Preparation method of yttria-stabilized zirconia ceramic green body and yttria-stabilized zirconia toughened alumina ceramic green body
By crosslinking yttrium-stabilized zirconia powder with a water-based dispersant to form a gel network, the inhomogeneity and cracking problems of zirconia and zirconia-toughened alumina ceramic blanks in the prior art were solved, and room temperature curing and crack-free preparation of high solids content slurry were achieved.
Patent Information
- Application Number
- CN202411547651.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-01
- Publication Date
- 2024-11-29
AI Technical Summary
Existing technologies for preparing large-sized or complex-shaped zirconia and zirconia-toughened alumina ceramic preforms suffer from issues such as product inhomogeneity, shape limitations, inconsistent temperatures, and the risk of cracking. Furthermore, they involve a wide variety of additives, complex processes, and potential toxicity.
A gel network was formed by crosslinking yttrium-stabilized zirconia powder with a water-based dispersant containing carboxylate groups. A water-based ceramic slurry with high solid content was prepared by stirring and ball milling. The slurry was then filtered, degassed, and sealed and cured at room temperature to avoid shrinkage and cracking during the drying process.
The integrity of yttrium oxide-stabilized zirconia ceramics and yttrium oxide-stabilized zirconia-toughened alumina ceramic blanks was achieved. The operation is simple, non-toxic and harmless, and the preparation process is free from deformation or cracks.
Smart Images

Figure CN119038990A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ceramic green body forming technology, specifically to a method for preparing yttrium oxide-stabilized zirconia ceramic green bodies and yttrium oxide-stabilized zirconia-toughened alumina ceramic green bodies. Background Technology
[0002] Zirconia ceramics and zirconia-toughened alumina ceramics (ZTA) possess unique properties such as high strength, wear resistance, and high toughness, making them valuable in metallurgy, chemical engineering, and high-end manufacturing equipment. While dry forming is commonly used for these ceramics, it suffers from inhomogeneities and shape limitations when preparing large-sized or complex-shaped products. In contrast, in-situ curing colloidal forming produces ceramic green bodies with uniform particle packing density. This not only lays the foundation for sintering ceramics with uniform microstructures but also allows for lower sintering temperatures, resulting in ceramic materials with superior performance. Furthermore, in-situ curing colloidal forming requires less equipment investment, facilitates the preparation of complex-shaped ceramic green bodies, and reduces manufacturing and subsequent machining costs. Therefore, in-situ curing colloidal forming represents a new direction for the development of high-performance zirconia and zirconia-toughened alumina ceramics.
[0003] Classic in-situ curing colloidal molding methods include gel casting and direct solidification. Chinese invention patent CN111908916A discloses a gel casting method for zirconia ceramics. Based on the classic gel casting system of acrylamide, it modifies acrylamide with B-ester and formaldehyde to increase the solid content of the slurry. Hydroquinone is added to the slurry to eliminate oxygen and prevent oxygen inhibition during curing, thus preparing zirconia ceramics with a relative density greater than 95%. However, this method requires the addition of many types of organic compounds, has a complex process, and suffers from acrylamide toxicity. Chinese invention patent CN105084874A discloses a solidification method for alumina and ZTA ceramics. By adding 1.5-3.5% food-grade glutinous rice flour as a gelling agent to the slurry, the curing of alumina and ZTA slurries is achieved. This method uses fewer additives, but the curing of glutinous rice flour requires a water bath at 70-90℃. During the water bath, the temperature difference between the inside and outside of the green body leads to inconsistent curing processes, making it difficult to guarantee the overall integrity of the green body, especially large or complex-shaped ceramic green bodies. Chinese invention patent CN108101534A discloses a method for gel casting to form yttrium oxide partially stabilized zirconia ceramic crucibles. It utilizes the principle of curing yttrium oxide sol and ammonium chloride at room temperature. Yttrium oxide sol and ammonium chloride curing agent are introduced sequentially into the yttrium oxide partially stabilized zirconia powder slurry to achieve curing. This method cures at room temperature, and the introduced yttrium oxide gel can act as a zirconia stabilizer after the slurry has cured and dried. However, it does not mention the dispersion of the slurry. Due to the presence of yttrium oxide gel, the solid content of the slurry is difficult to increase, resulting in a green body with low relative density, large drying shrinkage, and a high risk of cracking.
