Ligand of polyketone resin polymerization catalyst as well as preparation method and application of ligand
By using 1,1-bis[bis(2-methoxyphenyl)phosphinemethyl]cyclopropane as bistotin phosphine ligand, the problem of poor activity and thermal stability of polyketone resin catalysts was solved, and the catalytic reaction was improved Rate and efficiency achieve cost reduction and industrial application prospects.
Patent Information
- Application Number
- CN202411157091.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The existing polyketone resin polymerization catalysts have low ligand activity, poor thermal stability and complex synthesis.
1,1-bis[bis(2-methoxyphenyl)phosphine methyl]cyclopropane is used as bistooth phosphine ligand, and is prepared by chlorination reaction and substitution reaction, and is used for the production of palladium-based catalyst polyketone. Improve catalytic reaction rate and thermal stability.
High polymerization reaction rate and catalyst efficiency are achieved, and catalytic activity is maintained for a long time, reducing synthesis cost and complexity.
Smart Images

Figure BDA0005005309050000011 
Figure BDA0005005309050000021 
Figure BDA0005005309050000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a ligand of a polyketone resin polymerization catalyst and a preparation method and application thereof. Background Art
[0002] Polyketone is an engineering plastic whose main molecular chain is formed by carbon and hydrogen through high crystallization to form a tight crystalline structure. As a new green polymer material synthesized from carbon monoxide and olefins (ethylene, propylene), it has high impact strength. Compared with Nylon, the impact strength of PBT is 230% higher. The wear resistance of polyketone is 14 times that of POM. It has hydrocarbon barrier properties, and its gas barrier properties are equivalent to EVOH. Its chemical resistance allows it to remain stable in acids and alkalis (except strong acids and alkalis). Its strain capacity, recoverability, and toughness and rigidity balance are all higher than other engineering plastics such as POM and PA66. Since the synthetic raw materials of polyketone include carbon monoxide, one of the main sources of air pollution, and some grades can be degraded, it is a new green polymer material with broad development prospects in energy conservation and environmental friendliness.
[0003] The polymerization catalyst used to prepare polyketones usually consists of a system of Pd(II) / bidentate phosphine ligand / acid. The bisphosphine ligands with high catalytic activity used include 1,3-bis[bis(2-methoxyphenyl)phosphino]propane, ((2,2-dimethyl-1,3-dioxane-5,5-diyl)bis(methylene))bis(bis(2-methoxybenzene)phosphine), 33-bis-[bis-(2-methoxyphenyl)phosphinomethyl]-1,5-dioxa-spiro[5,5]undecane, etc. These ligands have problems such as low activity, poor thermal stability, and complex synthesis. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a ligand for a polyketone resin polymerization catalyst and a preparation method and application thereof, so as to solve the problems of low ligand activity, poor thermal stability and complex synthesis of the polyketone resin polymerization catalyst in the prior art.
[0005] In order to achieve the above-mentioned purpose and other related purposes, the present invention adopts the following technical solutions:
[0006] The first aspect of the present invention provides a ligand for a polyketone resin polymerization catalyst, wherein the ligand is 1,1-bis[di(2-methoxyphenyl)phosphinomethyl]cyclopropane, and its structural formula is shown in the following formula (I):
[0007]
[0008] The second aspect of the present invention provides a method for preparing the ligand of the above-mentioned polyketone resin polymerization catalyst, comprising the following steps:
[0009] (1) subjecting 1,1-cyclopropane dimethanol to a chlorination reaction with a chlorination reagent to obtain 1,1-dichloromethylcyclopropane;
[0010] (2) 1,1-dichloromethylcyclopropane is reacted with bis(2-methoxyphenyl)phosphine in the presence of a base to obtain 1,1-bis[bis(2-methoxyphenyl)phosphinomethyl]cyclopropane.
[0011] The third aspect of the present invention provides use of the above-mentioned ligand of the polyketone resin polymerization catalyst in the preparation of polyketone resin.
