Barium titanate ceramic as well as preparation method and application thereof

CN119038985APending Publication Date: 2024-11-29SHENZHEN INST OF ADVANCED ELECTRONICS MATERIALS +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410957948.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

而两段式烧结工艺所得到的陶瓷晶粒尺寸仍为μm级别,不能满足纳米晶陶瓷的需要求,限制了MLCC的进一步发展

Benefits of technology

[0031] The present invention accurately fits the temperature and holding time parameters in the sintering path at each sintering stage, especially focusing on significantly improving the efficiency of the initial stage of the sintering process. In this process, the initial sintering path is carefully designed as a gentle rising stage with a lower slope, aiming to prolong the densification process of ceramic materials and ensure that the ceramic body can fully undergo structural compaction before reaching a density of more than 95%. Subsequently, when the material density reaches the standard and reaches the threshold of rapid grain size growth, the slope of the sintering path increases rapidly. Although the density growth tends to stagnate at this stage, it effectively promotes the refinement and uniformization of grains. At the same time, The grain size of the final ceramic product is strictly controlled. By implementing the present invention, a barium titanate ceramic material with an average grain size of 630 nanometers and a density exceeding 92% has been successfully produced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038985A_ABST
    Figure CN119038985A_ABST
Patent Text Reader

Abstract

The invention discloses barium titanate ceramic as well as a preparation method and application thereof. The preparation method comprises the following steps: mixing barium titanate raw material powder with a binder, tabletting, and then carrying out multi-stage sintering, the multi-stage sintering sequentially comprises the following stages of platform heat preservation sintering, wherein after the temperature is increased to 1130-1150 DEG C, heat preservation is conducted for 5-10 min; sintering at high temperature: raising the temperature to 1150-1180 DEG C without heat preservation; the heating temperature of high-temperature sintering is higher than the heating temperature of platform heat preservation sintering; and low-temperature heat-preservation sintering: cooling to 850-950 DEG C, and then preserving heat for 20-30 hours. On the basis of ceramic sintering dynamics, sintering process temperatures and heat preservation time in different stages are determined by fitting a sintering path in the sintering process, so that the densification stage time of the ceramic in the sintering process is prolonged, and the ceramic density is improved while the ceramic grain size is controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of barium titanate ceramics, and in particular to a barium titanate ceramic and a preparation method and application thereof. Background Art

[0002] Barium titanate is the first commercial ferroelectric and piezoelectric ceramic material. It has attracted much attention in the field of electronic components due to its high dielectric constant and other properties, and is widely used in the preparation of multilayer ceramic capacitors (MLCC). Due to the miniaturization and high performance requirements of MLCC, the grains of barium titanate ceramic raw materials need to maintain high density while reducing their size to meet reliability requirements.

[0003] At present, the sintering process of barium titanate ceramic powder includes two-step pressureless sintering, hot pressing sintering, plasma spark sintering, etc. Among them, the two-step pressureless sintering is easy to operate and has low equipment requirements. At the same time, the sintered ceramic powder is relatively uniform, and the reliability and piezoelectric performance are improved. However, due to the trend of miniaturization of MLCC devices, the barium titanate ceramic dielectric layer needs to be thinned not only, but also the grain size of the sintered barium titanate ceramic powder needs to be further reduced. The ceramic grain size obtained by the two-stage sintering process is still at the μm level, which cannot meet the requirements of nanocrystalline ceramics and limits the further development of MLCC. Summary of the invention

[0004] In view of the above technical problems, the present invention provides a barium titanate ceramic and a preparation method and application thereof. The present invention improves the two-stage sintering process of the barium titanate ceramic, refines the grains and improves the density at the same time.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] In one aspect, the present invention provides a method for preparing a barium titanate ceramic, comprising the following steps:

[0007] The barium titanate raw material powder is mixed with a binder and pressed into tablets, and then sintered in multiple stages;

[0008] The multi-stage sintering includes the following stages in sequence:

[0009] Platform insulation sintering: heat up to 1130-1150℃ and keep warm for 5-10 minutes;

[0010] High temperature sintering: heating to 1150-1180°C without heat preservation; the heating temperature of the high temperature sintering is greater than the heating temperature of the platform heat preservation sintering;

[0011] Low temperature insulation sintering: cool down to 850-950℃ and keep warm for 20-30h.

