set between 500 mm / s and 3000 mm / s, and the spraying distance is controlled between 10 mm and 80 mm. The deposition of the protective coating which is high in quality, uniform in distribution, high in cohesion strength and excellent in anti-scouring performance is realized by accurately controlling thermal spraying process parameters.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal spraying, and in particular relates to a method for preparing an anti-scouring protective coating on the surface of an aerogel. Background Art

[0002] Aerogel is a nanoporous solid material with a three-dimensional skeleton structure formed by nanoscale particles / fibers cross-linked with nano-voids (see Figure 1 , Figure 2 ). Aerogel materials have great application potential in thermal insulation materials due to their large specific surface area, high porosity (more than 80% of aerogel is air), low density (its bulk density is adjustable within the range of 0.003-0.500g / cm-3, and the density of air is 0.00129g / cm-3), and extremely low thermal conductivity. Aerogel materials have very good thermal insulation effects, are light in weight and have good thermal insulation. Aerogels that are only one inch thick are equivalent to the thermal insulation function of 20 to 30 pieces of ordinary glass. Therefore, they are favored by aerospace and have broad application prospects in the field of thermal insulation, especially in hypersonic aircraft, where there is a huge demand for their application. They are called "magic materials that will change the world."

[0003] However, due to the low cohesive strength (<1MPa) caused by the nanoporous morphology of the three-dimensional skeleton structure, aerogel materials have poor mechanical properties, high brittleness and easy to break, making them particularly vulnerable to airflow erosion and unable to be used alone in a space with airflow. The greater the airflow speed, the faster the material will be blown away and fail, and a surface anti-erosion protective coating is urgently needed.

[0004] The existing technology generally adopts the following two methods to prepare surface anti-erosion protective coatings:

[0005] The first method is to prepare a protective coating by preparing a coating with a specific composition and applying the coating to the surface of a phenolic resin aerogel material using a coating process method, and then provide high temperature oxidation protection to the base material after drying. However, there are problems and disadvantages: (1) The coating strength of the physical coating method is low and not resistant to erosion; (2) The coating process has a long cycle, including coating and drying and curing; (3) It is difficult to control the uniformity of the coating structure and thickness; (4) The weight gain is obvious (due to the characteristics of the process, there are a variety of adhesives and dispersants in the coating, and the coating weight gain is obvious); (5) The heat treatment process to remove the adhesive makes the base material susceptible to heat damage; (6) It is easy to crack (the service life is very short at high temperatures, and the coating layer is easy to crack as its main failure mode).

[0006] The second method uses hydrophobic silicone rubber RTV-1 as a membrane base material and methyltriethoxysilane-modified SiO2 aerogel with a network structure as a filler to prepare a super-hydrophobic modified SiO2 aerogel / RTV-1 coating. This method is an improved material preparation method and does not fall into the category of material surface protective coating preparation. Summary of the invention

[0007] 1. Technical issues to be resolved

[0008] The present invention mainly aims at the above problems and proposes a method for preparing an anti-scouring protective coating on the surface of an aerogel. Its purpose is to solve how to prepare a protective coating by direct deposition on the surface of an aerogel material through a thermal spraying process, to achieve high cohesive strength and excellent anti-scouring performance of the protective coating, and to effectively solve the problem that aerogel materials fail due to rapid shedding under airflow scouring in a high temperature environment due to low cohesive strength, to overcome the key technical problem that aerogel surface coatings are difficult to deposit, and at the same time to ensure the overall lightweight and thermal insulation advantages of aerogel materials with protective coatings.

[0009] (II) Technical solution

[0010] To achieve the above object, the present invention provides a method for preparing an aerogel surface anti-scour protective coating, comprising the following steps:

[0011] Selecting aerogel material as the sprayed body;

[0012] Selecting a coating material according to the use environment and the temperature resistance range of the aerogel material;

[0013] The anti-erosion protective coating is prepared by spraying and depositing on the surface of the aerogel material by using a thermal spraying process and setting spraying process parameters. The spraying process parameters include: the spraying power is set between 25KW and 50KW, the spraying speed is set between 500mm / s and 3000mm / s, and the spraying distance is controlled between 10mm and 80mm.

[0014] Furthermore, the coating material is selected from alloy materials, carbide ceramic materials, boride ceramic materials, oxide ceramic materials or a mixture of the above materials, and the powder particle size is controlled at 10 μm-50 μm.

[0015] Furthermore, the thermal spraying process includes flame spraying, arc spraying, plasma spraying, HVOF, detonation spraying or cold spraying.

