Anti-aging modified anti-sagging resin as well as preparation method and coating thereof
By reacting benzophenone ultraviolet absorber with polyurea compounds to generate polyurea crystals, the problems of single and poor stability of traditional anti-sag resins are solved, and efficient anti-aging and anti-sag properties are achieved, which simplifies the Production processes and reduce environmental and health risks.
Patent Information
- Application Number
- CN202411212316.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional anti-sag resins have problems with single performance and poor stability during long-term use, and the direct addition of anti-aging agents may lead to incompatibility, affect sag performance, and potential harm to the environment and health.
Benzophenone-based ultraviolet absorbers are used as the synthetic raw material for anti-sag resins. Polyurea crystals are generated by reacting with polyurea compounds to avoid volatile problems and enhance anti-aging properties, ensuring compatibility with coatings.
It significantly improves the anti-aging and sag properties of the resin, extends the service life, simplifies the production process, reduces environmental pollution and health risks, and improves product quality and production efficiency.
Smart Images

Figure CN119039554A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coating additives, and in particular relates to an anti-aging modified anti-sagging resin and a preparation method thereof, and a coating. Background Art
[0002] Resin materials are widely used in coatings, composite materials, electronic packaging and construction. These applications require high aging resistance of resins to ensure the long-term stability and service life of products. However, resins will be affected by environmental factors (such as ultraviolet rays, temperature, humidity, etc.) during long-term use, resulting in gradual performance decline, embrittlement, color change and reduced mechanical properties.
[0003] In order to improve the aging properties of the resin, antioxidants, modifiers or other functional additives are usually added to it. However, these additives may be at risk of being incompatible with the coating resin matrix, which may lead to unstable performance, such as stratification or precipitation. In addition, the introduction of additives may also affect the processing properties of the resin, such as fluidity and curing speed, thereby affecting production efficiency and product quality. Since many antioxidants and modifiers are small molecule compounds and are volatile, they may have potential negative effects on the environment or human health during use and need to be carefully considered. In addition, the addition of new additives or modifiers may require adjustments to the production process of the coating, increasing the complexity of the process and the difficulty of management. Therefore, the research and introduction of new functional materials to replace traditional antioxidants and modifiers has become an urgent problem to be solved.
[0004] Paints with anti-sagging properties are a type of paint that has anti-sagging additives added to change its rheological properties. The main function of this type of paint is to prevent the paint from flowing when painting on vertical or inclined surfaces, resulting in uneven coating thickness or accumulation. The main principle of anti-sagging additives is to modify the resin matrix in the paint through polyurea compounds. The molecular structure of polyurea compounds easily forms hydrogen bonds, which makes the paint show higher viscosity when it is not subjected to or subjected to small external forces (such as slight gravity on a vertical surface), thereby reducing sagging. When a certain shear force is applied (such as during transportation or spraying), the hydrogen bonds are destroyed, and the resin shows lower viscosity and is easy to flow. Anti-sagging resins are mainly used for spraying large vertical surfaces or other applications that require anti-sagging. However, the anti-sagging resins currently on the market have a single performance. Although the initial performance has improved, aging, discoloration or performance degradation may occur during long-term use, affecting their long-term stability.
[0005] In summary, traditional anti-sagging resins have problems such as single performance and poor long-term stability. Directly adding antioxidants to coatings to improve their aging resistance will bring negative effects such as incompatibility, affect anti-sagging performance, pollute the environment and harm health. Summary of the invention
[0006] In view of the above technical problems, the present invention takes a new approach, using an anti-aging agent represented by a benzophenone ultraviolet light absorber as a synthetic raw material for an anti-sagging resin, i.e., a polyurea compound, so that the benzophenone ultraviolet light absorber exists in the form of polyurea crystals, thereby avoiding its volatilization risk and incompatibility with the coating, and also enhancing the anti-aging property of the anti-sagging resin. Therefore, the present invention provides an anti-aging modified anti-sagging resin, a preparation method thereof, and a coating.
[0007] To achieve the above object, the technical solution of the present invention is:
[0008] An anti-aging modified anti-sagging resin, calculated by weight, includes the following components:
[0009]
[0010] Preferably, the chemical structure of the primary amino-containing benzophenone is:
[0011]
[0012] Where R 1 —R 8 It is any one of the structures -H, -OH, -OCH3, -C4H9, -Cl and -OCH2CHOCH2, or any combination thereof; n=0-10.
[0013] Preferably, the chemical structure of the primary amino-containing benzophenone is:
[0014] That is, R1-R8 are all -H, n=0; or
[0015] That is, R2-R8 are all -H, R1=-OH, and n=1.
