Method for preparing porous lightweight ceramic thermal insulation material from blast furnace slag

Through the mixing and sintering of blast furnace slag, fly ash and other materials, porous light ceramic insulation materials are prepared, which solves the problems of high density, low flexural strength and high thermal conductivity of existing ceramic materials, and achieves low energy consumption and green Environmentally friendly building materials applications.

CN119039035APending Publication Date: 2024-11-29PANZHIHUA UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411165359.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The foamed ceramic materials prepared from existing blast furnace slag have too large density, low flexural strength, too high thermal conductivity, and too high sintering temperature, which is not conducive to energy conservation and emission reduction.

Method used

The mixture of blast furnace slag, fly ash, sodium carbonate, boric acid, adhesive and sodium phosphate is pressed and sintered to prepare porous light ceramic insulation materials. By controlling the sintering temperature and the use of adhesives, the materials are reduced. The bulk density and thermal conductivity of the product improve the flexural strength.

Benefits of technology

The prepared porous light ceramic insulation material has good flexural strength, low thermal conductivity and low volume density, which meets the standard requirements of thermal insulation foam ceramics outside building exterior walls, and has a reduced sintering temperature and energy consumption, which meets the requirements of green development. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007714260000061
    Figure BDA0005007714260000061
  • Figure BDA0005007714260000062
    Figure BDA0005007714260000062
  • Figure BDA0005007714260000071
    Figure BDA0005007714260000071
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, in particular to a method for preparing a porous lightweight ceramic thermal insulation material from blast furnace slag. The method for preparing the porous lightweight ceramic thermal insulation material by using the blast furnace slag comprises the following steps: 1) mixing: uniformly mixing the blast furnace slag, fly ash, sodium carbonate, boric acid, an adhesive and sodium phosphate, and sealing and placing for 20-30 hours to obtain a mixture; 2) blank making: pressing and drying the mixture obtained in the step 1) to obtain a blank; and (3) sintering: sintering the blank prepared in the step (2), and preserving heat to obtain the porous light-weight thermal insulation material. According to the invention, the blast furnace slag is used as a main raw material, one-time sintering is adopted, the porous lightweight ceramic thermal insulation material can be prepared and obtained, and the porous lightweight ceramic thermal insulation material has the advantages of good breaking strength, low heat conductivity coefficient, low volume density and low volume water absorption rate, and meets the standard requirements of building exterior wall external thermal insulation foamed ceramics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a method for preparing a porous lightweight ceramic thermal insulation material by utilizing blast furnace slag. Background Art

[0002] The rich vanadium-titanium magnetite in the Panxi area can produce a variety of metals after smelting. However, there is a large amount of slag after smelting, which also contains rich metal elements such as vanadium and titanium. Most factories deal with it by directly piling it up. my country has made some achievements in the utilization of blast furnace waste slag, and the utilization rate of blast furnace slag has reached about 80%, but there is still a certain gap compared with some developed countries. In recent years, my country has carried out a lot of research on the utilization of titanium-containing blast furnace slag, which is mainly divided into two aspects: on the one hand, the use of technical means to extract the precious metal substances contained in the slag; on the other hand, the overall utilization of the slag. The first method is not perfect in technology, the cost is too high, and it is easy to cause secondary pollution, so the second method is currently used to treat the slag.

[0003] The overall utilization of blast furnace slag is widely used in agriculture, construction industry and daily life. With the introduction of my country's dual carbon policy, the construction industry is also seeking transformation and upgrading. In most parts of China, the temperature is relatively cold in winter, and many families use air conditioners, floor heating and other heating tools indoors. If the building materials are replaced with a material that is both heat-insulating, solid and lightweight, then the heat loss in the house can be directly reduced, thereby reducing the use of heating measures such as air conditioners and floor heating, thereby reducing carbon emissions.

[0004] The invention with application number 201810378797.7 discloses a method for preparing foamed ceramic materials using blast furnace slag and high-aluminum fly ash, the method comprising the following steps: (1) grinding blast furnace slag, high-aluminum fly ash and silica sand and mixing them as raw materials; (2) preparing borax, sodium carbonate, calcium carbonate, sodium metaphosphate and clay as additives; (3) mixing the raw materials and additives to form a mixed material, and wet grinding and mixing to form a slurry; (4) spray granulation to form powder particles; (5) filling into a mold for baking and foaming and forming holes; (6) cooling to room temperature with the furnace to obtain a foamed ceramic material. The foamed ceramic obtained by this method has too high density, too low flexural strength, too high thermal conductivity, and too high sintering temperature, which is not conducive to energy conservation and emission reduction.