[0004] Therefore, how to provide a simple and easy method for preparing zirconia and zirconia-toughened alumina ceramic preforms has become a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0005] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a method for preparing yttrium oxide stabilized zirconia ceramic green bodies and yttrium oxide stabilized zirconia toughened alumina ceramic green bodies. The method utilizes the yttrium ions generated by the hydration of the stabilizer yttrium oxide in zirconia powder to crosslink with the carboxylate ions in the water-based dispersant to form a gel network, thereby achieving the curing of the slurry. No other curing agents need to be added. The operation is simple, non-toxic and harmless, and the prepared ceramic green body is intact without deformation or cracks.
[0006] The technical solution of this invention is as follows: On one hand, the present invention provides a method for preparing yttrium oxide-stabilized zirconia ceramic green bodies, comprising the following steps: S1 uses yttrium oxide-stabilized zirconia powder as raw material, adds a water-based dispersant containing carboxylate, and prepares a water-based ceramic slurry with a volume solid content >40% by stirring and ball milling. If the volume solid content of the water-based ceramic slurry is <40%, it will cause the green body to shrink greatly during the subsequent drying process and is prone to cracking. S2 measures the rheological properties of the water-based ceramic slurry during the stirring ball milling process. When 0.9 Pa·s < viscosity of the water-based ceramic slurry at a shear rate of 100 / s < 1 Pa·s, the ball milling is stopped. If the viscosity of the water-based ceramic slurry at a shear rate of 100 / s during the stirring ball milling process is > 1 Pa·s, its fluidity will be reduced, which is not conducive to subsequent process operations and will also affect the overall integrity of the green body. S3 filters and degasses the water-based ceramic slurry to remove grinding balls and air, then injects it into the mold and seals it at room temperature to prevent shrinkage and cracking of the green body caused by water evaporation and drying during the curing process of the water-based ceramic slurry. After S4 is placed for 24-48 hours, the water-based ceramic slurry changes from a fluid to an elastomer. Then, it is dried under controlled temperature and humidity to obtain yttrium oxide stabilized zirconia ceramic blank.
[0007] Preferably, in step S1, the water-based dispersant containing carboxylate is an ammonium salt aqueous solution of isobutylene and maleic anhydride copolymer, an ammonium citrate aqueous solution, or an ammonium polyacrylate aqueous solution.
[0008] Preferably, the molar percentage of yttrium oxide in the yttrium-stabilized zirconia powder is 3-8%; and the median diameter of the yttrium-stabilized zirconia powder is 50-500 nm.
[0009] Preferably, the amount of water-based dispersant containing carboxyl groups added is 0.3-3% of the mass of yttrium oxide-stabilized zirconia powder.
[0010] Preferably, in step S1, a stirred ball mill is used to prepare the water-based ceramic slurry. The stirred ball mill uses zirconia grinding balls with a diameter of 5 mm. The volume ratio of the grinding balls to the water-based ceramic slurry is (0.6-0.7):(0.3-0.4). The total volume of the water-based ceramic slurry and the grinding balls accounts for 60-70% of the total volume of the stirred ball mill.
[0011] Preferably, in step S2, the rotation speed of the ball mill during stirring is 80-150 rpm.
[0012] Preferably, in step S2, during the ball milling process, the viscosity of the water-based ceramic slurry is measured every 10 minutes using a rotational rheometer, with the rotor being a flat plate.
[0013] Preferably, in step S3, the temperature is 20-25°C under room temperature conditions.
[0014] Preferably, in step S4, the temperature and humidity controlled drying process is as follows: the temperature is controlled at 25°C, the ambient humidity is controlled above 80%RH in the initial stage of drying, and after 24 hours, the humidity is reduced to 40-60%RH. At the same time, the weight of the green body is weighed. When the weight of the green body no longer decreases, the drying is stopped, and the preparation of the yttrium oxide stabilized zirconia ceramic green body is completed.
[0015] On the other hand, the present invention provides a method for preparing a yttrium-stabilized zirconia-toughened alumina ceramic blank. In the above method for preparing a yttrium-stabilized zirconia ceramic blank, the yttrium-stabilized zirconia powder in step S1 is replaced with a mixed powder of yttrium-stabilized zirconia and alumina, and the alumina content in the mixed powder is 60-90 wt.%.
[0016] Compared with the prior art, the present invention has the following advantages: This invention provides a method for preparing yttrium oxide-stabilized zirconia ceramic green bodies and yttrium oxide-stabilized zirconia-toughened alumina ceramic green bodies. It ingeniously utilizes the yttrium ions generated by the hydration of the yttrium oxide stabilizer in the zirconia powder to crosslink with the carboxylate ions in the water-based dispersant to form a gel network, thereby achieving the curing of the slurry. No other curing agents need to be added. The operation is simple, non-toxic and harmless, and the prepared ceramic green bodies are intact without deformation or cracks. Attached Figure Description
[0017] Figure 1 This is a photograph of the yttrium oxide-stabilized zirconia ceramic preform prepared in Example 1 of the present invention.
