Anti-ablation complex-phase high-entropy ceramic coating and preparation method thereof
By introducing complex phase high-entropy carbides and high-entropy boronides into high-temperature ceramic coatings, forming a composite coating with a rock salt-shaped face-centered cubic and hexagonal crystal structure, the existing ceramic coatings in high-temperature ablation environment is solved. The brittleness and inhomogeneity problems achieve efficient anti-oxidation, ablation and thermal shock resistance, and are suitable for thermal protection of solid rocket engines and hypersonic aircraft.
Patent Information
- Application Number
- CN202410949977.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-29
AI Technical Summary
The existing ultra-high temperature ceramic coatings have high brittleness, small damage resistance, poor thermal shock resistance and uneven preparation problems in high-temperature ablation environment, and cannot effectively resist high-temperature ablation of 3000℃, limiting their solids. Application of hot-end components of rocket engines and hypersonic aircraft.
Develop a complex phase high entropy ceramic coating, including high entropy carbide (TiZrHfTaMx) C and high entropy boronide (TiZrHfTaNy) B2, spraying on the substrate through a dual-beam plasma thermal spraying process, optimizing high entropy carbide and high entropy The proportional configuration of the boride forms a composite coating with a rock salt-shaped face-centered cubic structure and a hexagonal crystal system structure.
The composite phase high entropy ceramic coating has excellent oxidation resistance at 1600°C, and exhibits good ablation resistance at 3000°C. The linear ablation rate is 3 to 4 μm/s, the binding force reaches 31 to 32MPa, and It can maintain thermal shock resistance of more than 10 times in the oxyacetylene combined with air-cooled repeated ablation test.
Smart Images

Figure CN119039016A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ablation-resistant ceramic coatings and relates to a 3000°C ablation-resistant composite high-entropy ceramic coating and a preparation method thereof. Background Art
[0002] During the service life of solid rocket engines and hypersonic vehicles, their hot end components are usually subject to high temperature ablation. With the increasing requirements for the performance of solid rocket engines and the Mach number of hypersonic vehicles, their hot end components are subject to ablation of heat flux up to 3000℃. Existing matrix materials such as C / C composite materials and graphite will suffer from severe ablation and cannot meet application requirements.
[0003] Ultra-High Temperature Ceramics refers to a class of ceramic materials that can maintain physical and chemical stability in high temperature environments (3000℃) and reaction atmospheres. It has high thermal conductivity, moderate thermal expansion coefficient and good anti-oxidation and ablation performance. It is a very promising non-ablative ultra-high temperature thermal protection material. However, the traditional ultra-high temperature ceramics have the problems of high brittleness, low damage tolerance, poor thermal shock resistance and inhomogeneity that is difficult to solve during the preparation process, which limits its application as a bulk material. Therefore, related research mainly focuses on the anti-ablation performance of ultra-high temperature ceramic coatings.
[0004] Ultra-high temperature ceramics are mainly multi-component composite ceramic materials composed of transition metal compounds such as hafnium, zirconium, and molybdenum. They have the characteristics of ultra-high temperature resistance, high thermal conductivity, and high strength. They have potential applications in the material composition of heat-bearing structural components such as the nose cone and wing leading edge of reusable spacecraft. Its multi-principal element design concept breaks away from the constraints of the inherent properties of the main elements and realizes "free" design and combination at the atomic level, which helps to obtain ultra-high temperature ceramic coatings with low thermal conductivity and a thermal expansion coefficient close to that of C / C composite materials. The obtained ultra-high temperature ceramic coatings have excellent thermal shock resistance.
[0005] Existing research on ultra-high temperature ceramic coatings usually requires mixing multiple ceramic components or making multi-layer ceramic coatings to meet the comprehensive performance of anti-oxidation, ablation, thermal shock, etc. required during service. These requirements for comprehensive performance in many aspects make the design, preparation and reliability of ultra-high temperature ceramic coatings face great challenges. In the real service environment of high temperature, low pressure and atomic oxygen atmosphere of aircraft, on the one hand, the oxidation of ultra-high temperature ceramic-based composite materials restricts its application as a thermal structure in the aircraft thermal protection system; on the other hand, the difference in thermal expansion properties of ultra-high temperature ceramics and their adjacent materials will cause contact stress. When the predicted thermal stress reaches the maximum allowable stress of the material, thermal shock damage behavior may occur. The existence of thermal stress limits the size and shape of ultra-high temperature ceramics; in addition, ultra-high temperature ceramic materials are prone to structural damage during the ablation process due to their own brittleness, small damage tolerance, poor thermal shock resistance and inhomogeneity that is difficult to solve during the preparation process.
[0006] In view of the above reasons, it is urgent to study a ceramic coating with excellent anti-ablation performance. Summary of the invention
[0007] In order to overcome the above problems, the inventors have conducted intensive research and developed an anti-ablation multiphase high entropy ceramic coating and a preparation method thereof. The coating comprises high entropy carbide and high entropy boride. The expression of the high entropy carbide is: (TiZrHfTaM x )C, the expression of the high entropy boride is: (TiZrHfTaN y )B2, M, N are each independently W, V, Nb or Mo, x, y are each independently 0 or 1, and the multiphase high entropy ceramic coating has the advantages of anti-oxidation, anti-ablation, and high thermal matching with the substrate, thereby completing the present invention.
[0008] Specifically, the purpose of the present invention is to provide the following aspects:
[0009] On the one hand, a multiphase high entropy ceramic coating is provided, wherein the coating comprises a high entropy carbide and a high entropy boride, wherein the high entropy carbide is expressed as: (TiZrHfTaM x )C, the expression of the high entropy boride is: (TiZrHfTaNy)B2, M, N are each independently W, V, Nb or Mo, x, y are each independently 0 or 1.