[0005] In view of this, it is of great significance to provide a method for preparing porous lightweight ceramic thermal insulation materials using blast furnace slag. Summary of the invention

[0006] The invention discloses a method for preparing a porous lightweight ceramic thermal insulation material by using blast furnace slag. The prepared porous lightweight ceramic material has good flexural strength and low density, and also has low thermal conductivity and volume water absorption.

[0007] The method for preparing a porous lightweight ceramic thermal insulation material using blast furnace slag of the present invention comprises the following steps:

[0008] 1) Mixing: Mix blast furnace slag, fly ash, sodium carbonate, boric acid, adhesive and sodium phosphate, seal and place at room temperature for 20 to 30 hours to obtain a mixture;

[0009] 2) blank making: pressing and drying the mixed material obtained in step 1) to obtain a blank;

[0010] 3) Sintering: Sintering the blank prepared in step 2) and keeping it warm to obtain a porous lightweight thermal insulation material.

[0011] In a specific embodiment of the present invention, in step 1) mixing, the particle size of the blast furnace slag is 20-100 mesh.

[0012] In a specific embodiment of the present invention, the particle size of the blast furnace slag is 60-80 mesh.

[0013] In a specific embodiment of the present invention, in step 1) mixing, the mass ratio of the blast furnace slag, fly ash, sodium carbonate, boric acid, adhesive and sodium phosphate is 5-65:0-60:5-15:5-10:1-5:1-5.

[0014] In a specific embodiment of the present invention, the mass ratio of blast furnace slag, fly ash, sodium carbonate, boric acid, adhesive and sodium phosphate is 35:30:15:10:5:5.

[0015] In a specific embodiment of the present invention, in step 1) mixing, the binder is kaolin and carboxymethyl cellulose.

[0016] In a specific embodiment of the present invention, in step 2) forming the blank, the pressing pressure is 5 to 20 MPa and the pressing time is 5 to 15 s.

[0017] In a specific embodiment of the present invention, in step 2) forming the blank, the drying temperature is 100-120° C. and the drying time is 1-2 hours.

[0018] In a specific embodiment of the present invention, step 3) sintering, the sintering and heat preservation is heating to a first temperature and keeping it at the first temperature, and then heating to a second temperature and keeping it at the second temperature.

[0019] In a specific embodiment of the present invention, the first temperature is 500° C., and the first temperature is kept for 1 to 2 hours; the second temperature is 700 to 900° C., and the second temperature is kept for 1 to 3 hours.

[0020] In one embodiment of the present invention, the second temperature is 825°C.

[0021] In a specific embodiment of the present invention, the temperature is maintained at the second temperature for 2 hours.

[0022] In the present invention, the main components of blast furnace slag are 27-28wt% CaO, 24-25wt% SiO 2 and 23-24wt% TiO 2 , thermogravimetric analysis of the original blast furnace slag found that the melting point of blast furnace slag was between 1000 and 1300°C; while the melting point of the mixture obtained by mixing blast furnace slag with fly ash, sodium carbonate, boric acid and other raw materials was in the range of 700 to 1100°C by thermogravimetric analysis.

[0023] The porous lightweight ceramic thermal insulation material prepared by the present invention using blast furnace slag has a volume density of 88-180 kg / m 3 , flexural strength is 0.69~5.99MPa, thermal conductivity is 0.09~0.35W·m -1 ·k -1 The apparent porosity is 24-26%.

[0024] The beneficial effects of the present invention are:

[0025] 1. The present invention uses blast furnace slag as the main raw material and adopts one-time sintering to prepare and obtain a porous lightweight ceramic thermal insulation material. The porous lightweight ceramic thermal insulation material has good flexural strength, low thermal conductivity, low volume density, and low volume water absorption, and meets the standard requirements of external thermal insulation foam ceramics for building exterior walls;

[0026] 2. The method of the present invention is simple and convenient, without complicated operation process, and is easy to realize industrialization. The sintering temperature in the preparation process is low, which greatly reduces the energy consumption of the preparation of foamed ceramics. The raw material blast furnace slag is industrial waste, which meets the requirements of green development and can be widely used in the construction field. DETAILED DESCRIPTION

[0027] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0028] The method for preparing a porous lightweight ceramic thermal insulation material using blast furnace slag comprises the following steps:

[0029] 1) Mixing: Mix blast furnace slag, fly ash, sodium carbonate, boric acid, adhesive and sodium phosphate, stir and granulate in a mortar for 10 to 15 minutes, seal and place at room temperature for 20 to 30 hours to obtain a mixture;

[0030] 2) blank making: pressing and drying the mixed material obtained in step 1) to obtain a blank;

[0031] 3) Sintering: Sintering the blank prepared in step 2) and keeping it warm to obtain a porous lightweight thermal insulation material.