[0012] A fourth aspect of the present invention provides a polyketone resin polymerization catalyst, comprising a metal palladium catalyst, trifluoroacetic acid and a ligand of the polyketone resin polymerization catalyst.
[0013] The fifth aspect of the present invention provides use of the above-mentioned polyketone resin polymerization catalyst in the preparation of polyketone resin.
[0014] As described above, the ligand of the polyketone resin polymerization catalyst and the synthesis method thereof of the present invention have the following beneficial effects:
[0015] 1. The ligand of the polyketone resin polymerization catalyst provided by the present invention is a new bidentate phosphine ligand, which is used for the production of polyketone with a palladium-based catalyst. Compared with the existing catalytic system, the bidentate phosphine ligand catalytic system of the present invention is used for the polymerization reaction to synthesize polyketone, which can obtain a higher polymerization reaction rate and a higher catalyst efficiency (kg polyketone / g palladium). At the same time, it has higher thermal stability than other catalytic systems and can be stored for a longer time while maintaining catalytic activity.
[0016] 2. The method for preparing the ligand of the polyketone resin polymerization catalyst provided by the present invention adopts 1,1-cyclopropane dimethanol which is lower in cost and easily available as the synthetic raw material, and a novel bidentate phosphine ligand can be obtained through two-step reactions of chlorination and substitution, which has lower cost, more convenient reaction and has prospects for industrial application. DETAILED DESCRIPTION
[0017] The ligand of the polyketone resin polymerization catalyst of the present invention and its preparation method and application are described in detail below.
[0018] The first aspect of the present invention provides a ligand for a polyketone resin polymerization catalyst, wherein the ligand is 1,1-bis[di(2-methoxyphenyl)phosphinomethyl]cyclopropane, and its structural formula is shown in the following formula (I):
[0019]
[0020] 1,1-bis[bis(2-methoxyphenyl)phosphinomethyl]cyclopropane, molecular weight 558.2. Since the two phosphines of the bisphosphine ligand will maintain a stable conformation away from each other due to steric hindrance when not coordinated, when coordinated with Pd, the huge steric hindrance of the methoxyphenyl group makes the thermal stability of the complex worse. When a rigid steric hindrance is added at a position two Cs away from P, the tendency of the two Ps to move away from each other due to the steric hindrance of the substituents can be suppressed, thereby improving the stability of the coordination structure. The 1,1-bis[bis(2-methoxyphenyl)phosphinomethyl]cyclopropane ligand provided by the present invention has a three-membered ring in the structural formula, which can achieve a better balanced steric hindrance effect due to its large ring rigidity, while minimizing the damage to stability. Therefore, compared with other ligand catalytic systems, it has higher thermal stability.
[0021] The second aspect of the present invention provides a method for preparing the ligand of the above-mentioned polyketone resin polymerization catalyst, comprising the following steps:
[0022] (1) subjecting 1,1-cyclopropane dimethanol to a chlorination reaction with a chlorination reagent to obtain 1,1-dichloromethylcyclopropane;
[0023] (2) 1,1-dichloromethylcyclopropane is reacted with bis(2-methoxyphenyl)phosphine in the presence of a base to obtain 1,1-bis[bis(2-methoxyphenyl)phosphinomethyl]cyclopropane.
[0024] In some embodiments of the present invention, in step (1), the chlorination agent is sulfonyl chloride. Preferably, the molar ratio of the sulfonyl chloride to the 1,1-cyclopropane dimethanol is 0.5 to 1.5:1, can be 0.5 to 1:1, or can be 1 to 1.5:1.
[0025] In some embodiments of the present invention, in step (1), the chlorination reaction is carried out in an organic solvent; the organic solvent is selected from dichloromethane or dichloroethane.
[0026] In some embodiments of the present invention, in step (1), the chlorination reagent is diluted with a solvent and then added dropwise to the reaction system. Preferably, the solvent used for dilution is the same as the solvent of the reaction system.