[0010] The high entropy carbide in the composite high entropy ceramic coating has a rock salt face-centered cubic structure, and the high entropy boride has a hexagonal crystal structure.
[0011] Wherein, based on the mass of the composite high entropy ceramic coating, the content of the high entropy carbide is 10 to 90 wt.%.
[0012] Wherein, the multiphase high entropy ceramic coating is 4MW / m 2 The heat flux density of oxyacetylene flame was ablated for 240s, and the linear ablation rate was 3-4μm / s.
[0013] In another aspect, a method for preparing the coating according to the first aspect is provided, the method comprising:
[0014] Step 1, preparing high entropy carbide and high entropy boride respectively;
[0015] Step 2: spraying the high entropy carbide and the high entropy boride on the substrate simultaneously to obtain the multiphase high entropy ceramic coating.
[0016] Wherein, in step 1, the expression of the high entropy carbide is: (TiZrHfTaM x )C, M is W, V, Nb or Mo, and x is 0 or 1.
[0017] Wherein, in step 1, the expression of the high entropy boride is: (TiZrHfTaN y )B2, N is W, V, Nb or Mo, and y is 0 or 1.
[0018] The beneficial effects of the present invention include:
[0019] (1) The multiphase high entropy ceramic coating provided by the present invention has excellent high-temperature oxidation resistance, and its average oxidation rate at 1600 degrees Celsius is 0.04-0.08 g·cm -2 ·h -1 .
[0020] (2) The multiphase high entropy ceramic coating provided by the present invention has excellent ablation resistance. -2 After 200s of flame ablation with a heat flux density, the linear ablation rate is 3-4μm / s.
[0021] (3) The bonding strength between the composite high entropy ceramic coating provided by the present invention and the substrate can reach 31 to 32 MPa.
[0022] (4) The multiphase high entropy ceramic coating provided by the present invention has excellent thermal shock resistance. Its thermal shock resistance is tested by repeated ablation using oxyacetylene combined with air cooling, with ablation for 10 seconds and air cooling for 10 seconds. The number of thermal shock resistance is not less than 10 times.
[0023] (5) The preparation method of the multiphase high entropy ceramic coating provided by the present invention adopts a dual-beam plasma thermal spraying process to achieve a proportional configuration of high entropy carbide and high entropy boride powders, thereby obtaining an antioxidant ablation coating for different application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] By reading the detailed description of the preferred specific embodiments below, various other advantages and benefits of the present invention will become clear to those of ordinary skill in the art. The drawings in the specification are only used for the purpose of illustrating the preferred embodiments and are not considered to be limitations of the present invention. Obviously, the drawings described below are only some embodiments of the present invention. For those of ordinary skill in the art, other drawings can also be obtained based on these drawings without creative work.
[0025] In the attached picture:
[0026] FIG1( a ) shows a SEM image of the high entropy carbide in Example 1;
[0027] FIG1( b ) shows the X-ray diffraction pattern of the high entropy carbide in Example 1;
[0028] FIG2( a ) shows a SEM image of the high entropy boride in Example 1;
[0029] FIG2( b ) shows the X-ray diffraction pattern of the high entropy boride in Example 1;
[0030] FIG3( a ) shows a macroscopic optical image of the multiphase high entropy ceramic coating prepared in Example 1;
[0031] FIG3( b ) shows a SEM image of the multiphase high entropy ceramic coating prepared in Example 1;
[0032] Figure 4 A macroscopic optical photograph of the multiphase high entropy ceramic coating prepared in Example 1 after ablation is shown;
[0033] FIG5( a ) shows a SEM image of the composite high entropy ceramic coating obtained in Example 1 after ablation;
[0034] FIG5( b ) shows the microscopic morphology of the central area of FIG5( a );
[0035] Figure 6 The scanning morphology of the coating ablation area in Example 1 is shown;
[0036] Figure 7 Show Figure 6 EDS spectrum at the yellow cross mark;
[0037] Figure 8 A schematic diagram showing a gradient change of high entropy carbides and high entropy borides in a coating according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0038] The following will refer to the attached Figure 1(a) to Figure 8Specific embodiments of the present invention are described in more detail. Although specific embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.
[0039] It should be noted that certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that technicians may use different nouns to refer to the same component. This specification and claims do not use the difference in nouns as a way to distinguish components, but use the difference in the functions of the components as the criterion for distinction. As mentioned throughout the specification and claims, "including" or "comprising" is an open term, so it should be interpreted as "including but not limited to". The subsequent description of the specification is a preferred embodiment of the present invention, but the description is based on the general principles of the specification and is not intended to limit the scope of the present invention. The scope of protection of the present invention shall be determined by the attached claims.
[0040] In the description of the present invention, it should be noted that the terms "upper", "lower", "inner", "outer", "front", "rear", etc. indicate positions or positional relationships based on the working state of the present invention, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third", and "fourth" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.
[0041] To facilitate understanding of the embodiments of the present invention, further explanation will be given below by taking specific embodiments as examples in conjunction with the accompanying drawings, and each of the accompanying drawings does not constitute a limitation on the embodiments of the present invention.
[0042] On the one hand, according to a multiphase high entropy ceramic coating provided by the present invention, the coating comprises a high entropy carbide and a high entropy boride, and the expression of the high entropy carbide is: (TiZrHfTaM x )C, the expression of the high entropy boride is: (TiZrHfTaN y )B2, M and N are each independently W, V, Nb or Mo, and x and y are each independently 0 or 1.