[0016] Furthermore, before the thermal spraying process is adopted, it also includes: using a plasma flame flow to preheat the surface of the aerogel material, and the spraying distance and spraying speed during the preheating are consistent with the spraying distance and spraying speed during the spraying process.

[0017] Furthermore, during the thermal spraying process, the primary gas flow rate is reduced and the secondary gas flow rate is increased so that the sprayed particles can be fully molten.

[0018] Furthermore, the thickness of the anti-scour protective coating is controlled within the range of 0.2 mm to 2.0 mm.

[0019] Furthermore, the deposition thickness of a single layer of the anti-scour protective coating does not exceed 0.01 mm.

[0020] Furthermore, the aerogel material is a mullite fiber reinforced SiO2 aerogel material.

[0021] (III) Beneficial effects

[0022] Compared with the prior art, the method for preparing an aerogel surface anti-scouring protective coating provided by the present invention achieves the deposition of a high-quality, uniformly distributed protective coating with high cohesive strength and excellent anti-scouring performance by precisely controlling the thermal spraying process parameters. Such technical effects are due to:

[0023] 1. High-power thermal spraying: Maintaining a high power range of 25KW to 50KW allows the sprayed particles to reach a fully molten or over-molten state. This is in contrast to conventional plasma spraying. In this solution, by reducing the primary gas flow and appropriately increasing the secondary gas flow, the flame enthalpy and temperature are increased, thereby increasing the degree of particle melting and the spreadability on the surface of the substrate material. This not only avoids the possible scouring effect of the flame flow on the substrate material, but also enhances the bonding strength of the coating, because fully molten particles are more likely to form a stable and continuous coating after hitting the substrate surface.

[0024] 2. Fast spraying speed: Setting the spraying speed to over 500mm / s, which is much higher than the traditional spraying speed standard (the traditional spraying speed is usually less than 500mm / s), helps to reduce the local airflow scouring effect and prevent the local temperature rise and excessive internal stress caused by the excessive thickness of the single-layer coating deposition (over 0.01mm), which may cause the coating to peel off. Fast spraying also helps to shorten the time for particles to contact and cool with the air, so that the particles still maintain sufficient heat and fluidity when they hit the substrate surface, promoting better coating formation.

[0025] 3. Close-range spraying: Optimize the spraying distance to 10mm to 80mm, which is shorter than the distance used in traditional plasma spraying. It can effectively reduce the cooling of molten particles during flight, and further ensure that the particles still have good liquid fluidity when they reach the surface of the substrate, which is beneficial to improve the density and adhesion of the coating.

[0026] In summary, the preparation method proposed in this scheme utilizes the special selection and control of the above-mentioned process parameters, which not only effectively improves the quality of the coating, but also maintains the advantages of lightweight and thermal insulation of aerogel materials, while significantly improving the service life and functionality under extreme conditions, and broadening the application range of aerogel materials in high temperature environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1This is a schematic diagram of the appearance of an aerogel material disclosed in this application.

[0028] Figure 2 This is a schematic diagram of the structure of a SiO2 aerogel disclosed in this application.

[0029] Figure 3 This is a schematic diagram of a surface protective coating of a mullite fiber reinforced SiO2 aerogel material disclosed in this application.

[0030] Figure 4 This is a curve chart of the weight loss value of an aerogel matrix after air flow scouring for 120 seconds disclosed in this application.

[0031] Figure 5 This is a graph showing the weight loss values ​​of three groups of coatings after air flow scouring for 24 hours disclosed in this application.

[0032] Reference numerals shown in the figure: 1, base material; 2, coating. DETAILED DESCRIPTION

[0033] The following are specific embodiments of the present invention, which are intended to further illustrate the technical solution of the present invention. Through the detailed description below, those skilled in the art should understand that these embodiments are only used to illustrate the present invention rather than to limit the scope of protection of the present invention.

[0034] Example 1

[0035] A method for preparing a surface plasma sprayed Y2O3-ZrO2 protective coating on a mullite fiber reinforced SiO2 aerogel substrate, the preparation method comprising the following steps:

[0036] Step 1, material selection and pretreatment: Select mullite fiber reinforced SiO2 aerogel as the matrix material 1 (see Figure 3 ). The surface is simply treated to remove foreign matter and impurities on the surface. Then, preheating is performed, and the surface of the base material 1 is heated using a plasma flame flow at a spraying distance of 50 mm and a spraying speed of 800 mm / s to reduce the temperature difference during the thermal spraying process.