[0018] Figure 2 This is a photograph of the yttrium oxide-stabilized zirconia ceramic preform prepared in Example 2 of the present invention.
[0019] Figure 3 This is a photograph of the yttrium oxide-stabilized zirconia ceramic preform prepared in Example 3 of the present invention.
[0020] Figure 4 This is a photograph of the yttrium oxide-stabilized zirconia ceramic preform prepared in Comparative Example 1 of this invention.
[0021] Figure 5 This is a photograph of the yttrium oxide-stabilized zirconia ceramic preform prepared in Comparative Example 2 of this invention.
[0022] Figure 6 This is a photograph of the yttrium oxide-stabilized zirconia ceramic preform prepared in Comparative Example 3 of this invention.
[0023] Figure 7 This is a photograph of the yttrium oxide-stabilized zirconia-toughened alumina ceramic preform prepared in Example 4 of this invention.
[0024] Figure 8 This is a photograph of the yttrium oxide-stabilized zirconia-toughened alumina ceramic preform prepared in Example 5 of this invention.
[0025] Figure 9 This is a photograph of the yttrium oxide-stabilized zirconia-toughened alumina ceramic preform prepared in Example 6 of the present invention.
[0026] Figure 10 This is a photograph of the yttrium oxide-stabilized zirconia-toughened alumina ceramic preform prepared in Comparative Example 4 of this invention.
[0027] Figure 11 This is a photograph of the yttrium oxide-stabilized zirconia-toughened alumina ceramic preform prepared in Comparative Example 5 of this invention.
[0028] Figure 12 This is a photograph of the yttrium oxide-stabilized zirconia-toughened alumina ceramic preform prepared in Comparative Example 6 of this invention. Detailed Implementation
[0029] To enable those skilled in the art to better understand the technical solutions of this invention, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments of this invention.
[0030] Example 1 The method for preparing the yttrium oxide-stabilized zirconia ceramic preform in this embodiment includes the following steps: S1 is used to prepare water-based 3YSZ ceramic slurry. Using 3 mol% yttrium-stabilized zirconia (3YSZ) powder with a D50 of 50 nm as raw material, and an aqueous solution of ammonium polyacrylate with a weight average molecular weight of 5500 as a water-based dispersant with a concentration of 40 wt.%, an 8 L stirred ball mill was used to prepare a water-based 3YSZ ceramic slurry. The total volume of the grinding balls and the water-based 3YSZ ceramic slurry accounted for 60% of the total volume of the stirred ball mill, and the volume ratio of the grinding balls to the water-based 3YSZ ceramic slurry was 0.6:0.4. First, zirconia grinding balls with a diameter of 5 mm were added to the stirred tank of the stirred ball mill, followed by deionized water and ammonium polyacrylate. After stirring evenly, 3YSZ powder was gradually added. The stirring speed during the addition of 3YSZ powder was 40 rpm, and the amount of ammonium polyacrylate added was 3% of the mass of 3YSZ powder. A water-based 3YSZ ceramic slurry with a volume solid content of 48% was prepared.
[0031] S2 Stirring Ball Mill The stirred ball mill was operated at 100 rpm. The viscosity of the water-based 3YSZ ceramic slurry was measured every 10 minutes using a rotational rheometer. The rotor was a flat plate. The viscosity of the water-based 3YSZ ceramic slurry showed a trend of first decreasing and then increasing. After 1.5 hours of stirred ball milling, the viscosity of the water-based 3YSZ ceramic slurry reached 0.95 Pa·s at a shear rate of 100 / s, and the ball milling was stopped.
[0032] S3 filtration and degassing The water-based 3YSZ ceramic slurry is discharged through the filter at the bottom of the stirred ball mill and subjected to vacuum degassing. The degassed water-based 3YSZ ceramic slurry is then poured into an aluminum alloy mold. A thin film is then placed on the upper surface of the mold to keep the water-based 3YSZ ceramic slurry in a sealed environment and allow it to cure in situ at room temperature of 25°C.