[0016] Preferably, the solvent is any one or more of xylene, S-100A high boiling point solvent or S-150 aromatic solvent.
[0017] Preferably, when the solvent is a mixed solvent of any two of xylene, S-100A high boiling point solvent or S-150 aromatic solvent, the arbitrary blending ratio is 1:0-10.
[0018] Preferably, the polymer resin is polyacrylic resin (PA) or / and polyester resin (PE).
[0019] Preferably, the isocyanate is hexamethylene diisocyanate (HDI) or / and diphenylmethane-4,4'-diisocyanate (MDI).
[0020] Based on the same inventive concept, the present invention also provides a method for preparing the anti-aging modified anti-sagging resin, comprising the following steps:
[0021] S1: mixing primary aminobenzhydrol with part of the solvent to prepare a primary aminobenzhydrol solution of a preset concentration;
[0022] S2: The polymer resin and the remaining solvent are mixed uniformly in a reaction kettle and stirred continuously, the temperature of the reaction system is maintained at 0-40° C., the primary aminobenzhydrol solution prepared in step S1 is dispersed into the reaction system, and diisocyanate is added and stirred to obtain the modified anti-sagging resin.
[0023] Based on the same inventive concept, the present invention also provides a coating, comprising the anti-aging modified anti-sagging resin.
[0024] Due to the adoption of the above technical solution, the present invention has the following advantages and positive effects compared with the prior art:
[0025] The modified anti-sagging resin provided by the present invention comprises a polymer resin, a solvent, a plurality of or a mixed diisocyanate, and a primary amino group-containing benzophenone. The primary amino group-containing benzophenone is used as a polyurea raw material, and a primary amine and primary amino group in the molecular structure react with the diisocyanate to form a polyurea crystal, thereby achieving the anti-sagging function of the resin, so that the benzophenone ultraviolet light absorber exists in the form of polyurea crystals, and the benzophenone ultraviolet light absorber becomes a part of the polyurea structure, thereby avoiding the volatility problem of the small molecule compound of the benzophenone ultraviolet light absorber, thereby avoiding the problem of environmental pollution and health hazards, and is more environmentally friendly and safer than the prior art.
[0026] In addition, benzophenone ultraviolet light absorber exists in the form of polyurea crystals, and together with polymer resin, it constitutes polyurea resin. When added to the coating, due to the principle of like-is-compatible, it is evenly dispersed with the coating, thus avoiding the problems of stratification and precipitation between the anti-aging agent and the coating.
[0027] At the same time, the present invention introduces benzophenone into the polyurea resin in the form of a chemical bond, so that benzophenone becomes a group in the molecular structure of the polyurea, which not only does not affect the anti-sagging performance of the resin, but also significantly enhances the anti-aging ability of the resin, prolongs its service life, and makes the anti-sagging resin have both anti-sagging and anti-aging properties. It is added to the coating in the form of an additive, which brings the same function to the coating while avoiding the stratification and volatility problems of traditional anti-aging additives, and simplifies the coating production process. Compared with the prior art, the coating process complexity is reduced, and the production efficiency and product quality are improved.
[0028] The modified anti-sagging resin preparation method provided by the present invention is to add and disperse a solution containing primary amino benzophenone into a reaction system consisting of a polymer resin and a solvent, and then add diisocyanate to the reaction system for stirring and reacting, thereby improving the synthesis process of the resin and enhancing the consistency and stability of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The rheological properties test results of the resin of Example 1 of the present invention;
[0030] Figure 2 The rheological properties test results of the resin of Example 2 of the present invention;
[0031] Figure 3 The rheological properties test results of the resin of Example 3 of the present invention;
[0032] Figure 4 The rheological properties test results of the resin of Comparative Example 1 of the present invention are as follows;
[0033] Figure 5 The rheological properties test results of the resin of Comparative Example 2 of the present invention are as follows;
[0034] Figure 6 The following are the rheological properties test results of the resin of Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0035] The present invention introduces an anti-aging agent into the anti-sagging resin matrix by chemical bonding, overcomes the volatility and compatibility of the anti-aging agent, and improves the anti-aging performance of the anti-sagging resin, but it is important to select a suitable anti-aging agent that does not affect the anti-sagging performance of the anti-sagging resin. The present invention selects a benzophenone ultraviolet light absorber because the molecular structure of benzophenone is highly symmetrical and contains a rigid aromatic ring, which not only does not affect the polyurea crystal structure, but also improves the crystallinity of the polyurea, so a benzophenone containing a primary amino group is selected.