[0027] In some embodiments of the present invention, in step (1), the temperature of the chlorination reaction is 0-40°C, which can be 0-5°C, 5-10°C, 10-15°C, 15-20°C, 20-25°C, 25-30°C, 30-35°C, or 35-40°C; preferably 20-25°C.
[0028] In some embodiments of the present invention, in step (1), the chlorination reaction time is 1 to 2 hours, can be 1 to 1.5 hours, or can be 1.5 to 2 hours; preferably 1.5 hours.
[0029] In some embodiments of the present invention, in step (1), after the reaction is completed, water is added for quenching; after quenching, the water in the reaction solution is usually separated.
[0030] In some embodiments of the present invention, step (1) further comprises washing the product obtained by the reaction, removing water and solvent. Preferably, the washing medium is an alkaline aqueous solution, and the alkaline aqueous solution is selected from an aqueous potassium carbonate solution, an aqueous sodium carbonate solution, an ammonium chloride solution, an aqueous sodium hydroxide solution or an aqueous potassium hydroxide solution, preferably an aqueous sodium carbonate solution; preferably, the method for removing water and solvent is vacuum distillation, and the vacuum distillation is preferably rotary distillation.
[0031] In some embodiments of the present invention, in step (2), the substitution reaction is carried out in an anhydrous and oxygen-free environment.
[0032] In some embodiments of the present invention, in step (2), the substitution reaction is carried out in an organic solvent; the organic solvent is an aprotic polar solvent, preferably, the organic solvent is N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), dimethyl sulfoxide (DMSO), N-methyl-2-pyrrolidone (NMP) or sulfolane.
[0033] In some embodiments of the present invention, in step (2), the base is selected from sodium tert-butoxide. Preferably, the molar ratio of the sodium tert-butoxide to the bis(2-methoxyphenyl)phosphine is 2 to 3.5:1, and can be 2 to 2.5:1, 2.5 to 3:1, or 3 to 3.5:1.
[0034] In some embodiments of the present invention, in step (2), the molar ratio of bis(2-methoxyphenyl)phosphine to 1,1-bischloromethylcyclopropane is 1.5-2:1, and can be 1.5-1.6:1, 1.6-1.7:1, 1.7-1.8:1, 1.8-1.9:1, or 1.9-2:1.
[0035] In some embodiments of the present invention, in step (2), the temperature of the substitution reaction is 45-80°C, and can be 45-50°C, 50-55°C, 55-60°C, 60-65°C, 65-70°C, 70-75°C, or 75-80°C.
[0036] In some embodiments of the present invention, in step (2), the substitution reaction time is 2 to 6 hours, which can be 2 to 2.5 hours, 2.5 to 3 hours, 3 to 3.5 hours, 3.5 to 4 hours, 4 to 4.5 hours, 4.5 to 5 hours, 5 to 5.5 hours, or 5.5 to 6 hours.
[0037] In some embodiments of the present invention, in step (2), after the reaction is completed, extraction, washing, drying, concentration and purification are also included. Preferably, the extractant for the extraction is water and an organic solvent; further preferably, the organic solvent used for the extractant is selected from any one or more combinations of dichloromethane, dichloroethane, ethyl acetate, methyl acetate, toluene, and xylene. In some specific embodiments of the present invention, the washing medium is a 30% to 60% methanol aqueous solution; in some specific embodiments of the present invention, the drying temperature is 60 to 120°C, which can be 60 to 70°C, 70 to 80°C, 80 to 90°C, 90 to 100°C, 100 to 110°C, and can also be 110 to 120°C; the drying time is 5 to 30 minutes, which can be 5 to 10 minutes, 10 to 15 minutes, 15 to 20 minutes, 20 to 25 minutes, and can also be 25 to 30 minutes; in some specific embodiments of the present invention, the purification includes recrystallization and drying, and preferably, the solvent used for the recrystallization is methanol.