[0012] As a preferred embodiment, the particle size of the barium titanate raw material powder is 100 to 180 nm;

[0013] And / or, the binder is polyvinyl alcohol; in some specific embodiments, the binder is a polyvinyl alcohol solution with a concentration of 5-8 wt %.

[0014] As a preferred embodiment, before the multi-stage sintering, a water drainage and binder removal process is further included; the water drainage and binder removal process is to remove the moisture and binder in the tablets;

[0015] In some specific embodiments, the drainage and debinding process comprises the following steps:

[0016] S1: Treat at 250-300℃ for 25-30min;

[0017] S2550~600℃ for 25~30min;

[0018] Preferably, the heating rate in step S1 is 1 to 5°C / min;

[0019] Preferably, the heating rate in step S2 is 1-5° C. / min.

[0020] As a preferred embodiment, during the platform heat preservation sintering, the heating rate is 5-10°C / min.

[0021] As a preferred embodiment, during the high temperature sintering, the heating rate is 5 to 10° C. / min.

[0022] As a preferred embodiment, during the low-temperature heat preservation sintering, the cooling rate is 15-20°C / min.

[0023] As a preferred embodiment, the barium titanate raw material powder and the binder are ground and sieved before mixing;

[0024] Preferably, the mesh number of the sieving is ≥200 mesh;

[0025] Preferably, the tabletting pressure is 350-365 MPa.

[0026] Preferably, the tableting time is 18 to 20 seconds.

[0027] In another aspect, the present invention provides barium titanate ceramics obtained by the above preparation method.

[0028] In another aspect, the present invention provides use of the above-mentioned barium titanate ceramic in electronic packaging;

[0029] Preferably, the invention is used for preparing MLCC.

[0030] The above technical solution has the following advantages or beneficial effects:

[0031] The present invention focuses on significantly improving the performance of the initial stage of the sintering process by accurately fitting the temperature and holding time parameters in the sintering path at each sintering stage. In this process, the initial sintering path is carefully designed as a gently rising stage with a relatively low slope, aiming to prolong the densification process of the ceramic material and ensure that the ceramic body can be fully structurally compacted before reaching a density of more than 95%. Subsequently, when the material density meets the standard and enters the threshold of rapid growth in grain size, the slope of the sintering path increases rapidly. Although the density growth tends to stagnate at this stage, it effectively promotes the refinement and homogenization of the grains, while strictly controlling the grain size of the final ceramic product. The implementation of the present invention successfully produced a barium titanate ceramic material with an average grain size of 630 nanometers and a density of more than 92%. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a flow chart of the sintering process of barium titanate ceramics in Examples 1-4 of the present invention.

[0033] Figure 2 The scanning electron microscope (SEM) images and particle size statistics of the barium titanate ceramics sintered in Examples 1-4 and Comparative Examples 1-2 of the present invention are shown.

[0034] Figure 3 The scanning electron microscope (SEM) images and particle size statistics of the barium titanate ceramics sintered in Comparative Examples 3-8 of the present invention are shown. DETAILED DESCRIPTION

[0035] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.

[0036] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.

[0037] Example 1

[0038] This embodiment provides a barium titanate ceramic, and the preparation method is as follows:

[0039] 7 g of barium titanate powder with a particle size of 100 nm and 1.05 g of 8 wt% polyvinyl alcohol solution (PVA solution, binder) were mixed in a mortar and then passed through a 200 mesh sieve; 0.35 g was weighed and cold-pressed into tablets at a pressure of 350 MPa for 20 seconds;

[0040] The pressed ceramic sheet is sintered; the sintering process in this embodiment is as follows Figure 1 As shown, the following process is included:

[0041] Drainage and debinding stage: heat up to 300℃ at a heating rate of 1℃ / min and keep warm for 30min to remove moisture; then heat up to 600℃ at the same rate and keep warm for 30min to remove residual PVA adhesive;

[0042] Stage (1) is platform heat preservation sintering: the temperature is raised to the target temperature at a rate of 10°C / min and then kept warm;

[0043] Stage (2) high temperature sintering: continue heating at a rate of 10°C / min to the target temperature without keeping warm;

[0044] Stage (3) low temperature sintering: cooling to the target temperature at a cooling rate of 20°C / min and then maintaining the temperature.