[0043] According to the present invention, the high entropy carbide in the multiphase high entropy ceramic coating has a rock salt face-centered cubic structure, and the high entropy boride has a hexagonal crystal structure.
[0044] Furthermore, the content of high entropy boride in the composite high entropy ceramic coating is selected according to the environment in which the coating is used. The higher the content of high entropy boride, the stronger the coating's resistance to ablation in an oxygen-rich environment. Preferably, based on the mass of the composite high entropy ceramic coating, the content of high entropy carbide is 10 to 90 wt.%.
[0045] According to the present invention, the thickness of the multiphase high entropy ceramic coating is 150-185 μm, the hardness is 55-58 GPa, the bonding force between the multiphase high entropy ceramic coating and the substrate is 31-32 Mpa, and the bonding force between the multiphase high entropy ceramic coating and the substrate is 4 MW / m 2 The linear ablation rate of the oxyacetylene flame with a heat flux of 240s is 3-4μm / s, and the average oxidation rate at 1600℃ is 0.04-0.08g·cm -2 ·h -1 .
[0046] On the other hand, a method for preparing the multiphase high entropy ceramic coating according to the first aspect is provided, the method comprising:
[0047] Step 1, preparing high entropy carbide and high entropy boride respectively;
[0048] Step 2: spraying the high entropy carbide and the high entropy boride on the substrate simultaneously to obtain the multiphase high entropy ceramic coating.
[0049] Specifically:
[0050] Step 1, prepare high entropy carbides and high entropy borides respectively.
[0051] In step 1, the expression of the high entropy carbide is: (TiZrHfTaM x )C, M is W, V, Nb or Mo, and x is 0 or 1.
[0052] Furthermore, the high entropy carbide is prepared by using Ti source, Zr source, Hf source and Ta source as raw materials, optionally adding W source, V source, Nb source or Mo source, mixing the raw materials, and subjecting the raw materials to high temperature solid solution ablation or carbon thermal reduction.
[0053] When preparing high entropy carbides, a high temperature solid solution ablation preparation method is used as an example, in which the Ti source, Zr source, Hf source and Ta source are TiC powder, ZrC powder, HfC powder and TaC powder respectively, and the optional W source, V source, Nb source or Mo source are WC powder, VC powder, NbC powder or MoC powder respectively. After mixing the metal carbides, they are ball milled and sintered in sequence to obtain high entropy carbides.
[0054] The amounts of the metal carbide raw materials are in an equimolar ratio.
[0055] Among them, the selection of ball milling parameters is closely related to the ball milling efficiency.
[0056] According to the present invention, the ball milling rate is 300-500 r / min, preferably 350-450 r / min, for example 400 r / min. As the ball milling rate increases, the ball milling efficiency will naturally increase, but if the ball milling rate is too high, the collision and extrusion effect between the ball milling balls and the ball milling materials will be weakened. Within the above parameter range, the ball milling rate is appropriate.
[0057] According to the present invention, the ball milling time is 3 to 10 hours, preferably 5 to 7 hours, for example 6 hours. As the ball milling time increases, more energy is generated during the ball milling; if the ball milling time is too long, the ball milled material will agglomerate, greatly affecting the performance of the material. The ball milling efficiency is better within the above range of ball milling time.
[0058] According to the present invention, the ball-to-material ratio used in ball milling is (3-8):1, preferably (4-6):1, for example 5:1. The increase of ball milling balls will promote the collision of ball milling materials, improve the energy conversion efficiency of ball milling materials, and effectively shorten the ball milling time; however, when the ball milling ball loading is too large, the ball milling materials cannot be effectively crushed due to the limited space in the ball mill tank.
[0059] According to the present invention, before sintering, the vacuum needs to be evacuated to below 6 Pa, which is beneficial to prevent oxidation during the sintering process.
[0060] Furthermore, inert gas such as nitrogen, argon, etc. is used as protective gas during the sintering process.
[0061] According to the present invention, the sintering temperature is 1500-2500°C, preferably 1600-2200°C, and most preferably 2000°C.
[0062] Among them, when the sintering temperature is 1500-2500, the obtained high entropy carbide has a better solid solubility, especially when the sintering temperature is 2000℃, the obtained high entropy carbide powder is a single solid solution structure, and this sintering temperature is not too high, the requirements for equipment are low, and the energy consumption of the preparation process is also low.
[0063] Furthermore, the sintering time is 1 to 10 hours, preferably 2 to 8 hours, and most preferably 6 hours.
[0064] Among them, as the sintering time increases, the solid solution reaction becomes more complete, but too long a time will not have a significant effect on the degree of solid solution reaction, but will increase energy consumption.
[0065] Preferably, after sintering, the obtained sintered product is ball-milled for a second time and then sieved to obtain the desired high entropy carbide.
[0066] The secondary milling efficiency will naturally increase with the increase of the secondary milling rate, but too high a secondary milling rate will weaken the collision and extrusion effect between the milling balls and the milled materials. The secondary milling rate is 300-500 r / min, preferably 350-450 r / min, for example 400 r / min.
[0067] According to the present invention, the secondary ball milling time does not need to be too long, as long as agglomeration does not occur and the performance is guaranteed. The secondary ball milling time is 0.5 to 3 hours, preferably 1 to 2 hours, for example 2 hours.
[0068] According to the present invention, the ball milling balls promote the collision of the ball milling materials, but when the ball milling balls are loaded too much, the ball milling materials cannot be effectively crushed due to the limited space in the ball milling tank. The ball milling material ratio used in the secondary ball milling is (3-8):1, preferably (4-6):1, for example 5:1.