[0038] The third aspect of the present invention provides use of the ligand of the polyketone resin polymerization catalyst in the preparation of polyketone resin.
[0039] The fourth aspect of the present invention provides a polyketone resin polymerization catalyst, comprising a metal palladium catalyst, trifluoroacetic acid and a ligand of the polyketone resin polymerization catalyst. In some embodiments of the present invention, the metal palladium catalyst is palladium acetate. Preferably, the molar ratio of the catalyst palladium acetate to the ligand 1,1-bis[di(2-methoxyphenyl)phosphinomethyl]cyclopropane is 0.5 to 1.5:1, can be 0.5 to 1:1, can also be 1 to 1.5:1, preferably 0.85:1.
[0040] The fifth aspect of the present invention provides the use of the above polyketone resin polymerization catalyst in the preparation of polyketone resin. The ligand catalyst system provided by the present invention has a higher catalytic efficiency than the existing ligand catalyst system and can exist relatively stably and maintain catalytic activity.
[0041] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0042] The specific embodiments of the present invention are further described in detail below in conjunction with preferred embodiments. When the embodiments provide numerical ranges, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, as those skilled in the art grasp the prior art and record the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.
[0043] Example 1
[0044] This embodiment provides a method for preparing a ligand of a polyketone resin polymerization catalyst, using 1,1-cyclopropane dimethanol as a starting material, and obtaining a target product through a two-step reaction of chlorination and substitution, and the reaction formula is as follows:
[0045]
[0046] The specific steps include:
[0047] Step 1: Dissolve 5.10g 1,1-cyclopropane dimethanol (0.05mol) in 150mL dichloromethane, take 14.8g sulfonyl chloride (0.11mol) and add it to 75mL dichloromethane to dilute it 5 times and then slowly add it to the reaction. During the dropwise addition, control the temperature below 40°C by water bath, stir the reaction for 1.5h, and then slowly add water to quench the reaction. Separate the water in the reaction solution, wash the organic phase with sodium carbonate aqueous solution again, and spin dry to obtain the oily product 1,1-dichloromethylcyclopropane (6.6g, yield 95%);
[0048] Step 2: Under anhydrous and oxygen-free conditions, 4.8g (1.5eq, 0.015mol) of bis(2-methoxyphenyl)phosphine was dissolved in 20g of DMF, and 3.4g (3.5eq, 0.035mol) of sodium tert-butoxide was added and stirred for 30min to complete the reaction. 1.4g (0.01mol) of 1,1-dichloromethylcyclopropane was dissolved in 40mL of DMF and slowly added dropwise to the reaction solution. After stirring for 30min, the temperature was raised to 60°C and reacted for 4h. After the reaction was completed, the solvent was recovered by vacuum distillation, and water and an organic solvent were added for extraction. The organic phase was collected, washed, dried, and concentrated to obtain a crude product; the crude product was recrystallized, and the solid was collected and dried to obtain the target product 1,1-bis[di(2-methoxyphenyl)phosphinomethyl]cyclopropane (light yellow solid, 5.1g, yield 91%).
[0049] 1HNMR(CDCl3): 7.29-7.15(m, 8H), 6.87-6.75(m, 8H), 3.7(s, 12H), 2.42(s, 4H), 0.3(s, 4H);
[0050] 31 P NMR (DMSO): -45.67 ppm.
[0051] Example 2
[0052] This embodiment provides a method for preparing a polyketone resin polymerization catalyst, which specifically comprises the following steps:
[0053] S1. Dissolve 21 mg of palladium acetate in 20 mL of acetone, add 0.11 mmol of the ligand prepared in Example 1, and stir at 25°C to dissolve.
[0054] S2. Add 75 μL of trifluoroacetic acid and stir for 1 hour to obtain a polyketone resin polymerization catalyst (in solution form).