[0033] S4 drying After standing for 48 hours, the water-based 3YSZ ceramic slurry gelled. The film was removed, and the ambient temperature was controlled at 25℃ and the humidity at 85%RH for drying. After drying for 24 hours, the ambient humidity was reduced to 50%RH and dried for another 48 hours. The weight of the green body no longer changed, and the drying was completed, obtaining the 3YSZ ceramic green body.
[0034] like Figure 1 As shown, the 3YSZ ceramic blank prepared in this embodiment is a square plate with dimensions of 115mm×115mm×10mm. The 3YSZ ceramic blank is intact and has no deformation or cracks.
[0035] Example 2 The method for preparing the yttrium oxide-stabilized zirconia ceramic preform in this embodiment includes the following steps: S1 is used to prepare water-based 8YSZ ceramic slurry. Using 8 mol% yttrium-stabilized zirconia (8YSZ) powder with a D50 of 500 nm as raw material and 40 wt.% ammonium citrate aqueous solution as water-based dispersant, an 8L stirred ball mill was used to prepare a water-based 8YSZ ceramic slurry. The total volume of the grinding balls and the water-based 8YSZ ceramic slurry accounted for 70% of the total volume of the stirred ball mill, and the volume ratio of the grinding balls to the water-based 8YSZ ceramic slurry was 0.7:0.3. First, zirconia grinding balls with a diameter of 5 mm were added to the stirred tank of the stirred ball mill, followed by deionized water and ammonium citrate. After stirring evenly, 8YSZ powder was gradually added. The stirring speed during the addition of 8YSZ powder was 40 rpm, and the amount of ammonium citrate added was 0.3% of the mass of 8YSZ powder. A water-based 8YSZ ceramic slurry with a volume solid content of 56% was prepared.
[0036] S2 Stirring Ball Mill The stirred ball mill was operated at a speed of 150 rpm. The viscosity of the water-based 8YSZ ceramic slurry was measured every 10 minutes using a rotational rheometer. The rotor was a flat plate. The viscosity of the water-based 8YSZ ceramic slurry showed a trend of first decreasing and then increasing. After 1 hour of stirred ball milling, the viscosity of the water-based 8YSZ ceramic slurry reached 0.93 Pa·s at a shear rate of 100 / s, and the ball milling was stopped.
[0037] S3 filtration and degassing The water-based 8YSZ ceramic slurry is discharged through the filter at the bottom of the stirred ball mill and subjected to vacuum degassing. The degassed water-based 8YSZ ceramic slurry is then poured into an aluminum alloy mold. A thin film is then placed on the upper surface of the mold to keep the water-based 8YSZ ceramic slurry in a sealed environment and allow it to cure in situ at room temperature of 20°C.
[0038] S4 drying After standing for 24 hours, the water-based 8YSZ ceramic slurry gelled. The film was removed, and the ambient temperature was controlled at 25℃ and the humidity at 80%RH for drying. After drying for 24 hours, the ambient humidity was reduced to 40%RH and then dried for another 48 hours. The weight of the green body no longer changed, and the drying was completed, obtaining the 8YSZ ceramic green body.
[0039] like Figure 2 As shown, the 8YSZ ceramic blank prepared in this embodiment is a square plate with dimensions of 117mm×117mm×10mm. The 8YSZ ceramic blank is intact and has no deformation or cracks.
[0040] Example 3 The method for preparing the yttrium oxide-stabilized zirconia ceramic preform in this embodiment includes the following steps: S1 is used to prepare water-based 5YSZ ceramic slurry. Using 5 mol% yttrium-stabilized zirconia (5YSZ) powder with a D50 of 200 nm as raw material, and an ammonium salt aqueous solution of isobutylene and maleic anhydride copolymer with a weight average molecular weight of 6000 as a water-based dispersant, with an ammonium salt aqueous solution concentration of 40 wt.%, a water-based 5YSZ ceramic slurry was prepared using an 8L stirred ball mill. The total volume of the grinding balls and the water-based 5YSZ ceramic slurry accounted for 65% of the total volume of the stirred ball mill. The volume ratio of the materials was 0.64:0.36. First, zirconia grinding balls with a diameter of 5 mm were added to the mixing tank of a stirred ball mill. Then, deionized water and ammonium salt of isobutylene and maleic anhydride copolymer were added and stirred evenly. Then, 5YSZ powder was gradually added. The stirring speed during the addition of 5YSZ powder was 40 rpm. The amount of ammonium salt of isobutylene and maleic anhydride copolymer added was 0.5% of the mass of 5YSZ powder. A water-based 5YSZ ceramic slurry with a volume solid content of 52% was prepared.