[0032] In some examples, in step 1) mixing, the particle size of the blast furnace slag is 20-100 mesh.

[0033] In some examples, the blast furnace slag has a particle size of 60-80 mesh.

[0034] In some examples, in step 1) mixing, the mass ratio of blast furnace slag, fly ash, sodium carbonate, boric acid, binder and sodium phosphate is 5-65:0-60:5-15:5-10:1-5:1-5.

[0035] In some examples, the mass ratio of the blast furnace slag, fly ash, sodium carbonate, boric acid, adhesive, and sodium phosphate is 35:30:15:10:5:5.

[0036] In some examples, in step 1) mixing, the binder is kaolin and carboxymethyl cellulose.

[0037] It should be noted that, in order to better play a bonding role, carboxymethyl cellulose is usually prepared with water into a 3% carboxymethyl cellulose solution, and the amount used is appropriate to make the mixture wet, avoiding the introduction of too much water and affecting the bonding effect of the mixture; the amount of kaolin is determined based on the amount of adhesive in the mixture and the amount of carboxymethyl cellulose introduced into the carboxymethyl cellulose solution.

[0038] In some examples, in step 2) forming the blank, the pressing pressure is 5 to 20 MPa and the pressing time is 5 to 15 s.

[0039] In some examples, in step 2), the pelletizing is performed at a drying temperature of 100° C. for 2 h.

[0040] In some examples, step 3) sintering, sintering and holding is heating to a first temperature and holding at the first temperature, and then heating to a second temperature and holding at the second temperature.

[0041] In the present invention, the temperature in the sintering process is programmed and the heating rate is 3-10°C / min.

[0042] In some examples, the first temperature is 500° C., and the first temperature is kept for 1 to 2 hours; the second temperature is 700 to 900° C., and the second temperature is kept for 1 to 3 hours.

[0043] In some examples, the second temperature is 825°C.

[0044] In some examples, the incubation at the first temperature is 1 h.

[0045] In some examples, the second temperature is maintained for 2 hours.

[0046] It should be noted that the second temperature is the final sintering temperature for preparing the porous lightweight ceramic thermal insulation material. After being kept at the second temperature and naturally cooled, the porous lightweight ceramic thermal insulation material can be obtained.

[0047] In order to further illustrate the technical solution of the present invention, the following embodiments are provided:

[0048] In the following examples, the chemical composition and content of blast furnace slag are: TiO 2 23.16%,Fe 2 O 3 2.64%, SiO 2 24.01%, MgO 7.47%, Al 2 0 3 13.49%, CaO 27.19%, V 2 0 5 0.82%, F 0.12%;

[0049] The chemical composition and content of fly ash are: TiO 2 1.809%,Fe 2 O 3 8.393%, SiO 2 46.48%, MgO9.4%, Al 2 0 3 30.71%, CaO 3.23%

[0050] The chemical composition and content of kaolin are: TiO 2 1%,Fe 2 O 3 0.8%,SiO 2 55.7%, Al 2 O 3 42.5%.

[0051] Example 1

[0052] This embodiment provides a method for preparing a porous lightweight ceramic thermal insulation material using blast furnace slag, comprising the following steps:

[0053] 1. According to the mass ratio of raw materials of different groups (sequentially marked as S1-1 to S1-4) provided in Table 1, 60-80 mesh blast furnace slag, fly ash, sodium carbonate, boric acid, kaolin, sodium phosphate and carboxymethyl cellulose are mixed in a mortar and stirred for 15 minutes, and sealed and placed at room temperature for 24 hours to obtain a mixture; wherein, the adhesive is composed of kaolin and carboxymethyl cellulose in a total of 5 parts by mass, and the carboxymethyl cellulose is configured into a carboxymethyl cellulose solution with a concentration of 3%. After the carboxymethyl cellulose solution is added to the mixture, a wetting effect (water content of about 15%) is achieved, and the mass part of kaolin is determined by the mass part of carboxymethyl cellulose introduced by the solution, so that the mass part of the adhesive is 5 parts;

[0054] Table 1

[0055]

[0056] 2. Pour the mixture into the mold, press at 15 MPa for 10 seconds, take out the blank sample and dry it in a drying oven at 100°C for 2 hours to obtain the blank;

[0057] 3. Place the blank into a crucible padded with alumina and into a muffle furnace, heat to 500°C at 5°C / min, and keep warm for 1 hour; then heat to 825°C at 5°C / min, keep warm for 2 hours, and take out when the furnace temperature is <400°C to obtain a porous lightweight ceramic thermal insulation material.