[0069] According to the present invention, after the secondary ball milling, the product is sieved through a 150-220 mesh sieve, such as a 200 mesh sieve, to ensure uniformity.
[0070] According to a preferred embodiment, the X-ray diffraction of the prepared high entropy carbide is shown in FIG. 1( b ), and it can be seen that it is a single rock salt type face-centered cubic structure.
[0071] When preparing high entropy carbide, taking the carbon thermal reduction method as an example, the Ti source, Zr source, Hf source and Ta source are TiO2 powder, ZrO2 powder, HfO2 powder and Ta2O5 powder respectively, and the optional W source, V source, Nb source or Mo source are WO3 powder, V2O5 powder, Nb2O5 powder or MoO2 powder respectively. The metal oxides are mixed with carbon powder, and the high entropy carbide is obtained by grinding and calcining in sequence.
[0072] According to the present invention, the amount of metal elements in each metal oxide is an equimolar ratio; the molar ratio between the total molar amount of metal in each metal oxide and the molar amount of carbon powder is 1:2.5-6, preferably 1:3-4, for example 1:3.2. Excessive carbon powder can ensure that the metal oxide is fully carbonized and reduced to form metal carbides, which are further dissolved into high entropy carbides; but there is no need for too much carbon powder, so as to avoid excessive carbon remaining in the final product and affecting the purity of the obtained high entropy carbide powder.
[0073] According to the present invention, when high entropy carbide is prepared using metal oxide and carbon powder as raw materials, the grinding rate is 300-500 r / min, preferably 400-480 r / min, for example 450 r / min; the grinding time is 3-10 h, preferably 4-6 h, for example 5 h; the ball-to-material ratio used in grinding is (3-8):1, preferably (4-6):1, for example 5:1.
[0074] According to the present invention, before calcination, the vacuum needs to be evacuated to below 6 Pa to avoid the reaction of the raw materials and their reaction products with oxygen and nitrogen in the air at high temperature to produce impurities, which is conducive to obtaining high-entropy carbides with higher purity.
[0075] Furthermore, an inert gas such as nitrogen, argon, etc. is used as a protective gas during the calcination process.
[0076] According to the present invention, the calcination temperature is 1200-2200° C., preferably 1600-2000° C., and most preferably 1800° C. The high entropy carbide obtained at this temperature has good solid solubility, and the powder has a single solid solution structure. At the same time, the temperature is not too high, the requirements for equipment are low, and the energy consumption of the preparation process is also low.
[0077] Furthermore, the calcination time is 1 to 10 hours, preferably 2 to 8 hours, and most preferably 5 hours. Within this sintering time, sufficient carbothermal reduction reaction and solid solution sintering can be taken into account, and the energy consumption of the preparation process is low.
[0078] Preferably, after calcination, the calcined product is ground twice, and then passed through a 150-220 mesh, such as a 200 mesh, sieve to obtain the desired high entropy carbide. The secondary grinding rate is 300-500 r / min, preferably 400-480 r / min, such as 450 r / min; the secondary grinding time is 0.5-3 h, preferably 1-2 h, such as 2 h; the ball-to-material ratio used in the secondary grinding is (3-8):1, preferably (4-6):1, such as 5:1.
[0079] In step 1, the expression of the high entropy boride is: (TiZrHfTaN y )B2, N is W, V, Nb or Mo, and y is 0 or 1.
[0080] Furthermore, the high entropy boride is prepared by using Ti source, Zr source, Hf source and Ta source as raw materials, optionally adding W source, V source, Nb source or Mo source, mixing the raw materials, and subjecting the raw materials to high temperature solid solution ablation or carbon thermal reduction.
[0081] When preparing high entropy borides, a high temperature solid solution ablation preparation method is used as an example, in which the Ti source, Zr source, Hf source and Ta source are TiB2 powder, ZrB2 powder, HfB2 powder and TaB2 powder respectively, and the optional W source, V source, Nb source or Mo source are WB4, VB2, NbB2 or MoB5 respectively. After mixing the metal borides, they are successively ball milled and sintered to obtain high entropy borides.
[0082] The usage of each metal boride raw material is in an equimolar ratio.
[0083] According to the present invention, the ball milling process parameters for preparing high entropy boride using metal boride as raw material are preferably consistent with the ball milling process parameters for preparing high entropy carbide using metal carbide as raw material. The ball milling rate is 300-500r / min, preferably 350-450r / min, for example 400r / min; the ball milling time is 3-10h, preferably 5-7h, for example 6h; the ball-to-material ratio used in the ball milling is (3-8):1, preferably (4-6):1, for example 5:1.
[0084] Furthermore, before sintering, the vacuum needs to be evacuated to below 6Pa; during the sintering process, an inert gas such as nitrogen, argon, etc. is used as a protective gas; the sintering temperature is 1600-2400°C, preferably 1800-2000°C, and most preferably 2000°C; the sintering time is 1-10h, preferably 2-8h, and most preferably 6h.
[0085] Preferably, after sintering, the obtained sintered product is ball-milled for a second time and then sieved to obtain the desired high entropy boride.
[0086] Furthermore, the secondary ball milling process parameters for preparing high entropy boride using metal boride as raw material are preferably consistent with the secondary ball milling process parameters for preparing high entropy carbide using metal carbide as raw material, and after secondary ball milling, the material is sieved through a 150-220 mesh sieve, such as a 200 mesh sieve. The secondary ball milling rate is 300-500 r / min, preferably 350-450 r / min, such as 400 r / min; the secondary ball milling time is 0.5-3 h, preferably 1-2 h, such as 2 h; the ball-to-material ratio used in the secondary ball milling is (3-8):1, preferably (4-6):1, such as 5:1.