[0037] Step 2, thermal spraying process: Use plasma spraying technology, select 7% Y2O3-ZrO2 powder material (particle size range 30μm) as the spraying material. Perform thermal spraying according to the following parameters:

[0038] Current: 470A; Voltage: 65V; Spraying power: 30KW; Main air flow: 40L / min; Secondary air flow: 5.0L / min; Spraying distance: 50mm; Spraying speed: 800mm / s.

[0039] Step 3, coating 2 thickness control and deposition: spray multiple times under the above thermal spraying process parameters until the required coating 2 thickness of 1.0 mm is reached. Ensure the uniformity of the coating and check the coating 2 layer by layer as needed (see Figure 3 )quality.

[0040] Step 4, post-processing and testing: After spraying, the surface quality of the coating 2 is inspected, including the uniformity and defects of the coating 2. Then, the cohesive strength test is performed.

[0041] Example 2

[0042] A method for preparing a high temperature resistant and anti-scour protective coating, the method comprising the following steps:

[0043] Step 1, material selection and pretreatment: Mullite fiber reinforced SiO2 aerogel is selected as the base material 1. Its surface is simply treated to remove foreign matter and impurities on the surface. Then, preheating is performed, and the surface of the base material 1 is heated using a plasma flame flow at a spraying distance of 70 mm and a spraying speed of 1000 mm / s to reduce the temperature difference during the thermal spraying process.

[0044] Step 2, thermal spraying process: Use plasma spraying technology, select 7% Y2O3-ZrO2 powder material (particle size range 10μm) as the spraying material. Perform thermal spraying according to the following parameters:

[0045] Current: 480A; Voltage: 68V; Spraying power: 32.6KW; Main air flow: 40L / min; Secondary air flow: 6.0L / min; Spraying distance: 70mm; Spraying speed: 1000mm / s.

[0046] Step 3, coating 2 thickness control and deposition: spray multiple times under the above thermal spraying process parameters until the required coating 2 thickness of 0.2 mm is reached. Ensure the uniformity of coating 2 and check the quality of coating 2 layer by layer as needed.

[0047] Step 4, post-processing and testing: After spraying, the surface quality of the coating 2 is inspected, including the uniformity and defects of the coating 2. Then, the cohesive strength test is performed.

[0048] Example 3

[0049] The preparation method of the optimized anti-scour protective coating comprises the following steps:

[0050] Step 1, material selection and pretreatment: Select mullite fiber reinforced SiO2 aerogel as the base material 1. Simply treat its surface to remove foreign matter and impurities on the surface. Then, preheat it, use plasma flame flow to heat the surface of the base material at a spraying distance of 80mm and a spraying speed of 1300mm / s to reduce the temperature difference during thermal spraying.

[0051] Step 2, thermal spraying process: using plasma spraying technology, select 7% Y2O3-ZrO2 powder material (particle size range 50μm) as the spraying material. Perform thermal spraying according to the following parameters:

[0052] Current: 500A; Voltage: 70V; Spraying power: 35KW; Main air flow: 40L / min; Secondary air flow: 8.0L / min; Spraying distance: 80mm; Spraying speed: 1300mm / s.

[0053] Step 3, coating 2 thickness control and deposition: spray multiple times under the above thermal spraying process parameters until the required coating 2 thickness of 2.0 mm is reached. Ensure the uniformity of coating 2 and check the quality of coating 2 layer by layer as needed.

[0054] Step 4, post-processing and testing: After spraying, the surface quality of the coating 2 is inspected, including the uniformity and defects of the coating 2. Then, the cohesive strength test is performed.

[0055] The process parameters of the above-mentioned embodiments 1 to 3 are as follows:

[0056]

[0057]

[0058] Plasma sprayed Y2O3-ZrO2 protective coating cohesive strength test: According to GB / T8642-2002 "Determination of tensile bond strength of thermal spraying". Because the cohesive strength of mullite fiber reinforced SiO2 aerogel material is too low to be tested by the above standard test, the ASTM D790 method is used to test its bending strength for macroscopic comparison.

[0059] The results are shown in the table below:

[0060]

[0061] Among them, the average bending strength of the mullite fiber reinforced SiO2 aerogel material is 0.86MPa, while the average cohesive strength of the Y2O3-ZrO2 coatings prepared in Examples 1-3 is above 32MPa, and the lowest cohesive strength of a single sample is above 29MPa, indicating that coating 2 has excellent cohesive strength, which is very beneficial to the anti-scouring performance of coating 2.

[0062] Comparison of the anti-scouring performance test results of mullite fiber reinforced SiO2 aerogel material and aerogel with protective coating samples:

[0063] Test conditions: air flow velocity is 20m / s, ambient temperature (1200℃), sample weight loss is in grams.

