Ceramic core high-low temperature synchronous strengthening method
By using high and low temperature synchronous reinforcement solution and photocuring technology, the problem of cumbersome and deformation of the ceramic core strengthening process is solved, and the high and low temperature synchronous reinforcement of the ceramic core is achieved, which improves its strength and stability.
Patent Information
- Application Number
- CN202411163482.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
The strengthening process of existing ceramic cores requires high-temperature and low-temperature reinforcement, and the process is complicated and it is easy to cause deformation and cracking of ceramic cores in complex structures. Traditional reinforcements are incompatible with each other, so it is impossible to achieve synchronous strengthening of high and low temperatures.
High and low temperature synchronous enhancement solution, including photocuring resin, nano SiO2, nano Al2O3, silicon nitride whiskers, is used to photocure after ultrasonic dispersion and vacuum impregnation, simplifying the strengthening process and avoiding deformation caused by thermal effects.
The strengthening process of ceramic cores is significantly simplified, its low-temperature and high-temperature strength is improved, deformation and cracking are avoided, and the synchronous strengthening of high and low temperatures is achieved.
Smart Images

Figure CN119039049A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic core strengthening, and in particular provides a high-low temperature synchronous strengthening method for a ceramic core. Background Art
[0002] As a transition piece for forming the hollow inner cavity structure of precision castings, the ceramic core has the following functions: forming the inner cavity shape of precision castings, and together with the outer mold and mold shell, ensuring the dimensional accuracy of the wall thickness of precision castings. During use, the ceramic core must meet the requirements of normal temperature wax pressure fluid impact, high temperature casting metal liquid impact, and effective removal of the ceramic core after the casting is completed under precision casting conditions. Among them, low temperature strength and high temperature strength are one of the most core indicators for evaluating the performance of ceramic cores.
[0003] In order to meet the above strength indicators, the strengthening process of ceramic cores is generally as follows: ceramic core - special high temperature strengthening liquid preparation (generally silica sol or ethyl silicate hydrolyzate) - immerse the ceramic core in the high temperature strengthening liquid for 5-30 minutes - natural drying or drying - special low temperature strengthening liquid preparation (generally epoxy resin or varnish) - immerse the ceramic core in the low temperature strengthening liquid for 30-60 minutes - natural drying - put it in the oven for high temperature hardening (generally 120℃ for 2 hours). The above process mainly has the following problems: 1. High temperature strengthening and low temperature strengthening need to be carried out separately, and the process is relatively cumbersome. 2. Thermal curing treatment is required during the strengthening process. For ceramic cores with complex structures, especially thin-walled ceramic cores, deformation, cracking and other phenomena will occur. 3. The content of SiO2, an effective ingredient in the high temperature strengthener, is generally below 30%, and the strengthening effect is general.
[0004] Therefore, proposing a high and low temperature simultaneous strengthening process method for ceramic cores has become an urgent problem to be solved. Summary of the invention
[0005] The purpose of the present invention is to provide a high-low temperature synchronous strengthening method for a ceramic core to solve the problems existing in the prior art.
[0006] In order to achieve the above object, the present invention provides a high-low temperature synchronous strengthening method for a ceramic core, comprising: immersing the ceramic core to be strengthened into a high-low temperature synchronous strengthening solution for vacuum impregnation; performing photocuring on the impregnated ceramic core to finally obtain a strengthened ceramic core;
[0007] The method for preparing the high and low temperature simultaneous strengthening solution comprises:
[0008] Step 1: According to the mass percentage, weigh the following raw materials according to the following ratio: photocurable resin 40-60wt%, nano-SiO2 1-50wt%, nano-Al2O3 1-60wt%, silicon nitride whisker 0.1-1wt%;
[0009] Step 2: Place the photocurable resin into an ultrasonic dispersing device, and add silicon nitride whiskers, nano-SiO2, and nano-Al2O3 in proportion while stirring;
[0010] Step 3: Start the ultrasonic dispersing equipment to ultrasonically disperse the raw materials to obtain a uniformly dispersed high and low temperature synchronous strengthening solution.
[0011] Preferably, the light-curable resin is 8602UV glue.
[0012] Preferably, the working parameters of the ultrasonic dispersion equipment are: ultrasonic power 200-560W, dispersion time 20-60min.
[0013] Preferably, the vacuum impregnation time is 15-30 minutes.
[0014] Preferably, the light curing method is: put the impregnated ceramic core into a UV curing box with 110mw / cm 2 UV light irradiation for 8-120s.