[0045] The temperature and holding time of each sintering stage in this embodiment are shown in Table 1.

[0046] The SEM images and density of the barium titanate ceramics prepared in this example are shown in Figure 2 As shown in a and Table 1, the ceramic grain size obtained by SEM statistics is 631.15 nm, and the ceramic density measured by the Archimedean drainage method is 92.26%.

[0047] Table 1

[0048]

[0049]

[0050] Example 2

[0051] The preparation method of the barium titanate ceramic in this embodiment is the same as that in Embodiment 1, except that the sintering process is different, as follows:

[0052] 7g of barium titanate powder with a particle size of 100nm and 1.05g of 8wt% PVA solution were mixed in a mortar and then passed through a 200-mesh sieve; 0.35g was weighed and cold-pressed into tablets at a pressure of 350MPa for 20s;

[0053] The pressed ceramic sheet is sintered, and the sintering process includes the following steps:

[0054] Drainage and debinding stage: heat up to 300℃ at a heating rate of 1℃ / min and keep warm for 30min to remove moisture; then heat up to 600℃ at the same rate and keep warm for 30min to remove residual PVA adhesive;

[0055] Stage (1) is platform heat preservation sintering: heating to 1130°C at a rate of 10°C / min and keeping at that temperature for 5 min;

[0056] Stage (2) high temperature sintering: continue heating at a rate of 10°C / min to the target temperature without keeping warm;

[0057] Stage (3) low temperature sintering: cooling to the target temperature at a cooling rate of 20°C / min and then maintaining the temperature.

[0058] The temperature and holding time of each sintering stage in this embodiment are shown in Table 1.

[0059] The SEM images and density of the barium titanate ceramics prepared in this example are shown in Figure 2 b and Table 1, the ceramic grain size obtained by SEM statistics is 726.35 nm, and the ceramic density measured by the Archimedean drainage method is 92.99%.

[0060] Example 3

[0061] The preparation method of the barium titanate ceramic in this embodiment is the same as that in Embodiment 1, except that the sintering process is different, as follows:

[0062] 7g of barium titanate powder with a particle size of 100nm and 1.05g of 8wt% PVA solution were mixed in a mortar and then passed through a 200-mesh sieve; 0.35g was weighed and cold-pressed into tablets at a pressure of 350MPa for 20s;

[0063] The pressed ceramic sheets are sintered in a furnace, and the sintering process includes the following steps:

[0064] Drainage and debinding stage: heat up to 300℃ at a heating rate of 1℃ / min and keep warm for 30min to remove moisture; then heat up to 600℃ at the same rate and keep warm for 30min to remove residual PVA adhesive;

[0065] Stage (1) is platform heat preservation sintering: heating to the target temperature at a rate of 10°C / min and keeping the temperature for 10 min.

[0066] Stage (2) high temperature sintering: heating to 1150°C at a rate of 10°C / min without insulation;

[0067] Stage (3) low temperature sintering: rapidly cool to the target temperature at a cooling rate of 20°C / min and then keep warm.

[0068] The temperature and holding time of each sintering stage in this embodiment are shown in Table 1.

[0069] The SEM images and density of the barium titanate ceramics prepared in this example are shown in Figure 2 c and Table 1, the ceramic grain size obtained by SEM statistics is 709.31 nm, and the ceramic density measured by the Archimedean drainage method is 91.78%.