[0041] S2 Stirring Ball Mill The stirred ball mill was operated at a speed of 80 rpm. The viscosity of the water-based 5YSZ ceramic slurry was measured every 10 minutes using a rotational rheometer. The rotor was a flat plate. The viscosity of the water-based 5YSZ ceramic slurry showed a trend of first decreasing and then increasing. After 1.3 hours of stirred ball milling, the viscosity of the water-based 5YSZ ceramic slurry at a shear rate of 100 / s reached 0.98 Pa·s, and the ball milling was stopped.
[0042] S3 filtration and degassing The water-based 5YSZ ceramic slurry is discharged through the filter at the bottom of the stirred ball mill and subjected to vacuum treatment. The degassed water-based 5YSZ ceramic slurry is then poured into an aluminum alloy mold. A thin film is then placed on the upper surface of the mold to keep the water-based 5YSZ ceramic slurry in a sealed environment and allow it to cure in situ at room temperature of 23°C.
[0043] S4 drying After standing for 36 hours, the water-based 5YSZ ceramic slurry gelled. The film was removed, and the ambient temperature was controlled at 25℃ and the humidity at 85%RH for drying. After drying for 24 hours, the ambient humidity was reduced to 60%RH and then dried for another 48 hours. The weight of the green body no longer changed, and the drying was completed, obtaining the 5YSZ ceramic green body.
[0044] like Figure 3 As shown, the 5YSZ ceramic blank prepared in this embodiment is a square plate with dimensions of 116mm×116mm×10mm. The 5YSZ ceramic blank is intact and has no deformation or cracks.
[0045] Comparative Example 1 The difference from Example 1 is that in step S1, polyethylene glycol is used to replace ammonium polyacrylate in an equal amount.
[0046] The water-based 3YSZ ceramic slurry prepared in Comparative Example 1 failed to solidify in the aluminum alloy mold, resulting in a green body with sufficient strength. This is because polyethylene glycol does not contain carboxyl groups and cannot undergo a cross-linking reaction with yttrium ions on the surface of the 3YSZ powder, thus failing to produce a gel-curing effect. Figure 4 As shown, the 3YSZ ceramic green body prepared in Comparative Example 1 is a square plate with dimensions of 58mm×58mm×8mm, which cracked after drying.
[0047] Comparative Example 2 The difference from Example 1 is that in step S1, the amount of ammonium polyacrylate added is 1.5 wt.% of the mass of 3YSZ powder, and a water-based 3YSZ ceramic slurry with a volume solid content of 34% is prepared.
[0048] Based on this, it was found that the water-based 3YSZ ceramic slurry exhibited a slow curing rate during the curing process in step S3, only curing into a wet blank with a certain strength after 72 hours. For example... Figure 5 As shown, the 3YSZ ceramic green body prepared in Comparative Example 2 is a square plate with dimensions of 59mm×59mm×8mm. After drying at 25℃ and 85%RH for 12h in step S4, it cracked.
[0049] Comparative Example 3 The difference from Example 1 is that in step S4, after standing for 48 hours, the water-based 3YSZ ceramic slurry gels, the film is removed, and the ambient temperature is controlled at 25°C and the humidity at 50%RH for drying. After drying for 60 hours, the weight of the green body no longer changes, the drying is completed, and a 3YSZ ceramic green body is obtained.
[0050] like Figure 6 As shown, the 3YSZ ceramic green body prepared in Comparative Example 3 is a square plate with dimensions of 116mm×116mm×10mm. However, due to the low humidity at the beginning of drying, the moisture in the 3YSZ ceramic green body evaporated too quickly, resulting in cracks during the drying process.
[0051] Example 4 The method for preparing the yttrium oxide-stabilized zirconia-toughened alumina ceramic preform of this embodiment includes the following steps: S1 Preparation of Water-Based Ceramic Slurry Using a mixture of 3YSZ powder with D50=50nm and alumina powder with D50=0.45μm as raw materials, the alumina powder content in the mixture is 80wt.%. An aqueous solution of ammonium polyacrylate with a weight average molecular weight of 5500 and a concentration of 40wt.% was used as a water-based dispersant. An 8L stirred ball mill was used to prepare a water-based ceramic slurry. The total volume of the grinding balls and the water-based ceramic slurry accounted for 65% of the total volume of the stirred ball mill, and the volume ratio of the grinding balls to the water-based ceramic slurry was 0.64:0.36. First, zirconia grinding balls with a diameter of 5mm were added to the mixing tank of the stirred ball mill, followed by deionized water and ammonium polyacrylate. After stirring evenly, the mixed powder was gradually added. The stirring speed during the addition of the mixed powder was 40rpm, and the amount of ammonium polyacrylate added was 0.9% of the mass of the mixed powder. A water-based ceramic slurry with a volume solids content of 50% was prepared.