[0015] The present invention provides a method for simultaneous high and low temperature strengthening of a ceramic core. The method adopts a one-time strengthening scheme with a photocurable resin as a carrier and nano-SiO2, nano-Al2O3, and silicon nitride whiskers as high-temperature reinforcing agents, which significantly simplifies the strengthening process. In addition, since there is almost no thermal effect during the photocuring process, deformation, cracking, and the like of the thin-walled ceramic core during the thermal curing process are avoided. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work:
[0017] Figure 1 A schematic flow chart of a high-low temperature simultaneous strengthening method for a ceramic core provided by the present invention. DETAILED DESCRIPTION
[0018] The present invention will be further explained below in conjunction with specific implementation schemes, but the present invention is not limited thereto.
[0019] The ceramic core used in the precision casting process must meet the requirements of normal temperature wax compression fluid impact under precision casting conditions, high temperature casting metal liquid impact, and the ceramic core must be able to be effectively removed after the casting is completed. Among them, low-temperature strength and high-temperature strength are one of the most core indicators. The existing process adopts a step-by-step strengthening process of first high-temperature strengthening and then low-temperature strengthening. The process is cumbersome. In addition, heat curing treatment is required during low-temperature strengthening, which will cause deformation and cracking of the ceramic core. Traditional high-temperature strengtheners (generally silica sol or ethyl silicate hydrolyzate) belong to water-based systems, while traditional low-temperature strengtheners (generally epoxy resin or varnish) belong to oily systems. The two strengtheners are insoluble in each other and cannot achieve simultaneous high and low temperature strengthening.
[0020] In view of the existing problems, the present invention provides a high-low temperature synchronous strengthening method for a ceramic core, comprising: immersing the ceramic core to be strengthened into a high-low temperature synchronous strengthening solution for vacuum impregnation; performing photocuring on the impregnated ceramic core to finally obtain a strengthened ceramic core;
[0021] Specifically, the preparation method of the high-low temperature simultaneous strengthening solution comprises: weighing the following raw materials in the following proportions: 40-60wt% of a photocurable resin (one of 8602UV glue, K2018 UV glue, and 9310UV glue), 1-50wt% of nano-SiO2, 1-60wt% of nano-Al2O3, and 0.1-1wt% of silicon nitride whiskers. First, the photocurable resin (such as 8602UV glue) is placed in an ultrasonic dispersion device, and silicon nitride whiskers, nano-SiO2, and nano-Al2O3 are added in proportion while stirring, and the ultrasonic dispersion device is started, the ultrasonic power is controlled at 200-560W, and the dispersion time is 20-60min, so as to obtain a uniformly dispersed high-low temperature simultaneous strengthening solution.
[0022] Put an appropriate amount of the above-mentioned high and low temperature simultaneous strengthening solution in the sample tank, immerse the ceramic core to be strengthened in the strengthening solution, then place the sample tank in a vacuum box to evacuate the vacuum, and keep it in the vacuum state for 15-30 minutes before taking it out.
[0023] The ceramic core is placed in a UV curing box with 110mw / cm 2 UV light irradiation for 8-120s to achieve curing and complete the strengthening process.
[0024] The high-low temperature synchronous strengthening process of the ceramic core provided by the present invention achieves the high-low temperature synchronous strengthening of the ceramic core by dispersing silicon nitride whiskers, nano-SiO2, and nano-Al2O3 powders into a photocurable resin, which significantly simplifies the process and working hours. Specifically, the low-temperature strength of the ceramic core is improved by the photocurable resin, and at the same time, the nano-SiO2, nano-Al2O3, and silicon nitride whiskers impregnated into the ceramic core significantly improve the high-temperature strength of the ceramic core by promoting the high-temperature resistant quartz crystal transformation, sealing pores, and fiber toughening. The photocurable resin can not only play the role of a dispersant, allowing the silicon nitride whiskers, nano-SiO2, and nano-Al2O3 powders to smoothly enter the pores of the ceramic core, but also play a role in improving the low-temperature strength of the ceramic core. At the same time, the silicon nitride whiskers entering the ceramic core play a role in fiber toughening, the nano-SiO2 plays a role in promoting the high-temperature resistant quartz crystal transformation, and the nano-Al2O3 plays a role in sealing pores. The three materials work together to maximize the high-temperature strength of the ceramic core.
[0025] Example 1
[0026] Preparation of high and low temperature simultaneous strengthening solution: weigh the following raw materials according to the following ratio: 60wt% of photocurable resin 8602UV glue, 38.9wt% of nano-SiO2, 1wt% of nano-Al2O3, and 0.1wt% of silicon nitride whisker. First, put the photocurable resin 8602UV glue into the ultrasonic dispersion equipment, add silicon nitride whisker, nano-SiO2, and nano-Al2O3 in proportion while stirring, start the ultrasonic dispersion equipment, control the ultrasonic power at 200W, and the dispersion time is 50min to obtain a uniformly dispersed high and low temperature simultaneous strengthening solution.