[0087] According to a preferred embodiment, the X-ray diffraction of the prepared high entropy boride is shown in FIG. 2( b ), from which it can be seen that it has a single hexagonal crystal structure.
[0088] When preparing high entropy boride, taking carbothermal reduction as an example, the Ti source, Zr source, Hf source and Ta source are TiO2 powder, ZrO2 powder, HfO2 powder and Ta2O5 powder respectively, and the optional W source, V source, Nb source or Mo source are WO3 powder, V2O5 powder, Nb2O5 powder or MoO2 powder respectively. The metal oxides, boron trioxide powder and carbon powder are mixed, ground and calcined in sequence to obtain high entropy carbide.
[0089] According to the present invention, the amount of metal elements in each metal oxide is an equimolar ratio; the molar ratio between the total molar amount of metal in each metal oxide, the molar amount of boron trioxide powder and the molar amount of carbon powder is 1: (1-1.2): (5-8), preferably 1: 1: 6. Under this condition, it can be ensured that the metal oxide is fully boron-thermally reduced to form a metal boride, which is further dissolved into a high-entropy boride, and it can be avoided that excess carbon remains in the final product, affecting the purity of the obtained high-entropy boride powder.
[0090] According to the present invention, the grinding process parameters for preparing high entropy boride using metal oxide, boron trioxide powder and carbon powder as raw materials are preferably consistent with the grinding process parameters for preparing high entropy boride using metal boride as raw materials. The grinding rate is 300-500r / min, preferably 400-480r / min, such as 450r / min; the grinding time is 3-10h, preferably 4-6h, such as 5h; the ball-to-material ratio used in grinding is (3-8):1, preferably (4-6):1, such as 5:1.
[0091] Furthermore, before calcination, the vacuum needs to be evacuated to below 6 Pa; during the calcination process, an inert gas such as nitrogen, argon, etc. is used as a protective gas; the calcination temperature is 1800-2400°C, preferably 1900-2100°C, and most preferably 1900°C; the sintering time is 1-10h, preferably 2-8h, and most preferably 4.5h.
[0092] Preferably, after calcination, the calcined product is ground twice and then passed through a 150-220 mesh, such as a 200 mesh, sieve to obtain the desired high entropy boride.
[0093] Further, the secondary grinding process parameters for preparing high entropy borides using metal oxides, boron trioxide powder and carbon powder as raw materials are preferably consistent with the secondary grinding process parameters for preparing high entropy borides using metal borides as raw materials, and after secondary grinding, the borides are sieved through a 150-220 mesh sieve, such as a 200 mesh sieve. The secondary grinding rate is 300-500 r / min, preferably 400-480 r / min, such as 450 r / min; the secondary grinding time is 0.5-3 h, preferably 1-2 h, such as 2 h; the ball-to-material ratio used in the secondary grinding is (3-8):1, preferably (4-6):1, such as 5:1.
[0094] In step 1, the metal elements in the high entropy carbides and high entropy borides selected for preparing the composite high entropy ceramic coating need to have a high melting point, and the metal carbides, metal borides, and metal oxides have the same crystal form and compatibility and can be dissolved into a single solid solution structure.
[0095] In step 1, the high entropy carbides and high entropy borides in the composite high entropy ceramic coating contain four metal elements, namely Ti, Zr, Hf and Ta. The melting points of the metal carbides (TiC, ZrC, HfC and TaC) and metal borides (TiB2, ZrB2, HfB2 and TaB2) of these elements are extremely high, and they can effectively resist the mechanical erosion of the high-temperature flame flow during the high-temperature ablation process. In addition, the melting points of the metal oxides of the four metal elements Ti, Zr, Hf and Ta are also relatively high, which can ensure that the coating still has good resistance to high-temperature flame flow erosion after being oxidized during the high-temperature ablation process. At the same time, the four metal oxides are relatively dense, and the oxide layer generated by them can alleviate the further oxidation of the coating, effectively improving the anti-oxidation and ablation performance of the coating.
[0096] Among them, W, V, Nb or Mo have good compatibility with Ti, Zr, Hf and Ta, and can form corresponding high-entropy carbides or high-entropy borides.
[0097] Furthermore, the addition of W, V, and Mo can cause the coating to oxidize in a high-temperature oxidation environment to generate WO3, V2O5, and MoO2, which are easily volatilized at high temperatures and have two beneficial effects: first, it cools the coating surface; second, it prevents the coating from increasing internal stress and cracking due to oxidation volume expansion, which in turn leads to oxidation and ablation of the coating. The addition of Nb and Mo, while ensuring the high melting point and excellent high-temperature strength of the composite high-entropy ceramic coating, has the following beneficial effects on the coating: first, it reduces the density of the coating, which is conducive to lightweight; second, it improves the plasticity and mechanical strength of the composite high-entropy ceramic coating.
[0098] In the present invention, the multiphase high entropy ceramic coating is a composite coating of high entropy carbide and high entropy boride, which takes into account the advantages of both high entropy carbide and high entropy boride, and makes up for the shortcomings of both. High entropy carbide has a high melting point and high high temperature strength, and has excellent high temperature ablation resistance, but it is severely oxidized at high temperature, especially in an oxygen-rich environment, and ablation damage is very fast. High entropy boride also has the advantages of high melting point and high high temperature strength, and has excellent ablation resistance. It is easy to oxidize to form dense glassy boron oxide in a high temperature oxidation environment, providing a certain antioxidant effect, but boron oxide will volatilize rapidly after exceeding 1100°C and lose its protective effect. By compounding high entropy carbide with high entropy boride, the internal distribution of high entropy boride in the coating can be utilized. The boron oxide generated by high temperature oxidation has excellent antioxidant properties, which hinders the internal diffusion of oxygen. At the same time, the internal boron oxide lacks a volatilization path at high temperature and can maintain this antioxidant property. Therefore, the composite coating has excellent resistance to ultra-high temperature oxygen-rich ablation.