[0055] Example 3
[0056] This embodiment provides a method for preparing a polyketone resin, which specifically comprises the following steps:
[0057] 200 mL of methanol and 1.2 mL of the polyketone resin polymerization catalyst prepared in Example 2 were added to a 250 mL reactor, and 9.5 g of the polyketone finished powder was added as a seed. The reactor was replaced with nitrogen 5 times, and then the temperature was raised to 90 ° C. A mixed gas of carbon monoxide and ethylene (molar ratio of 1:1) was introduced to make the pressure in the reactor reach 53 bar, and the reaction lasted for 7 hours. Finally, the reaction was terminated by cooling and depressurizing. The obtained polyketone powder 1 (excluding 9.5 g of seeds) was collected, the molecular weight was determined, and the catalytic efficiency 1 was calculated.
[0058] Stability test: A polyketone resin polymerization catalyst (in solution form) was prepared by the same preparation method as in Example 2. After the catalyst was allowed to stand for a day and a night, a polyketone resin was prepared by the same preparation method as in Example 3, using the polyketone resin polymerization catalyst. The polyketone powder obtained (excluding 9.5 g of seeds) was collected, the molecular weight was determined, and the catalytic efficiency 2 was calculated.
[0059] Comparative Example 1
[0060] In this comparative example, 9 different catalyst ligands were prepared.
[0061] (1) Using the bromide represented by formula A as a raw material, ligand 1-5 is prepared by the following reaction:
[0062]
[0063] Wherein, according to the different groups R1, the brominated raw materials represented by formula A are shown in the following Table 1.
[0064] Table 1 Preparation of ligands 1 to 5 Brominated compounds represented by formula A
[0065] A Ligand 1 1,3-Dibromopropane Ligand 2 1,3-Dibromo-2,2-dimethylpropane Ligand 3 1,1-Bis(bromoethyl)cyclohexane Ligand 4 1,1-Bis(bromoethyl)cycloheptane Ligand 5 Bis(bromomethyl)ether
[0066] Under anhydrous and oxygen-free conditions, 1.0g of bis(2-methoxyphenyl)phosphine was dissolved in 11g of DMF in a water bath at room temperature to obtain a colorless transparent liquid, 0.5g of sodium tert-butoxide was added, and stirring was continued for one hour. Under anhydrous and oxygen-free conditions, 2.6mmol of the bromide raw material shown in formula A was dissolved in 5.3g of DMF at room temperature and slowly added dropwise to the reaction solution, and the temperature was controlled between 20 and 25°C throughout the process. After stirring for 30min, the temperature was raised to 60°C and reacted for 4h. 10mL of water and 10mL of toluene were added to the reaction for extraction. After stirring and standing, the upper and lower layers were separated, and the upper toluene phase was collected and washed with water several times, and then anhydrous sodium sulfate was added to dry it. The toluene solution was distilled under reduced pressure to recover toluene to obtain a crude product. Methanol was added to distill it out azeotropically with toluene, and a solid product, i.e., ligand 1-5, was obtained after drying and cooling.
[0067] (2) Using the ketone compound represented by formula B as a raw material, ligand 6-9 is prepared by the following reaction:
[0068]
[0069]
[0070] Among them, according to the different groups R2, the ketone compounds represented by formula B and the brominated compounds represented by formula C are shown in the following Table 2.