[0064] Under the same test environment, the weight loss results (g) of the substrate and coating after air flow scouring are shown in the following table:

[0065]

[0066] Figure 4 , Figure 5 The graphs show the weight loss measurement results of the mullite fiber reinforced SiO2 aerogel material matrix itself and the sample with an anti-scour protective coating under the same air flow velocity (20m / s) and the same ambient temperature (1200℃) test conditions.

[0067] Among them, the aerogel matrix material dispersed and peeled off very quickly in the scouring sample. After 120 seconds, the matrix sample was almost completely blown away, resulting in complete failure. The weight loss of the five samples was 15.3 grams to 17.5 grams, with an average weight loss of 16.4 grams.

[0068] For the samples with plasma sprayed anti-scour protective coating on the surface, under the same test conditions, after 24 hours of high-temperature airflow test, the weight loss of the samples was very small, ranging from 0.11 grams to 0.5 grams. Among them, the weight loss of the coating in Example 2 was the smallest, and the weight loss of the five samples ranged from 0.11 grams to 0.17 grams, with an average weight loss of 0.15 grams. The coating was intact and had no peeling, and there was no damage or change visible to the naked eye. The internal aerogel matrix material was intact, showing a very excellent protection function against high-temperature airflow scour.

[0069] The above embodiments illustrate the preparation method of the aerogel surface anti-scouring protective coating of the present invention. By adjusting the thermal spraying process parameters, a protective coating with high cohesive strength and excellent scouring resistance is successfully formed on the surface of the aerogel material, and the lightweight thermal insulation properties of the aerogel material are ensured.

[0070] Therefore, no matter from which point of view, the embodiments should be regarded as illustrative and non-restrictive, and the scope of the present application is limited by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present application. Any figure mark in the claims should not be regarded as limiting the claims involved. In addition, it is obvious that the word "comprising" does not exclude other units or steps, and the singular does not exclude the plural. Multiple units or devices stated in the device claim can also be implemented by the same unit or device through software or hardware. The words first, second, etc. are used to indicate names, and do not indicate any particular order.

[0071] The above embodiments are only used to illustrate the technical solution of the present application and are not intended to limit it. Although the present application has been described in detail with reference to the preferred embodiments, a person skilled in the art should understand that the technical solution of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application.

Claims

1. A method for preparing an anti-scour protective coating on an aerogel surface, characterized in that: The following steps are involved: Selecting aerogel material as the sprayed body; Selecting a coating material according to the use environment and the temperature resistance range of the aerogel material; The anti-erosion protective coating is prepared by spraying and depositing on the surface of the aerogel material by using a thermal spraying process and setting spraying process parameters. The spraying process parameters include: the spraying power is set between 25KW and 50KW, the spraying speed is set between 500mm / s and 3000mm / s, and the spraying distance is controlled between 10mm and 80mm.

2. The method for preparing an aerogel surface anti-scour protective coating according to claim 1, characterized in that: The coating material is selected from alloy materials, carbide ceramic materials, boride ceramic materials, oxide ceramic materials or a mixture of the above materials, and the powder particle size is controlled at 10 μm-50 μm.

3. The method for preparing an aerogel surface anti-scour protective coating according to claim 1, characterized in that: The thermal spraying process includes flame spraying, arc spraying, plasma spraying, HVOF, detonation spraying or cold spraying.

4. The method for preparing an aerogel surface anti-erosion protective coating according to claim 1, characterized in that: Before the thermal spraying process is adopted, the method further includes: preheating the surface of the aerogel material using a plasma flame flow, and the spraying distance and spraying speed during the preheating are consistent with the spraying distance and spraying speed during the spraying process.

5. The method for preparing an aerogel surface anti-scour protective coating according to claim 1, characterized in that: During the thermal spraying process, the main gas flow rate is reduced and the secondary gas flow rate is increased to achieve a fully molten state of the sprayed particles.

6. The method for preparing an aerogel surface anti-erosion protective coating according to claim 1, characterized in that: The thickness of the anti-scour protective coating is controlled within the range of 0.2 mm to 2.0 mm.

7. The method for preparing an aerogel surface anti-erosion protective coating according to claim 1, characterized in that: The deposition thickness of a single layer of the anti-scour protective coating does not exceed 0.01 mm.

8. The method for preparing an aerogel surface anti-scour protective coating according to claim 1, characterized in that: The aerogel material is a mullite fiber reinforced SiO2 aerogel material.