[0036] It should be noted that: the anti-aging agent currently on the market is generally an externally added small molecule compound, and these additives often have compatibility problems with the resin matrix, resulting in coatings being prone to stratification, precipitation and other phenomena during use, affecting the performance and quality of the product. In addition, the use of traditional anti-aging agents may also increase process complexity and reduce production efficiency. The present invention, by using primary amino-containing benzophenone as raw material, directly integrates anti-aging function into polyurea structure, solves this compatibility problem, achieves the high compatibility of resin and anti-aging agent, and simplifies the production process.
[0037] Most of the currently used anti-aging agents are volatile organic compounds (VOCs), which release harmful substances during use, not only polluting the environment, but also causing potential harm to human health. The presence of these volatile substances also affects the long-term stability of the resin, resulting in performance degradation. The present invention introduces a benzophenone ultraviolet light absorber into the polyurea resin in the form of a chemical bond, so that benzophenone becomes a group of the polyurea molecular structure, effectively reducing the volatility problem, providing a more environmentally friendly and safe solution, and significantly improving the durability and anti-aging performance of the resin.
[0038] Existing anti-sagging resins can effectively reduce sagging in the initial stage of use, but are prone to aging, discoloration and performance degradation during long-term use, affecting the service life of coating products. The present invention introduces primary amino benzophenone into the polyurea structure, which not only effectively improves the anti-sagging performance in the initial stage, but also significantly enhances the anti-aging ability of the resin, prolongs its long-term service life, and overcomes the shortcomings of the prior art.
[0039] The following is a further detailed description of an anti-aging modified anti-sagging resin and its preparation method and coating proposed by the present invention in conjunction with the accompanying drawings and specific embodiments. The advantages and features of the present invention will become more apparent from the following description.
[0040] Example 1: SA compound + HDI in PA resin
[0041] In a 1000mL dispersion tank equipped with a high-speed dispersion disk and a thermometer, 447.50g PA (solid content: 70.00%) and 72.83g xylene were added in sequence, nitrogen was introduced, and the mixture was stirred evenly at 1000rpm. When the temperature in the tank was 23°C, 15.28g (77.55mmol) of SA compound + 15g of xylene mixed solution was quickly added dropwise to the dispersion tank, and the mixture was stirred and dispersed at 4000rpm for 1 minute. Then 6.38g (37.93mmol) of HDI was added to the dispersion tank, the stirring rate was increased to 4000rpm, and the mixture was dispersed for 40 minutes to obtain an opaque thixotropic resin R1 with a fineness of ≤10μm. After sealing part of the R1 resin, it was placed in a 50°C water bath and stored under 20WUVA-340 lamp for 10 days, then taken out and marked as the resin R1' after hot storage with a fineness of ≤10μm.
[0042] The high shear (1000s) of resin R1 and R1' after 10 days of heat storage (50°C) and illumination (20W UVA-340) were measured by rotational rheometer. -1 ) and low shear viscosity (1s -1 ) changes and determine the shear factor.
[0043] Example 2 SA compound + HDI in PE resin
[0044] In a 1000mL dispersion tank equipped with a high-speed dispersion disk and a thermometer, 423.30g of PE (solid content: 72.00%) and 97.16g of xylene were added in sequence, nitrogen was introduced, and the mixture was stirred evenly at 1000rpm. When the temperature in the tank was 23°C, 15.28g (77.55mmol) of SA compound + 15g of xylene mixed solution was quickly added dropwise to the dispersion tank, and the mixture was stirred and dispersed at 4000rpm for 1 minute. Then 6.38g (37.93mmol) of HDI was added to the dispersion tank, the stirring rate was increased to 4000rpm, and the mixture was dispersed for 40 minutes to obtain an opaque resin R2 with a fineness of ≤10μm. After sealing part of the R2 resin, it was placed in a 50°C water bath and stored under 20W UVA-340 lamp for 10 days, marked as the resin R2' after hot storage, with a fineness of ≤10μm.
[0045] The high shear (1000s) of resin R2 and R2' after 10 days of heat storage (50°C) and illumination (20W UVA-340) were measured by rotational rheometer. -1 ) and low shear viscosity (1s -1 ) changes and determine the shear factor.