[0099] In step 1, high entropy carbides and high entropy borides are prepared by carbon thermal reduction of metal oxides, and the raw materials for their preparation are relatively cheap and the preparation temperature is relatively low, which is suitable for industrialization; high entropy carbides and high entropy borides are prepared by metal carbides and metal borides, respectively, and the obtained high entropy carbides and high entropy borides have high purity and simple raw materials, but the cost of metal carbides is relatively high. In practice, different raw materials can be selected according to needs.
[0100] Step 2: spraying the high entropy carbide and the high entropy boride on the substrate simultaneously to obtain the multiphase high entropy ceramic coating.
[0101] In step 2, the substrate may be graphite, C / C composite material, tungsten-copper infiltrated, high-temperature alloy, etc., for example, C / C composite material.
[0102] In step 2, before spraying, the substrate is pretreated in advance, and the pretreatment includes roughening and degreasing. The roughening is performed by sandblasting, and preferably white corundum with a particle size of 30 to 120 mesh is used for sandblasting. For example, white corundum with a particle size of 3 mesh is used for sandblasting to obtain a substrate with a surface roughness of Ra3.0 to Ra6.0, such as Ra5.0; acetone or alcohol is used for ultrasonic cleaning for degreasing.
[0103] In step 2, the spraying adopts plasma thermal spraying, which has the advantages of strong bonding force, high preparation efficiency, application on workpieces of different sizes and shapes, wide range of sprayable materials, high coating quality, no through cracks, large and controllable coating thickness, easy engineering and low cost.
[0104] In step 2, high entropy carbide and high entropy boride are sprayed simultaneously, for example, high entropy carbide and high entropy boride are respectively placed in two powder feeders of a dual-beam plasma spraying system for spraying, and the powder feeding amount is program-controlled by the two powder feeders to achieve the configuration of the two powders. During spraying, the spraying power and spraying distance of high entropy carbide and high entropy boride are kept consistent to ensure the uniformity of spraying. The spraying power is 30-35kW, and the spraying distance is 80-100mm, for example, the spraying power is 30kW, the spraying distance is 100mm, and another example is the spraying power is 35kW, and the spraying distance is 80mm.
[0105] In step 2, the ratio of high entropy carbide to high entropy boride is controlled by adjusting the powder feeding rates of two powder feeders of the dual-beam plasma spraying system respectively. Generally, the powder feeding rates of high entropy carbide and high entropy boride are both between 1 and 5 kg / h.
[0106] Furthermore, by program-controlled powder feeding rate change of the powder feeder, the ratio of the two ceramics can be controlled to change with thickness. For example, the powder feeding rates of high entropy carbide and high entropy boride are set to appropriate ranges in the dual-beam plasma spraying system, respectively, so as to achieve a gradual change in the content of high entropy carbide and high entropy boride in the coating from the bottom (close to the substrate) to the outer surface (far away from the substrate). For example, the powder feeding rate of high entropy carbide is set to 1-5 kg / h in the dual-beam plasma spraying system, and the powder feeding rate of high entropy boride is set to 5-1 kg / h. At this time, the high entropy boride content of the coating obtained after spraying gradually decreases from the bottom to the outer surface, and the high entropy carbide content is the opposite, that is, it gradually increases from the bottom to the outer surface, so as to avoid the oxidation volatilization of the external high entropy boride, and utilize the slower volatilization of the boron oxide generated by internal oxidation to improve the anti-oxidation performance and action time of the internal high entropy boride, thereby improving the anti-oxidation and ablation performance and anti-oxidation ablation time of the entire coating, such as Figure 8 shown.
[0107] Of course, the powder feeding rates of high entropy carbide and high entropy boride can also be set to be the same, in which case the high entropy carbide and high entropy boride are uniformly doped in the obtained coating. For example, the powder feeding rate of high entropy carbide is 2 kg / h, and the powder feeding rate of high entropy boride is 2 kg / h.
[0108] In addition to the above, the powder feeding rate of high entropy carbide and the powder feeding rate of high entropy boride can also be set to specific values, in which case the high entropy carbide and high entropy boride in the obtained coating are distributed in the same proportion in each layer. For example, the powder feeding rate of high entropy carbide is 2 kg / h, and the powder feeding rate of high entropy boride is 1 kg / h.
[0109] In step 2, the working gases used in plasma thermal spraying are argon and hydrogen.
[0110] Example:
[0111] The present invention is further described below through specific examples, but these examples are merely exemplary and do not constitute any limitation to the scope of protection of the present invention.
[0112] Example 1 :
[0113] (1) 0.1 mol TiC, 0.1 mol ZrC, 0.1 mol HfC and 0.1 mol TaC were mixed and placed in a ball mill at 400 r / min for 6 h, with a ball-to-material weight ratio of 5:1. After the ball milling, a mixed powder was obtained. The mixed powder was placed in a graphite crucible, placed in a vacuum sintering system, evacuated to below 6 Pa, and argon was introduced into the sintering system. The mixture was sintered at 2000°C for 6 h, and then the sintered product was placed in a ball mill at 400 r / min for a second ball milling for 2 h. The ball-to-material weight ratio was 5:1. After the second ball milling, the mixture was sieved through a 200 mesh sieve to obtain a high entropy carbide with a particle size of 200 mesh.