[0058] The performance parameters of the porous lightweight ceramic thermal insulation material of this embodiment are shown in Table 2.

[0059] Table 2

[0060]

[0061] Example 2

[0062] This embodiment provides a method for preparing a porous lightweight ceramic thermal insulation material using blast furnace slag, comprising the following steps:

[0063] 1. Take 60-80 mesh blast furnace slag, fly ash, sodium carbonate, boric acid, kaolin, sodium phosphate and carboxymethyl cellulose in a mass ratio of 35:30:15:10:5:5, mix them in a mortar and stir for 15 minutes, seal and place at room temperature for 24 hours to obtain a mixture;

[0064] 2. Pour the mixture into the mold, press at 15 MPa for 10 seconds, take out the blank sample and dry it in a drying oven at 100°C for 2 hours to obtain the blank;

[0065] 3. Place different blanks in a crucible padded with alumina and put them together in a muffle furnace, heat them to 500°C at 5°C / min, and keep them warm for 1 hour; then heat the different blanks to 700°C, 800°C, 850°C and 875°C at 5°C / min respectively (marked in sequence as S2-1 to S2-4), keep them warm for 2 hours, and take them out when the furnace temperature is <400°C to obtain a porous lightweight ceramic thermal insulation material.

[0066] The performance parameters of the porous lightweight ceramic thermal insulation material of this embodiment are shown in Table 3.

[0067] Table 3

[0068]

[0069] Example 3

[0070] This embodiment provides a method for preparing a porous lightweight ceramic thermal insulation material using blast furnace slag, comprising the following steps:

[0071] 1. Take 40-60 mesh blast furnace slag, fly ash, sodium carbonate, boric acid, kaolin, sodium phosphate and carboxymethyl cellulose in a mass ratio of 35:30:15:10:5:5, mix them in a mortar and stir for 15 minutes, seal and place at room temperature for 24 hours to obtain a mixture;

[0072] 2. Pour the mixture into the mold, press at 15 MPa for 10 seconds, take out the blank sample and dry it in a drying oven at 100°C for 2 hours to obtain the blank;

[0073] 3. Place four groups of identical blanks into crucibles padded with alumina and into a muffle furnace together, heat to 500°C at 5°C / min, and keep warm for 1h; then heat the blanks to 825°C at 5°C / min, keep warm for 1h, 1.5h and 2.5h respectively (marked in sequence as S3-1 to S3-3), take them out when the furnace temperature is <400°C, and obtain a porous lightweight ceramic thermal insulation material.

[0074] The performance parameter statistics of the porous lightweight ceramic thermal insulation material of this embodiment are shown in Table 4.

[0075] Table 4

[0076]

[0077] Example 4

[0078] This embodiment provides a method for preparing a porous lightweight ceramic thermal insulation material using blast furnace slag, comprising the following steps:

[0079] 1. Take 20-40 mesh and 40-60 mesh blast furnace slag (marked as S4-1 and S4-2 in sequence) in a mass ratio of 35:30:15:10:5:5, mix with fly ash, sodium carbonate, boric acid, kaolin, sodium phosphate and carboxymethyl cellulose in a mortar and stir for 15 minutes, seal and place at room temperature for 24 hours to obtain a mixture;

[0080] 2. Pour the mixture into the mold, press at 15 MPa for 10 seconds, take out the blank sample and dry it in a drying oven at 100°C for 2 hours to obtain the blank;

[0081] 3. Place the blank into a crucible padded with alumina and place them together into a muffle furnace, heat to 500°C at 5°C / min, and keep warm for 1 hour; then heat the blanks to 825°C at 5°C / min, keep warm for 2 hours, and take them out when the furnace temperature is <400°C to obtain a porous lightweight ceramic thermal insulation material.

[0082] The performance parameter statistics of the porous lightweight ceramic thermal insulation material of this embodiment are shown in Table 5.