[0052] S2 Stirring Ball Mill The stirred ball mill was operated at a speed of 100 rpm. The viscosity of the water-based ceramic slurry was measured every 10 minutes using a rotational rheometer. The rotor was a flat plate. The viscosity of the water-based ceramic slurry showed a trend of first decreasing and then increasing. After 2.4 hours of stirred ball milling, the viscosity of the water-based ceramic slurry at a shear rate of 100 / s reached 0.94 Pa·s, and the ball milling was stopped.
[0053] S3 filtration and degassing The water-based ceramic slurry is discharged through the filter at the bottom of the stirred ball mill and subjected to vacuum degassing. The degassed water-based ceramic slurry is then poured into an aluminum alloy mold. A thin film is then placed on the upper surface of the mold to keep the water-based ceramic slurry in a sealed environment and allow it to solidify in situ at room temperature of 25°C.
[0054] S4 drying After standing for 36 hours, the water-based ceramic slurry gelled. The film was removed, and the ambient temperature was controlled at 25°C and the humidity at 85%RH for drying. After drying for 24 hours, the ambient humidity was reduced to 50%RH and then dried for another 48 hours. The weight of the green body no longer changed, and the drying was completed, obtaining a yttrium-stabilized zirconia-toughened alumina ceramic green body.
[0055] like Figure 7 As shown, the yttrium-stabilized zirconia toughened alumina ceramic blank prepared in this embodiment is a square plate with dimensions of 57.5mm × 57.5mm × 10mm. The ceramic blank is intact and has no deformation or cracks.
[0056] Example 5 The method for preparing the yttrium oxide-stabilized zirconia-toughened alumina ceramic preform of this embodiment includes the following steps: S1 Preparation of Water-Based Ceramic Slurry Using a mixture of 3YSZ powder with D50=50nm and alumina powder with D50=0.45μm as raw materials, the alumina powder content in the mixture is 60wt.%. A 40wt.% ammonium citrate aqueous solution is used as a water-based dispersant. An 8L stirred ball mill is used to prepare a water-based ceramic slurry. The total volume of the grinding balls and the water-based ceramic slurry accounts for 70% of the total volume of the stirred ball mill, and the volume ratio of the grinding balls to the water-based ceramic slurry is 0.6:0.4. First, zirconia grinding balls with a diameter of 5mm are added to the stirred tank of the stirred ball mill. Then, deionized water and ammonium citrate are added and stirred evenly. Then, the mixed powder is gradually added. The stirring speed is 40rpm during the addition of the mixed powder. The amount of ammonium citrate added is 2.3% of the mass of the mixed powder. A water-based ceramic slurry with a volume solids content of 48% is prepared.
[0057] S2 Stirring Ball Mill The stirred ball mill was operated at a speed of 150 rpm. The viscosity of the water-based ceramic slurry was measured every 10 minutes using a rotational rheometer. The rotor was a flat plate. The viscosity of the water-based ceramic slurry showed a trend of first decreasing and then increasing. After 2 hours of stirred ball milling, the viscosity of the water-based ceramic slurry reached 0.96 Pa·s at a shear rate of 100 / s, and the ball milling was stopped.
[0058] S3 filtration and degassing The water-based ceramic slurry is discharged through the filter at the bottom of the stirred ball mill and subjected to vacuum degassing. The degassed water-based ceramic slurry is then poured into an aluminum alloy mold. A thin film is placed on the upper surface of the mold to keep the water-based ceramic slurry in a sealed environment and allow it to solidify in situ at room temperature of 20°C.
[0059] S4 drying After standing for 24 hours, the water-based ceramic slurry gelled. The film was removed, and the ambient temperature was controlled at 25°C and the humidity at 85%RH for drying. After drying for 24 hours, the ambient humidity was reduced to 60%RH and dried for another 60 hours. The weight of the green body no longer changed, and the drying was completed, obtaining a yttrium-stabilized zirconia-toughened alumina ceramic green body.
[0060] like Figure 8 As shown, the yttrium oxide stabilized zirconia toughened alumina ceramic blank prepared in this embodiment is a square plate with dimensions of 119mm×119mm×10mm. The ceramic blank is intact and has no deformation or cracks.