[0070] Example 4

[0071] The preparation method of the barium titanate ceramic in this embodiment is the same as that in Embodiment 1, except that the sintering process is different, as follows:

[0072] 7g of barium titanate powder with a particle size of 100nm and 1.05g of 8wt% PVA solution were mixed in a mortar and then passed through a 200-mesh sieve; 0.35g of the mixed powder was weighed and cold-pressed into tablets at a pressure of 350MPa for 20s;

[0073] The pressed ceramic sheet is sintered, and the sintering process includes the following steps:

[0074] Drainage and debinding stage: heat up to 300℃ at a heating rate of 1℃ / min and keep warm for 30min to remove moisture; then heat up to 600℃ at the same rate and keep warm for 30min to remove residual PVA adhesive;

[0075] Stage (1) is platform heat preservation sintering: the temperature is raised to the target temperature at a rate of 10°C / min and then kept warm;

[0076] Stage (2) high temperature sintering: continue heating at a rate of 10°C / min to the target temperature without keeping warm;

[0077] Stage (3) low temperature sintering: cooling to the target temperature at a cooling rate of 20°C / min and then maintaining the temperature.

[0078] The temperature and holding time of each sintering stage in this embodiment are shown in Table 1.

[0079] The SEM images and density of the barium titanate ceramics prepared in this example are shown in Figure 2 As shown in d and Table 1, the ceramic grain size obtained by SEM statistics is 560.85 nm, and the ceramic density measured by the Archimedean drainage method is 89.96%.

[0080] Comparative Example 1

[0081] The preparation method of the barium titanate ceramic in this comparative example is the same as that in Example 1. The temperature and holding time of each sintering stage are shown in Table 1. The difference is that the temperature in the sintering stage (2) is 1200°C.

[0082] The SEM images and density of the barium titanate ceramics prepared in this comparative example are shown in FIG. Figure 2 As shown in e and Table 1, the ceramic grain size obtained by SEM statistics is 1065.66 nm, and the ceramic density measured by the Archimedean drainage method is 97.83%.

[0083] Comparative Example 2

[0084] The preparation method of the barium titanate ceramic in this comparative example is the same as that in Example 1. The temperature and holding time of each sintering stage are shown in Table 1. The difference is that the temperature of the sintering stage (3) is 950°C.

[0085] The SEM images and density of the barium titanate ceramics prepared in this comparative example are shown in FIG. Figure 2 As shown in f and Table 1, the ceramic grain size obtained by SEM statistics is 1264.13 nm, and the ceramic density measured by the Archimedean drainage method is 95.18%.

[0086] Comparative Example 3

[0087] The preparation method of the barium titanate ceramic in this comparative example is the same as that in Example 2. The temperature and holding time of each sintering stage are shown in Table 1. The difference is that the sintering platform temperature of the two-stage sintering is 1150°C.

[0088] The SEM images and density of the barium titanate ceramics prepared in this comparative example are shown in FIG. Figure 3 As shown in a and Table 1, the ceramic grain size obtained by SEM statistics is 62921nm, and the ceramic density measured by the Archimedean drainage method is 85.40%.

[0089] Comparative Example 4

[0090] The preparation method of barium titanate ceramics in this comparative example is the same as that in Example 1. The temperature and holding time of each sintering stage are shown in Table 1. The difference is that the temperature of stage (1) is 1050°C and the holding time is 10 min; the temperature of stage (2) is 1150°C.

[0091] The SEM images and density of the barium titanate ceramics prepared in this comparative example are shown in FIG. Figure 3 b and Table 1, the ceramic grain size obtained by SEM statistics is 639.89 nm, and the ceramic density measured by the Archimedean drainage method is 84.44%.

[0092] Comparative Example 5

[0093] The preparation method of the barium titanate ceramic in this comparative example is the same as that in Example 4. The temperature and holding time of each sintering stage are shown in Table 1. The difference is that the temperature of stage (1) is 1100°C.

[0094] The SEM images and density of the barium titanate ceramics prepared in this comparative example are shown in FIG. Figure 3 c and Table 1, the ceramic grain size obtained by SEM statistics is 658.51 nm, and the ceramic density measured by the Archimedean drainage method is 83.39%.