[0071] Table 2 Preparation of Ligands 6 to 9 Ketone compounds represented by Formula B and brominated compounds represented by Formula C
[0072] B C Ligand 6 Cyclohexanone 3,3-Bis(bromoethyl)-1,5-dioxazolo[5.5]undecane Ligand 7 Cyclododecanone 3,3-Bis(bromoethyl)-1,5-dioxazolo[5.11]heptadecane Ligand 8 acetone 5,5-Bis(bromoethyl)-2,2-dimethyl-1,3-dioxolane Ligand 9 3-Pentanone 5,5-Bis(bromoethyl)-2,2-diethyl-1,3-dioxolane
[0073] Under nitrogen atmosphere, 2,2-(bromomethyl)propane-1,3-diol (1 g, 3.8 mmol) was dissolved in 15 g of dichloromethane. 5.7 mmol of the ketone compound raw material shown in formula B was added to the mixture and cooled until the internal temperature reached 0 to 5°C. While maintaining the internal temperature, 0.1 g of concentrated sulfuric acid was added, and then the mixture was stirred at an internal temperature of 0 to 5°C for 2 hours. The obtained mixture was washed twice with an aqueous solution containing sodium bicarbonate, then washed with water, and then dried with anhydrous sodium sulfate, and the solvent was removed by distillation under reduced pressure to obtain the intermediate brominated compound shown in formula C. The intermediate brominated compound shown in formula C was dissolved in DMF solvent, and then reacted and purified according to the preparation method of ligand 1-5 to obtain ligand 6-9.
[0074] Ligand 1: {3-[bis(2-methoxyphenyl)phosphino]propyl}bis(2-methoxyphenyl)phosphine; 1 HNMR(CDCl3): 7.24-7.17(m, 8H), 6.85-6.71(m, 8H), 3.72(s, 12H), 2.51(d, 4H), 1.34(s, 2H);
[0075] Ligand 2: {3-[bis(2-methoxyphenyl)phosphino]-2,2-dimethylpropyl}bis(2-methoxyphenyl)phosphine; 1 HNMR(CDCl3): 7.23-7.16(m, 8H), 6.81-6.73(m, 8H), 3.70(s, 12H), 2.53(d, 4H), 1.25(s, 6H);
[0076] Ligand 3: [(1-{[bis(2-methoxyphenyl)phosphino]methyl}cyclohexyl)methyl]bis(2-methoxyphenyl)phosphine; 1 HNMR(CDCl3): 7.28-7.14(m, 8H), 6.84-6.71(m, 8H), 3.72(s, 12H), 2.53(d, 4H), 1.24(s, 10H);
[0077] Ligand 4: [(1-{[bis(2-methoxyphenyl)phosphino]methyl}cycloheptyl)methyl]bis(2-methoxyphenyl)phosphine; 1 HNMR(CDCl3): 7.23-7.14(m, 8H), 6.81-6.72(m, 8H), 3.70(s, 12H), 2.55(d, 4H), 1.25(s, 12H);
[0078] Ligand 5: ({[bis(2-methoxyphenyl)phosphino]methoxy}methyl)bis(2-methoxyphenyl)phosphine; 1 HNMR(CDCl3): 7.23-7.16(m, 8H), 6.81-6.73(m, 8H), 3.91(d, 4H), 3.70(s, 12H);
[0079] Ligand 6: [(3-{[bis(2-methoxyphenyl)phosphino]methyl}-1,5-dioxaspiro[5.5]undec-3-yl)methyl]bis(2-methoxyphenyl)phosphine; 1 HNMR(CDCl3): 7.23-7.26(m, 8H), 6.85-6.85(m, 8H), 3.92(s, 4H), 3.72(s, 12H), 2.54(d, 4H), 1.44(s, 4H), 1.22(s, 6H);
[0080] Ligand 7: [(3-{[bis(2-methoxyphenyl)phosphino]methyl}-1,5-dioxaspiro[5.11]heptadecan-3-yl)methyl]bis(2-methoxyphenyl)phosphine; 1 HNMR(CDCl3): 7.26-7.16(m, 8H), 6.87-6.75(m, 8H), 3.72(s, 4H), 3.70(s, 12H), 2.51(d, 4H), 1.21-1.36(m, 18H);
[0081] Ligand 8: [(5-{[bis(2-methoxyphenyl)phosphino]methyl}-2,2-dimethyl-1,3-dioxan-5-yl)methyl]bis(2-methoxyphenyl)phosphine; 1 HNMR(CDCl3): 7.26-7.16(m, 8H), 6.87-6.75(m, 8H), 3.92(s, 4H), 3.70(s, 12H), 2.51(d, 4H), 1.44(s, 6H);
[0082] Ligand 9: [(5-{[bis(2-methoxyphenyl)phosphino]methyl}-2,2-diethyl-1,3-dioxan-5-yl)methyl]bis(2-methoxyphenyl)phosphine; 1 HNMR (CDCl3): 7.26-7.16 (m, 8H), 6.87-6.75 (m, 8H), 3.92 (s, 4H), 3.70 (s, 12H), 2.51 (d, 4H), 1.43 (s, 4H), 1.28 (s, 6H).