[0061] Example 6 The method for preparing the yttrium oxide-stabilized zirconia-toughened alumina ceramic preform of this embodiment includes the following steps: S1 Preparation of Water-Based Ceramic Slurry A mixed powder of 3YSZ powder with D50=50nm and alumina powder with D50=0.45μm was used as raw material, with the alumina powder content in the mixed powder being 90wt.%. An ammonium salt aqueous solution of isobutylene-maleic anhydride copolymer with a weight average molecular weight of 6000 was used as a water-based dispersant, with the concentration of the isobutylene-maleic anhydride copolymer ammonium salt aqueous solution being 40wt.%. An 8L stirred ball mill was used to prepare the water-based ceramic slurry. The total volume of the grinding balls and the water-based ceramic slurry accounted for the total volume of the stirred ball mill. The volume ratio of grinding balls to water-based ceramic slurry was 0.7:0.3. First, zirconia grinding balls with a diameter of 5 mm were added to the mixing tank of a stirred ball mill. Then, deionized water and ammonium salt of isobutylene-maleic anhydride copolymer were added and stirred evenly. Then, the mixed powder was gradually added. The stirring speed during the addition of the mixed powder was 40 rpm. The amount of ammonium salt of isobutylene-maleic anhydride copolymer added was 0.7% of the mass of the mixed powder. A water-based ceramic slurry with a volume solid content of 51% was prepared.
[0062] S2 Stirring Ball Mill The stirred ball mill was operated at a speed of 80 rpm. The viscosity of the water-based ceramic slurry was measured every 10 minutes using a rotational rheometer. The rotor was a flat plate. The viscosity of the water-based ceramic slurry showed a trend of first decreasing and then increasing. After 3 hours of stirred ball milling, the viscosity of the water-based ceramic slurry reached 0.92 Pa·s at a shear rate of 100 / s, and the ball milling was stopped.
[0063] S3 filtration and degassing The water-based ceramic slurry is discharged through the filter at the bottom of the stirred ball mill and subjected to vacuum degassing. The degassed water-based ceramic slurry is then poured into an aluminum alloy mold. A thin film is then placed on the upper surface of the mold to keep the water-based ceramic slurry in a sealed environment and allow it to solidify in situ at room temperature of 25°C.
[0064] S4 drying After standing for 48 hours, the water-based ceramic slurry gelled. The film was removed, and the ambient temperature was controlled at 25°C and the humidity at 85%RH for drying. After drying for 24 hours, the ambient humidity was reduced to 40%RH and then dried for another 36 hours. The weight of the green body no longer changed, and the drying was completed, obtaining a yttrium-stabilized zirconia-toughened alumina ceramic green body.
[0065] like Figure 9 As shown, the yttrium-stabilized zirconia toughened alumina ceramic blank prepared in this embodiment is a square plate with dimensions of 108mm×86mm×10mm. The ceramic blank is intact and has no deformation or cracks.
[0066] Comparative Example 4 The difference from Example 4 is that in step S1, polyethylene glycol is used to replace ammonium polyacrylate in an equal amount.
[0067] The water-based ceramic slurry prepared in Comparative Example 4 did not solidify in the aluminum alloy mold, failing to yield a green body with sufficient strength. This is because polyethylene glycol does not contain carboxylate groups and cannot undergo a cross-linking reaction with yttrium ions on the surface of 3YSZ powder, thus preventing the gel-curing effect. Figure 10 As shown, the ceramic blank prepared in Comparative Example 4 is a square plate with dimensions of 145 mm × 145 mm × 10 mm, and there is some peeling on the surface after drying.
[0068] Comparative Example 5 The difference from Example 4 is that in step S1, the amount of ammonium polyacrylate added is 0.5 wt.% of the mass of the mixed powder, and a water-based ceramic slurry with a volume solid content of 35% is prepared.
[0069] Based on this, it was found that the water-based ceramic slurry cured slowly during the curing process in step S3, taking 80 hours to solidify into a wet blank with a certain strength. For example... Figure 11 As shown, the ceramic blank prepared in Comparative Example 5 is a square plate with dimensions of 117mm×117mm×10mm. After drying at 25℃ and 85%RH for 12 hours in step S4, it cracked.
[0070] Comparative Example 6 The difference from Example 4 is that in step S4, after standing for 36 hours, the water-based ceramic slurry gels, the film is removed, the ambient temperature is controlled at 25°C and the humidity at 50%RH, and drying is carried out. After drying for 55 hours, the weight of the green body no longer changes, the drying is completed, and a yttrium-stabilized zirconia toughened alumina ceramic green body is obtained.