[0114] FIG1(a) shows a scanning electron microscope microscopic morphology of the prepared high entropy carbide, and FIG1(b) shows an X-ray diffraction pattern of the prepared high entropy carbide, indicating that it is basically a single rock salt type face-centered cubic structure.
[0115] (2) 0.1 mol TiB2, 0.1 mol ZrB2, 0.1 mol HfB2 and 0.1 mol TaB2 were mixed and placed in a ball mill for 6 hours at 400 r / min, with a ball-to-material weight ratio of 5:1. After the ball milling was completed, a mixed powder was obtained. The mixed powder was placed in a graphite crucible, placed in a vacuum sintering system, evacuated to below 6 Pa, argon was introduced into the sintering system, and sintered at 2000°C for 6 hours. The sintered product was then placed in a ball mill for a second time at 400 r / min for 2 hours, with a ball-to-material weight ratio of 5:1. After the second ball milling was completed, it was sieved through a 200-mesh sieve to obtain a high entropy boride with a particle size of ~200 mesh.
[0116] FIG2(a) shows a scanning electron microscope microscopic morphology of the prepared high entropy boride, and FIG2(b) shows an X-ray diffraction pattern of the prepared high entropy boride, indicating that it is basically a single hexagonal crystal structure.
[0117] (3) C / C composite material was selected as the matrix, and white corundum with a particle size of 30 mesh was used for sandblasting. The obtained matrix surface roughness was Ra5.0. After treatment, it was cleaned with high-pressure gas and cleaned with alcohol in an ultrasonic cleaner for standby use.
[0118] (4) The high entropy carbide and high entropy boride prepared in step (1) are placed in two powder feeders of a dual-beam plasma spraying system respectively. The plasma spraying power of the high entropy carbide spray gun is 30 kW, the spraying distance is 100 mm, and the powder feeding rate is 2 kg / h. The plasma spraying power of the high entropy boride spray gun is 30 kW, the spraying distance is 100 mm, and the powder feeding rate is 1 kg / h. After spraying, a multiphase high entropy ceramic coating is obtained, and the high entropy carbide content in the obtained coating is about 67 wt.%.
[0119] Figure 3(a) shows a macroscopic optical image of the prepared multiphase high-entropy ceramic coating, from which it can be seen that the coating is uniform and flat as a whole; Figure 3(b) shows a scanning electron microscope microscopic morphology of the prepared multiphase high-entropy ceramic coating, from which it can be seen that the coating has a layered structure with pores. The layered structure of the coating is formed by a large number of parallel disc-shaped particles bonded to each other. These particles are formed by high-speed collision of semi-molten high-entropy ceramic particles. The pores in the coating are caused by the mutual stacking and solidification shrinkage of the particles during the spraying process.
[0120] After testing, the thickness of the prepared composite high entropy ceramic coating is 152μm, the hardness is 55GPa, and the bonding strength with the C / C composite matrix is 31MPa. The thermal shock resistance is tested by repeated ablation with oxyacetylene combined with air cooling, ablation for 10s, air cooling for 10s, and the number of thermal shock resistance reaches 12 times. The coating is 4MW / m 2 After 240s of oxyacetylene flame ablation with a heat flux density, the linear ablation rate is 3μm / s, and the average oxidation rate of the coating at 1600℃ is 0.08g·cm -2 ·h -1 .
[0121] Figure 4 Figure 5(a) shows the macroscopic optical photograph of the composite high entropy ceramic coating after ablation; Figure 5(a) shows the SEM microscopic morphology of the coating after ablation; Figure 4 It can be clearly seen from Figure 5(a) that after ablation, the coating surface has ablation center area, transition area and edge area; Figure 4 It can also be seen that the ablation center area is slightly raised, the color of the transition area changes, and the edge area does not change much; overall, there is no depression on the sample surface, indicating that the sample is not severely ablated and has sufficient strength to resist flame erosion during the ablation process; at the same time, the coating does not fall off, indicating that the coating has excellent ablation resistance. It can also be seen from Figure 5(a) that the surface of the coating becomes loose after ablation, and there are some molten blown structures in the transition area.
[0122] Figure 5(b) shows the microscopic morphology of the central area of Figure 5(a). It can be seen that there are no obvious cracks and holes in the coating in the ablation center area. This is because the B2O3 generated by the oxidation of high-entropy boride in the coating during the high-temperature ablation process has excellent antioxidant properties and fluidity, which can effectively alleviate the oxidation of the coating and play a role in the self-healing of the coating cracks through fluidity.
[0123] Figure 6 SEM images showing the ablated area of the coating. Figure 7 Show Figure 6 The EDS energy spectrum at the yellow cross mark and the specific EDS energy spectrum element analysis results are shown in Table 1.
[0124] Table 1:
[0125] element Content (at.%) O 65.5 Ti 9.6 Zr 8.4 Hf 8.2 Ta 8.3 total 100
[0126] Combination Figure 7 From the energy spectrum analysis results in Table 1, it can be seen that the surface of the ablation area is the alloy oxidation product.
[0127] Example 2 :
[0128] (1) 0.1 mol TiO2, 0.1 mol ZrO2, 0.1 mol HfO2, 0.05 mol Ta2O5, 0.05 mol Nb2O5 and 1.6 mol carbon powder were mixed and placed in a ball mill and ground at 450 r / min for 5 h, with a ball-to-material weight ratio of 5:1. After grinding, a mixed powder was obtained. The mixed powder was placed in a graphite crucible, placed in a vacuum sintering system, evacuated to below 6 Pa, and argon was introduced into the sintering system. The mixture was calcined at 1800°C for 5 h, and then the calcined product was placed in a ball mill and ground for a second time at 450 r / min for 2 h. The ball-to-material weight ratio was 5:1. After the second grinding, the mixture was sieved through a 200-mesh sieve to obtain a high entropy carbide with a particle size of 200 mesh.