[0046] Example 3 SB compound + MDI in PA
[0047] In a 1000mL dispersion tank equipped with a high-speed dispersion disk and a thermometer, 447.50g of PA (solid content: 70.00%) and 72.83g of xylene were added in sequence, nitrogen was introduced, and the mixture was stirred evenly at 1000rpm. When the temperature in the tank was 23°C, 17.60g (77.55mmol) of SB compound + 15g of xylene mixed solution was quickly added dropwise to the dispersion tank, and the mixture was stirred and dispersed at 4000rpm for 1 minute. Then 9.49g (37.93mmol) of MDI was added to the dispersion tank, the stirring rate was increased to 4000rpm, and the mixture was dispersed at 4000rpm for 40 minutes to obtain an opaque thixotropic resin R3 with a fineness of ≤10μm. After sealing part of the R3 resin, it was placed in a 50°C water bath and stored under 20W UVA-340 lamp for 10 days, then taken out and marked as the resin R3' after hot storage with a fineness of ≤10μm.
[0048] The high shear (1000s) of resin R3 and R3' after 10 days of heat storage (50°C) and illumination (20W UVA-340) were measured by rotational rheometer. -1 ) and low shear viscosity (1s -1 ) changes and determine the shear factor.
[0049] Comparative Example 1: Benzylamine + HDI in PA
[0050] In a 1000mL dispersion tank equipped with a high-speed dispersion disk and a thermometer, 447.50g of PA (solid content: 70.00%) and 87.83g of xylene were added in sequence, nitrogen was introduced, and the mixture was stirred evenly at 1000rpm. When the temperature in the tank was 23°C, 8.31g (77.55mmol) of benzylamine was quickly added dropwise to the dispersion tank, and the mixture was stirred and dispersed at 4000rpm for 1 minute. Then 6.38g (37.93mmol) of HDI was added to the dispersion tank, the stirring rate was increased to 4000rpm, and the mixture was dispersed for 40 minutes to obtain an opaque thixotropic resin R4 with a fineness of ≤10μm. After sealing part of the R4 resin, the resin was placed in a 50°C water bath and stored under 20W UVA-340 lamp for 10 days, and then taken out and marked as the resin R4' after hot storage, and the fineness was measured to be ≤10μm.
[0051] The high shear (1000s) of resin R4 and R4' after 10 days of heat storage (50°C) and illumination (20W UVA-340) was measured by rotational rheometer. -1 ) and low shear viscosity (1s -1 ) changes and determine the shear factor.
[0052] Comparative Example 2: Benzylamine + HDI in PE
[0053] In a 1000mL dispersion tank equipped with a high-speed dispersion disk and a thermometer, 423.30g of PE (solid content: 72.00%) and 112.16g of xylene were added in sequence, nitrogen was introduced, and the mixture was stirred evenly at 1000rpm. When the temperature in the tank was 23°C, 8.31g (77.55mmol) of benzylamine was quickly added dropwise to the dispersion tank, and the mixture was stirred and dispersed at 4000rpm for 1 minute. Then 6.38g (37.93mmol) of HDI was added to the dispersion tank, the stirring rate was increased to 4000rpm, and the mixture was dispersed for 40 minutes to obtain an opaque resin R5 with a fineness of ≤10μm. After sealing part of the R5 resin, the resin was placed in a 50°C water bath and stored under 20W UVA-340 lamp for 10 days, and then taken out and marked as the resin R5' after hot storage, and the fineness was measured to be ≤10μm.
[0054] The high shear (1000s) of resin R5 and R5' after 10 days of heat storage (50°C) and illumination (20W UVA-340) were measured by rotational rheometer. -1 ) and low shear viscosity (1s -1 ) changes and determine the shear factor.
[0055] Comparative Example 3: Benzylamine + MDI in PA
[0056] In a 1000mL dispersion tank equipped with a high-speed dispersion disk and a thermometer, 447.50g of PA (solid content: 70.00%) and 87.83g of xylene were added in sequence, nitrogen was introduced, and the mixture was stirred evenly at 1000rpm. When the temperature in the tank was 23°C, 8.31g (77.55mmol) of benzylamine was quickly added dropwise to the dispersion tank, and the mixture was stirred and dispersed at 4000rpm for 1 minute. Then 9.49g (37.93mmol) of MDI was added to the dispersion tank, the stirring rate was increased to 4000rpm, and the mixture was dispersed at 4000rpm for 40 minutes to obtain an opaque thixotropic resin R6 with a fineness of ≤10μm. After sealing part of the R6 resin, the resin was placed in a 50°C water bath and stored under irradiation of a 20W UVA-340 lamp for 10 days, and then taken out and marked as the resin R6' after hot storage, and the fineness was measured to be ≤10μm.
[0057] The high shear (1000s) of resin R6 and R6' after 10 days of heat storage (50°C) and illumination (20W UVA-340) were measured by rotational rheometer. -1 ) and low shear viscosity (1s -1 ) changes and determine the shear factor.