[0071] like Figure 12As shown, the ceramic blank prepared in Comparative Example 6 is a square plate with dimensions of 115mm×115mm×10mm. However, due to the low humidity at the beginning of drying, the moisture in the ceramic blank evaporates too quickly, resulting in cracks during the drying process.
Claims
1. A method for preparing a yttria-stabilized zirconia ceramic body, characterized in that: The following steps are involved: S1 uses yttria-stabilized zirconia powder as raw material, adds a carboxylate-containing water-based dispersant, and prepares a water-based ceramic slurry with a volume solid content of more than 40% by stirring ball milling; S2 measures the rheological properties of the water-based ceramic slurry during the stirring ball milling process. When 0.9 Pa·s < the viscosity of the water-based ceramic slurry at a shear rate of 100 / s < 1 Pa·s, the ball milling is stopped; S3: filtering and degassing the water-based ceramic slurry to remove the grinding balls and air therein, and then injecting it into the mold and sealing it at room temperature; After S4 is placed for 24-48 hours, the water-based ceramic slurry is transformed from a fluid into an elastomer, and then the yttria-stabilized zirconia ceramic body is obtained by temperature-controlled and humidity-controlled drying.
2. The method for preparing the yttria-stabilized zirconia ceramic body according to claim 1, characterized in that: In step S1, the carboxylate-containing water-based dispersant is an aqueous solution of ammonium salt of a copolymer of isobutylene and maleic anhydride, an aqueous solution of ammonium citrate, or an aqueous solution of ammonium polyacrylate.
3. The method for preparing the yttria-stabilized zirconia ceramic body according to claim 1, characterized in that: In the yttria-stabilized zirconia powder, the molar percentage of yttria is 3-8%; and the median diameter of the yttria-stabilized zirconia powder is 50-500nm.
4. The method for preparing a yttria-stabilized zirconia ceramic body according to claim 1, wherein: In step S1, the amount of the carboxylate-containing water-based dispersant added is 0.3-3% of the mass of the yttria-stabilized zirconia powder.
5. The method for preparing the yttria-stabilized zirconia ceramic body according to claim 1, characterized in that: In step S1, a water-based ceramic slurry is prepared using a stirring ball mill. Zirconia grinding balls with a diameter of 5 mm are used in the stirring ball mill. The volume ratio of the grinding balls to the water-based ceramic slurry is (0.6-0.7): (0.3-0.4). The total volume of the water-based ceramic slurry and the grinding balls accounts for 60-70% of the total volume of the stirring ball mill.
6. The method for preparing the yttria-stabilized zirconia ceramic body according to claim 5, characterized in that: In step S2, during the stirring ball milling, the rotation speed of the stirring ball mill is 80-150 rpm.
7. The method for preparing a yttria-stabilized zirconia ceramic body according to claim 1, characterized in that: In step S2, during the stirring ball milling process, the viscosity of the water-based ceramic slurry is measured every 10 minutes using a rotational rheometer, and the rotor is a flat plate.
8. The method for preparing the yttria-stabilized zirconia ceramic body according to claim 1, characterized in that: In step S3, the temperature is 20-25°C under room temperature conditions.
9. The method for preparing a yttria-stabilized zirconia ceramic body according to claim 1, characterized in that: In step S4, the temperature and humidity controlled drying process is as follows: the temperature is controlled at 25°C, and in the initial stage of drying, the ambient humidity is controlled at above 80%RH. After 24 hours, the humidity is reduced to 40-60%RH, and the weight of the green body is weighed at the same time. When the weight of the green body no longer decreases, the drying is stopped to complete the preparation of the yttria-stabilized zirconia ceramic green body.
10. A method for preparing a yttria-stabilized zirconia-toughened alumina ceramic body, characterized in that: In the method for preparing a yttria-stabilized zirconia ceramic body according to any one of claims 1 to 9, the yttria-stabilized zirconia powder in step S1 is replaced with a mixed powder of yttria-stabilized zirconia and alumina, and the amount of alumina added to the mixed powder is 60-90wt.%.
Citation Information
Patent Citations
Method for preparing ceramic body
CN103130509A
Preparation method of high-density ceramic biscuit
CN115246158A
Forming method of ceramic green body
CN115448704A
Binder coagulation casting
US5900201A
Cited By
Preparation method of submillimeter zirconia microspheres
CN120365058A
Preparation method of sub-millimeter zirconia microbeads
CN120365058B