[0083] Table 5

[0084]

[0085] Example 5

[0086] This embodiment provides a method for preparing a porous lightweight ceramic thermal insulation material using blast furnace slag, comprising the following steps:

[0087] 1. Take 60-80 mesh blast furnace slag, fly ash, sodium carbonate, boric acid, kaolin, sodium phosphate and carboxymethyl cellulose in a mass ratio of 35:30:15:10:5:5, mix them in a mortar and stir for 15 minutes, seal and place at room temperature for 24 hours to obtain a mixture;

[0088] 2. Pour the mixture into the mold, press at 15 MPa for 10 seconds, take out the blank sample and dry it in a drying oven at 100°C for 2 hours to obtain the blank;

[0089] 3. Place the blank into a crucible padded with alumina and place them together into a muffle furnace, heat to 500°C at 5°C / min, and keep warm for 1 hour; then heat the blanks to 825°C at 5°C / min, keep warm for 2 hours respectively, and take them out when the furnace temperature is <400°C to obtain a porous lightweight ceramic thermal insulation material.

[0090] The performance parameters of the porous lightweight ceramic thermal insulation material obtained in this embodiment are:

[0091] Bulk density: 128.55kg / m 3 ;

[0092] Volume water absorption: 3.63%;

[0093] Flexural strength: 3.93MPa;

[0094] Thermal conductivity: 0.09W·m -1 ·k -1 .

Claims

1. A method for preparing a porous lightweight ceramic thermal insulation material using blast furnace slag, characterized in that: The following steps are involved: 1) Mixing: Mix blast furnace slag, fly ash, sodium carbonate, boric acid, kaolin and sodium phosphate, seal and place at room temperature for 20 to 30 hours to obtain a mixture; 2) blank making: pressing and drying the mixed material obtained in step 1) to obtain a blank; 3) Sintering: Sintering the blank prepared in step 2) and keeping it warm to obtain a porous lightweight thermal insulation material.

2. The method for preparing a porous lightweight ceramic thermal insulation material using blast furnace slag according to claim 1, characterized in that: Step 1) Mixing, the particle size of the blast furnace slag is 20-100 mesh; preferably, the particle size of the blast furnace slag is 60-80 mesh.

3. The method for preparing a porous lightweight ceramic thermal insulation material using blast furnace slag according to claim 1 or 2, characterized in that: Step 1) mixing, the mass ratio of blast furnace slag, fly ash, sodium carbonate, boric acid, binder and sodium phosphate is 5-65:0-60:5-15:5-10:1-5:1-5.

4. The method for preparing a porous lightweight ceramic thermal insulation material using blast furnace slag according to claim 3, characterized in that: The mass ratio of the blast furnace slag, fly ash, sodium carbonate, boric acid, binder and sodium phosphate is 35:30:15:10:5:

5.

5. The method for preparing porous lightweight ceramic thermal insulation material using blast furnace slag according to claim 1, characterized in that: Step 1) mixing materials, wherein the adhesive is kaolin and carboxymethyl cellulose.

6. The method for preparing porous lightweight ceramic thermal insulation material using blast furnace slag according to claim 1, characterized in that: Step 2) forming the blank, wherein the pressing pressure is 5 to 20 MPa and the pressing time is 5 to 15 seconds.

7. The method for preparing porous lightweight ceramic thermal insulation material using blast furnace slag according to claim 1, characterized in that: Step 2) forming the blank, wherein the drying temperature is 100-120° C. and the drying time is 1-2 hours.

8. The method for preparing porous lightweight ceramic thermal insulation material using blast furnace slag according to claim 1, characterized in that: Step 3) sintering, wherein the sintering and heat preservation is heating to a first temperature and heat preservation at the first temperature, and then heating to a second temperature and heat preservation at the second temperature.

9. The method for preparing porous lightweight ceramic thermal insulation material using blast furnace slag according to claim 8, characterized in that: The first temperature is 500°C, and the temperature is kept at the first temperature for 1 to 2 hours; the second temperature is 700 to 900°C, and the temperature is kept at the second temperature for 1 to 3 hours; preferably, the second temperature is 825°C.

10. The method for preparing porous lightweight ceramic thermal insulation material using blast furnace slag according to claim 9, characterized in that: Keep at the second temperature for 2 hours.

Citation Information

Patent Citations

  • Preparation method for electrolytic manganese residue porous ceramics

    CN102584316A

  • Foaming microcrystal material based on smelt slag and production process thereof

    CN108439809A

  • Method for preparing foaming ceramic materials from blast-furnace slags and high-aluminum pulverized coal ash

    CN108503371A

  • Ceramic material prepared from coal ash and medium-titanium blast furnace slag and preparation method of ceramic material