[0095] Comparative Example 6

[0096] The preparation method of barium titanate ceramics in this comparative example is the same as that in Example 1. The temperature and holding time of each sintering stage are shown in Table 1. The difference is that stage (1) is not set and the temperature of stage (2) is 1200°C.

[0097] The SEM images and density of the barium titanate ceramics prepared in this comparative example are shown in FIG. Figure 3 As shown in d and Table 1, the ceramic grain size obtained by SEM statistics is 468nm, and the ceramic density measured by the Archimedean drainage method is 77%.

[0098] Comparative Example 7

[0099] The preparation method of the barium titanate ceramic in this comparative example is the same as that in Example 4. The temperature and holding time of each sintering stage are shown in Table 1. The difference is that stage (1) is not set.

[0100] The SEM images and density of the barium titanate ceramics prepared in this comparative example are shown in FIG. Figure 3 As shown in e and Table 1, the ceramic grain size obtained by SEM statistics is 595.21 nm, and the ceramic density measured by the Archimedean drainage method is 78.38%.

[0101] Comparative Example 8

[0102] The preparation method of the barium titanate ceramic in this comparative example is the same as that in comparative example 3. The temperature and holding time of each sintering stage are shown in Table 1. The difference is that stage (1) is not set and the temperature of stage (3) is 950°C.

[0103] The SEM images and density of the barium titanate ceramics prepared in this comparative example are shown in FIG. Figure 3 As shown in f and Table 1, the ceramic grain size obtained by SEM statistics is 661.64nm, and the ceramic density measured by the Archimedean drainage method is 83.64%.

[0104] It can be seen from the above examples and comparative examples that in the sintering process of the present invention, the platform insulation and the insulation temperature in stage (1) have an important influence on achieving good density. Not setting stage (1) or not setting the insulation temperature high enough is not conducive to achieving good density. If the temperature in stage (2) and stage (3) is too high, the particle size will be too large.

[0105] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing barium titanate ceramics, characterized in that: The following steps are involved: The barium titanate raw material powder is mixed with a binder and pressed into tablets, and then sintered in multiple stages; The multi-stage sintering includes the following stages in sequence: Platform insulation sintering: heat up to 1130-1150℃ and keep warm for 5-10 minutes; High temperature sintering: heating to 1150-1180°C without heat preservation; the heating temperature of the high temperature sintering is greater than the heating temperature of the platform heat preservation sintering; Low temperature insulation sintering: cool down to 850-950℃ and keep warm for 20-30h.

2. The method according to claim 1, characterized in that The particle size of the barium titanate raw material powder is 100 to 180 nm; Preferably, the binder is polyvinyl alcohol; Preferably, the binder is a polyvinyl alcohol solution.

3. The method according to claim 1, characterized in that Before the multi-stage sintering, it also includes drainage and debinding treatment.

4. The method according to claim 3, characterized in that The drainage and debinding process comprises the following steps: S1: Treat at 250-300℃ for 25-30min; S2550~600℃ for 25~30min; Preferably, the heating rate in step S1 is 1 to 5°C / min; Preferably, the heating rate in step S2 is 1-5° C. / min.

5. The method according to claim 1, characterized in that: During the platform heat preservation sintering, the heating rate is 5-10°C / min.

6. The method according to claim 1, characterized in that During the high temperature sintering, the heating rate is 5-10° C. / min.

7. The method according to claim 1, characterized in that During the low-temperature heat preservation sintering, the cooling rate is 15-20°C / min.

8. The method according to claim 1, characterized in that The barium titanate raw material powder and the binder are ground and sieved before mixing; Preferably, the mesh number of the sieving is greater than or equal to 200; Preferably, the tabletting pressure is 350-365 MPa; Preferably, the tableting time is 18 to 20 seconds.

9. A barium titanate ceramic, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the barium titanate ceramic according to claim 9 in electronic packaging; Preferably, the invention is used for preparing MLCC.

Citation Information

Patent Citations

  • Nanocrystalline barium titanate thermal-sensitive ceramic and preparation method thereof

    CN108264344A

  • Preparation method of doped bismuth ferrite-barium titanate-based lead-free piezoelectric ceramic material

    CN114180952A