[0027] Vacuum impregnation strengthening: put an appropriate amount of the above high and low temperature simultaneous strengthening solution into the sample tank, immerse the ceramic core to be strengthened into the strengthening solution, then place the sample tank in a vacuum box to evacuate the vacuum, and keep it in the vacuum state for 15 minutes before taking it out.
[0028] Light curing: The ceramic core is placed in a UV curing box with 110mw / cm 2 Irradiate with UV light for 30 seconds to achieve curing and complete the strengthening process.
[0029] Example 2
[0030] Preparation of high and low temperature simultaneous strengthening solution: weigh the following raw materials according to the following ratio: 40wt% of photocurable resin 8602UV glue, 20wt% of nano-SiO2, 39.5wt% of nano-Al2O3, and 0.5wt% of silicon nitride whisker. First, put the photocurable resin (8602UV glue) into an ultrasonic dispersing device, add silicon nitride whisker, nano-SiO2, and nano-Al2O3 in proportion while stirring, start the ultrasonic dispersing device, control the ultrasonic power at 400W, and the dispersing time is 30min to obtain a uniformly dispersed high and low temperature simultaneous strengthening solution.
[0031] Vacuum impregnation strengthening: put an appropriate amount of the above-mentioned high and low temperature simultaneous strengthening solution into the sample tank, immerse the ceramic core to be strengthened into the strengthening solution, then place the sample tank into a vacuum box to evacuate the vacuum, and keep it in the vacuum state for 20 minutes before taking it out.
[0032] Light curing: The ceramic core is placed in a UV curing box with 110mw / cm 2 UV light is irradiated for 50 seconds to achieve curing and complete the strengthening process.
[0033] Example 3
[0034] Preparation of high and low temperature simultaneous strengthening solution: weigh the following raw materials according to the following ratio: 50wt% of light-curing resin (8602UV glue), 15wt% of nano-SiO2, 34wt% of nano-Al2O3, and 1wt% of silicon nitride whisker. First, put the light-curing resin (8602UV glue) into an ultrasonic dispersing device, add silicon nitride whisker, nano-SiO2, and nano-Al2O3 in proportion while stirring, start the ultrasonic dispersing device, control the ultrasonic power at 560W, and the dispersing time is 20min to obtain a uniformly dispersed high and low temperature simultaneous strengthening solution.
[0035] Vacuum impregnation strengthening: put an appropriate amount of the above-mentioned high and low temperature simultaneous strengthening solution into the sample tank, immerse the ceramic core to be strengthened into the strengthening solution, then place the sample tank in a vacuum box to evacuate the vacuum, and keep it in the vacuum state for 30 minutes before taking it out.
[0036] Light curing: The ceramic core is placed in a UV curing box with 110mw / cm 2 The UV light is irradiated for 120 seconds to achieve curing and complete the strengthening process.
[0037] The strength comparison between the process of the present invention and the existing process is shown in the following table:
[0038]
[0039] The detailed description of the present invention is written in a progressive manner, emphasizing the differences between the various implementations, and similar parts thereof can be referred to each other.
[0040] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for simultaneously strengthening a ceramic core at high and low temperatures, characterized in that: include: Immersing the ceramic core to be strengthened into a high-low temperature simultaneous strengthening solution for vacuum impregnation; The impregnated ceramic core is light-cured to finally obtain a strengthened ceramic core; The method for preparing the high and low temperature simultaneous strengthening solution comprises: Step 1: According to the mass percentage, weigh the following raw materials according to the following ratio: photocurable resin 40-60wt%, nano-SiO2 1-50wt%, nano-Al2O3 1-60wt%, silicon nitride whisker 0.1-1wt%; Step 2: Place the photocurable resin into an ultrasonic dispersing device, and add silicon nitride whiskers, nano-SiO2, and nano-Al2O3 in proportion while stirring; Step 3: Start the ultrasonic dispersing equipment to ultrasonically disperse the raw materials to obtain a uniformly dispersed high and low temperature synchronous strengthening solution.
2. The high and low temperature simultaneous strengthening method of a ceramic core according to claim 1, characterized in that: The light-curable resin is 8602UV glue.
3. The high and low temperature simultaneous strengthening method of a ceramic core according to claim 1, characterized in that: The working parameters of the ultrasonic dispersion equipment are: ultrasonic power 200-560W, dispersion time 20-60min.
4. The high and low temperature simultaneous strengthening method of a ceramic core according to claim 1, characterized in that: The vacuum impregnation time is 15-30 minutes.
5. The high and low temperature simultaneous strengthening method of a ceramic core according to claim 1, characterized in that: The light curing method is as follows: the impregnated ceramic core is placed in a UV curing box with 110 mw / cm 2 UV light irradiation for 8-120s.
Citation Information
Patent Citations
Ceramic core reinforcer as well as preparation method and application method thereof
CN107986819A