[0083] Comparative Example 2
[0084] This comparative example adopts the same operation as Example 2, except that the ligand prepared in Example 1 is replaced by 9 different catalyst ligands prepared in Comparative Example 1 to prepare 9 catalysts.
[0085] Comparative Example 3
[0086] This comparative example adopts the same operation as Example 3, except that the 9 catalysts prepared in Comparative Example 2 are used to replace the polyketone resin polymerization catalyst prepared in Example 2, and the obtained polyketone powder 1 (excluding 9.5g of seeds) is collected, the molecular weight is measured and the catalytic efficiency 1 is calculated.
[0087] Stability test: The 9 different catalyst ligands prepared in Comparative Example 1 were respectively used to prepare catalysts (in solution form) using the same preparation method as in Comparative Example 2. After the obtained catalysts were allowed to stand for a day and a night, the same preparation method as in Example 3 was used to prepare polyketone resin using the catalyst as a polyketone catalyst. The polyketone powder obtained (excluding 9.5 g of seeds) was collected, the molecular weight was measured, and the catalytic efficiency 2 was calculated.
[0088] The polyketone resins, catalytic efficiency and stability obtained in the above examples and comparative examples are shown in Table 3 below.
[0089] Table 3 Polyketone resins, catalytic efficiency and stability obtained in Examples and Comparative Examples
[0090]
[0091] As shown in Table 3, as the steric hindrance of the bridge structure in the phosphine ligand continues to increase, the catalytic efficiency of the obtained catalyst is limited, but the stability of the catalyst decreases rapidly. Only the bridge structure with moderate steric hindrance can improve the catalytic efficiency while making the complex catalyst relatively stable and maintain catalytic activity. This is because the two phosphines of the diphosphine ligand will maintain a stable conformation away from each other due to steric hindrance when they are not coordinated. After coordination with Pd, the huge steric hindrance of the methoxyphenyl group makes the thermal stability of the complex worse. When a rigid steric hindrance is added to the position two Cs away from P, the tendency of the two Ps to move away from each other due to the steric hindrance of the substituents can be suppressed, thereby improving the stability of the coordination structure. Since the distance between the substituent of the bridge structure and one P is less than the distance between P and P, when the steric hindrance of the substituent of the bridge structure is too large, the ligand changes its conformation to achieve chelation coordination with Pd, which will hinder the steric hindrance of the substituted group, making the coordination structure unstable and easy to decompose. When the substituent added to the bridge structure at the center of the ligand is a 3-6-membered ring, the trend of decreasing thermal stability is not obvious. Among several ligands, the three-membered ring can play a better balanced steric effect due to its greater ring rigidity, while at the same time causing the least damage to stability. At the same time, the raw materials of the three-membered ring are easier to obtain than the four-membered ring or even the six-membered ring, and have good economic benefits.
[0092] In summary, the present invention effectively overcomes various shortcomings of the prior art and has high industrial utilization value.
[0093] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A ligand for a polyketone resin polymerization catalyst, characterized in that: The ligand is 1,1-bis[di(2-methoxyphenyl)phosphinomethyl]cyclopropane, and its structural formula is shown in the following formula (I):
2. A method for preparing a ligand of a polyketone resin polymerization catalyst as claimed in claim 1, characterized in that: The steps include: (1) subjecting 1,1-cyclopropane dimethanol to a chlorination reaction with a chlorination reagent to obtain 1,1-dichloromethylcyclopropane; (2) 1,1-dichloromethylcyclopropane is reacted with bis(2-methoxyphenyl)phosphine in the presence of a base to obtain 1,1-bis[bis(2-methoxyphenyl)phosphinomethyl]cyclopropane.