[0058] The above-mentioned fineness test is measured in accordance with the national standard GB / T 1724-2019.
[0059] According to the conventional detection method in the art, the above resin is subjected to rheological behavior test
[0060] Test instrument model: Test conditions: 10# rotor, temperature: 25℃, speed is divided into two sections, the first section: 1000s -1 Cutting time: 5 minutes; second section: 1s -1 Cutting time 9 minutes.
[0061] Shear factor: Calculate according to the following formula: X = A0 / A1. Where A0 is the sample rotation speed of 1s -1 The viscosity at A1 is the sample speed of 1000s -1 The viscosity at .
[0062] The shear viscosity test results of the resins of Examples 1-3 and Comparative Examples 1-3 before and after heat storage are as follows: Figure 1-6 The rheological properties test results are shown in Table 1. Figure 1-3 It can be concluded that the obtained resin has anti-sagging performance before and after heat storage, indicating that the polyurea synthesized with primary aminobenzophenone as raw material can also have anti-sagging performance. Figure 1-6 It can be seen from the comparison that the shear viscosity of the resins in Examples 1-3 is basically unchanged before and after heat storage, while the shear viscosity of the resins in Comparative Examples 1-3 is reduced after heat storage.
[0063] Table 1 Test results of viscosity and shear factor of resin before and after heat storage of Examples 1-3 and Comparative Examples 1-3
[0064]
[0065]
[0066] By comparing the low shear viscosity and shear factor before and after thermal storage, it can be seen that the viscosity of Examples 1-3 does not change much after thermal storage and illumination, and the storage stability is good, while the viscosity of Comparative Examples 1-3 decreases significantly, and the storage stability is poor.
[0067] From the rheological results of the embodiments and comparative examples before and after heat storage and illumination in the attached drawings and Table 1, it can be seen that the low shear viscosity and shear factor of the comparative example change significantly, while the viscosity of the embodiments changes less, the storage stability is better, and the shear factor changes less than ±5% in 10 days under 50°C water bath and UVA-340 lamp irradiation. It is further explained that the polyurea resin provided by the present invention, which is formed by synthesizing polyurea crystals with diisocyanate using primary amino benzophenone as raw material, not only effectively improves the anti-sagging performance in the initial stage, but also significantly enhances the anti-aging ability of the resin and prolongs its long-term service life.
[0068] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Even if various changes are made to the present invention, if these changes fall within the scope of the claims of the present invention and their equivalents, they still fall within the protection scope of the present invention.
Claims
1. An anti-aging modified anti-sagging resin, characterized in that: Calculated by weight, it includes the following components:
2. The anti-aging modified anti-sagging resin according to claim 1, characterized in that: The chemical structure of the primary amino-containing benzophenone is: Where R 1 —R 8 It is any one of the structures -H, -OH, -OCH3, -C4H9, -Cl and -OCH2CHOCH2, or any combination thereof; n=0-10.
3. The anti-aging modified anti-sagging resin according to claim 2, characterized in that: The chemical structure of the primary amino-containing benzophenone is:
4. The anti-aging modified anti-sagging resin according to claim 1, characterized in that: The solvent is any one or more of xylene, S-100A high boiling point solvent or S-150 aromatic hydrocarbon solvent.
5. The anti-aging modified anti-sagging resin according to claim 4, characterized in that: When the solvent is a mixed solvent of any two of xylene, S-100A high boiling point solvent or S-150 aromatic hydrocarbon solvent, the arbitrary blending ratio is 1:0-10.
6. The anti-aging modified anti-sagging resin according to claim 1, characterized in that: The polymer resin is polyacrylic acid resin and / or polyester resin.
7. The anti-aging modified anti-sagging resin according to claim 1, characterized in that: The diisocyanate is hexamethylene diisocyanate or / and diphenylmethane-4,4'-diisocyanate.
8. A method for preparing the anti-aging modified anti-sagging resin according to any one of claims 1 to 7, characterized in that: The steps include: S1: mixing primary aminobenzhydrol with part of the solvent to prepare a primary aminobenzhydrol solution of a preset concentration; S2: The polymer resin and the remaining solvent are mixed uniformly in a reaction kettle and stirred continuously, the temperature of the reaction system is maintained at 0-40° C., the primary aminobenzhydrol solution prepared in step S1 is dispersed into the reaction system, and diisocyanate is added and stirred to obtain the modified anti-sagging resin.
9. A coating, characterized in that: The invention comprises the anti-aging modified anti-sagging resin according to any one of claims 1 to 7.