[0129] (2) 0.1 mol TiO2, 0.1 mol ZrO2, 0.1 mol HfO2, 0.05 mol Ta2O5, 0.05 mol Nb2O5, 0.5 mol B2O3 and 3 mol carbon powder were mixed and placed in a ball mill and ground at 450 r / min for 5 h, with a ball-to-material weight ratio of 5:1. After grinding, a mixed powder was obtained. The mixed powder was placed in a graphite crucible, placed in a vacuum sintering system, evacuated to below 6 Pa, and argon was introduced into the sintering system. The mixture was calcined at 1900°C for 4.5 h, and then the calcined product was placed in a ball mill and ground for a second time at 450 r / min for 2 h. The ball-to-material weight ratio was 5:1. After the second grinding, the mixture was sieved through a 200-mesh sieve to obtain a high entropy boride with a particle size of 200 mesh.
[0130] (3) C / C composite material was selected as the matrix, and white corundum with a particle size of 40 mesh was used for sandblasting. The obtained matrix surface roughness was Ra4.0. After treatment, it was cleaned with high-pressure gas and cleaned with alcohol in an ultrasonic cleaner for standby use.
[0131] (4) The high entropy carbide and high entropy boride prepared in step (1) are placed in two powder feeders of a dual-beam plasma spraying system respectively. The plasma spraying power of the high entropy carbide spray gun is 35 kW, the spraying distance is 80 mm, and the powder feeding rate is 2 kg / h. The plasma spraying power of the high entropy boride spray gun is 35 kW, the spraying distance is 80 mm, and the powder feeding rate is 2 kg / h. After spraying, a multiphase high entropy ceramic coating is obtained, and the high entropy carbide content in the obtained coating is about 50 wt.%.
[0132] After testing, the thickness of the prepared composite high entropy ceramic coating is 183μm, the hardness is 58GPa, and the bonding strength with the C / C composite matrix is 32MPa. The thermal shock resistance is tested by repeated ablation with oxyacetylene combined with air cooling, ablation for 10s, air cooling for 10s, and the number of thermal shock resistance reaches 11 times. 2 After 240s of oxyacetylene flame ablation with a heat flux density, the linear ablation rate is 4μm / s, and the average oxidation rate of the coating at 1600℃ is 0.04g·cm -2 ·h -1 .
[0133] The present invention is described in detail above in combination with preferred embodiments and exemplary examples. However, it should be noted that these specific embodiments are only illustrative explanations of the present invention and do not constitute any limitation on the protection scope of the present invention. Without exceeding the spirit and protection scope of the present invention, various improvements, equivalent substitutions or modifications may be made to the technical content of the present invention and its embodiments, which all fall within the protection scope of the present invention. The protection scope of the present invention shall be subject to the attached claims.
Claims
1. A multiphase high entropy ceramic coating, It is characterized in that The coating comprises high entropy carbide and high entropy boride, and the expression of the high entropy carbide is: (TiZrHfTaM x )C, the expression of the high entropy boride is: (TiZrHfTaN y )B 2 , M and N are each independently W, V, Nb or Mo.
2. The coating according to claim 1, It is characterized in that Preferably, x is 0 or 1.
3. The coating according to claim 1, It is characterized in that y is either 0 or 1.
4. The coating according to claim 1, It is characterized in that The high entropy carbide in the multiphase high entropy ceramic coating has a rock salt face-centered cubic structure.
5. The coating according to claim 1, It is characterized in that The high entropy boride in the multiphase high entropy ceramic coating has a hexagonal crystal structure.
6. The coating according to claim 1, It is characterized in that Calculated based on the mass of the composite high entropy ceramic coating, the content of the high entropy carbide is 10 to 90 wt.%.
7. The coating according to claim 1, It is characterized in that The multiphase high entropy ceramic coating has a 2 The heat flux density of oxyacetylene flame was ablated for 240s, and the linear ablation rate was 3-4μm / s.
8. A method for preparing a coating according to any one of claims 1 to 7, It is characterized in that The method comprises: Step 1, preparing high entropy carbide and high entropy boride respectively; Step 2: spraying the high entropy carbide and the high entropy boride on the substrate simultaneously to obtain the multiphase high entropy ceramic coating.
9. The method according to claim 8, It is characterized in that In step 1, the expression of the high entropy carbide is: (TiZrHfTaM x )C, M is W, V, Nb or Mo, and x is 0 or 1.
10. The method according to claim 8, It is characterized in that In step 1, the expression of the high entropy boride is: (TiZrHfTaN y )B 2 , N is W, V, Nb or Mo, and y is 0 or 1.
Citation Information
Patent Citations
Method for synchronously feeding powder to prepare ceramic based thermal barrier coating of continuous and gradual variation structure
CN105951028A
Double-gradient heat-insulation anti-ablative coating and preparation method thereof
CN109338270A
Preparation method of multi-component ultrahigh-temperature oxidation-resistant ablation-resistant ceramic coating
CN115231954A
Two-phase high-entropy ceramic based on microstructure regulation and control as well as preparation method and application of two-phase high-entropy ceramic
CN115385696A
Ablation-resistant high-entropy carbide-high-entropy diboride-silicon carbide multiphase ceramic and preparation thereof
US20230167029A1
Cited By
Medium-entropy ceramic material as well as preparation method and application thereof
CN119019171A
A medium-entropy ceramic material, a preparation method and application thereof
CN119019171B