3. The method for preparing a ligand of a polyketone resin polymerization catalyst according to claim 2, characterized in that: In step (1), one or more of the following features are included: (1a) The chlorination agent is sulfonyl chloride; (1b) the chlorination reaction is carried out in an organic solvent; (1c) the chlorination reagent is diluted with a solvent and then added dropwise to the reaction system; (1d) The temperature of the chlorination reaction is 0 to 40° C.; (1e) The chlorination reaction time is 1 to 2 hours; (1f) after the reaction is completed, water is added to quench the reaction; (1g) The process also includes washing the product obtained by the reaction and removing water and solvent.
4. The preparation method according to claim 3, characterized in that: In step (1), one or more of the following features are included: (1a1) the molar ratio of the sulfonyl chloride to the 1,1-cyclopropane dimethanol is 0.5 to 1.5:1; (1b1) the organic solvent is selected from dichloromethane or dichloroethane; (1c1) The solvent used for dilution is the same as the solvent of the reaction system; (1g1) The washing medium is an alkaline aqueous solution; (1g2) The method for removing water and solvent is distillation under reduced pressure.
5. The method for preparing a ligand of a polyketone resin polymerization catalyst according to claim 2, characterized in that: In step (2), one or more of the following features are included: (2a) The substitution reaction is carried out in an anhydrous and oxygen-free environment; (2b) the substitution reaction is carried out in an organic solvent; (2c) the base is selected from sodium tert-butoxide; (2d) the molar ratio of bis(2-methoxyphenyl)phosphine to 1,1-bischloromethylcyclopropane is 1.5 to 2:1; (2d) The temperature of the substitution reaction is 45 to 80° C.; (2e) The substitution reaction time is 2 to 6 hours; (2f) After the reaction is completed, it also includes extraction, washing, drying, concentration and purification.
6. The method for preparing a ligand of a polyketone resin polymerization catalyst according to claim 5, characterized in that: In step (2), one or more of the following features are included: (2b1) The organic solvent is an aprotic polar solvent, preferably any one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone and sulfolane; (2c1) the molar ratio of the sodium tert-butoxide to the bis(2-methoxyphenyl)phosphine is 2 to 3.5:1; (2f1) The extraction agent of the extraction is water and an organic solvent; (2f2) the washing medium is water; (2f3) The drying temperature is 60 to 120° C. and the drying time is 5 to 30 minutes; (2f4) The purification includes recrystallization and drying.
7. The method for preparing a ligand of a polyketone resin polymerization catalyst according to claim 6, characterized in that: In step (2), one or more of the following features are included: (2f11) the organic solvent used as the extractant is selected from one or more combinations of dichloromethane, dichloroethane, ethyl acetate, methyl acetate, toluene and xylene; (2f41) The solvent used for the recrystallization is methanol.
8. Use of the ligand of the polyketone resin polymerization catalyst as claimed in claim 1 in the preparation of polyketone resin.
9. A polyketone resin polymerization catalyst, characterized in that The invention comprises a metal palladium catalyst, trifluoroacetic acid and a ligand of the polyketone resin polymerization catalyst as claimed in claim 1.
10. Use of the polyketone resin polymerization catalyst according to claim 9 in the preparation of polyketone resin.
Citation Information
Patent Citations
Ligand for polyketone polymerization catalyst and preparation method thereof
CN114149464A
Catalyst ligand as well as preparation method and application thereof
CN116535441A
Macrocyclic diphosphine ligand as well as preparation method and application thereof
CN118146264A
Process for preparing polyketones
EP0619334A1