Self-healing type polymer elastomer material and application thereof in pressure sensor

By introducing dynamic disulfide bonds and acyl hydrazone bonds into polymer elastomer materials, combining antioxidants, self-healing and antioxidant properties are achieved, solving the problems of degradation and aging of traditional materials, and improving the stability of the sensor and Service life.

CN119039556APending Publication Date: 2024-11-29SUZHOU MOGAN ELECTRONIC TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411071528.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The performance of traditional pressure sensor materials decreases after long-term use or external damage, resulting in increased measurement errors or failures, and is susceptible to oxygen and ultraviolet rays, poor anti-aging performance, affecting stability and service life.

Method used

Using self-healing polymer elastomer materials, the antioxidant pentaerythritol tetra(3,5-di-tert-butyl-4-hydroxy)phenyl propionate is combined with the antioxidant pentaerythritol tetrahydric acid ester by introducing double reversible bonds of dynamic disulfide and acyl hydrazone bonds. , realize the self-healing and antioxidant properties of the material, and enhance the chemical crosslinking ability and compatibility.

Benefits of technology

The material can respond quickly and repair itself when damaged, extend its service life and improve reliability, effectively inhibit thermal oxygen aging, improve antioxidant performance, and is suitable for triboelectric pressure sensors and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039556A_ABST
    Figure CN119039556A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a self-healing polymer elastomer material, which comprises the following steps: S1, placing polydimethylsiloxane in a vacuum drying oven, vacuumizing and heating; s2, uniformly mixing polyethylene glycol and pentamethylene diisocyanate, and adding an organic bismuth catalyst to obtain a prepolymer; by introducing a double reversible bond containing a dynamic disulfide bond and an acylhydrazone bond, the material can quickly respond and self-repair when damaged, the dynamic disulfide bond can be broken and recombined under proper conditions, physical crosslinking and decrosslinking of the material are realized, the original performance of the material is further recovered, and by introducing an aldehyde-containing polymer, an aldehyde group can react with a hydrazide group, so that the mechanical property of the material is improved. The acylhydrazone bond can enhance the chemical crosslinking ability of the material, so that the self-healing process is more efficient and stable, the completeness of the material can be quickly recovered when the material is damaged by the outside world due to the synergistic effect of the double reversible bond, the service life of the material is greatly prolonged, and the reliability of the material is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of self-repairing materials, and in particular to a self-healing polymer elastomer material and application thereof in a pressure sensor. Background Art

[0002] In the development of modern industry and science and technology, sensors are key components for obtaining information, and their performance stability and reliability are crucial to the stable operation of the entire system. In the field of pressure sensors, due to their wide application in multiple industries such as automobiles, aerospace, and medical equipment, higher requirements are placed on the durability and self-healing ability of materials. After long-term operation or damage from external forces, the performance of traditional pressure sensor materials may decline, resulting in increased measurement errors or even failure, which requires frequent maintenance and replacement, increasing costs and maintenance difficulties.

[0003] With the rapid development of science and technology, polymer elastomer materials have been widely used in many fields due to their excellent elasticity, flexibility and processability. Especially in the field of sensors, polymer elastomer materials are widely used in the contact layer of equipment such as triboelectric pressure sensors due to their unique properties to detect tiny pressure changes. However, in actual use, polymer elastomer materials are also affected by environmental factors such as oxygen and ultraviolet rays, causing their performance to gradually decline. They often face challenges such as poor anti-aging performance and easy damage, which directly affects the stability and service life of the sensor.

[0004] Therefore, it is necessary to improve the deficiencies in the prior art to solve the above problems. Summary of the invention

[0005] The present invention overcomes the deficiencies of the prior art and provides a self-healing polymer elastomer material and application thereof in a pressure sensor.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a self-healing polymer elastomer material, comprising the following steps:

[0007] S1, placing polydimethylsiloxane in a vacuum drying oven, evacuating and heating, to complete the pretreatment of polydimethylsiloxane;

[0008] S2. In a nitrogen environment, polyethylene glycol and pentamethylene diisocyanate are uniformly mixed, an organic bismuth catalyst is added, and the mixture is reacted at a certain temperature to obtain a prepolymer;

[0009] S3, mixing the self-healing agent 1 containing a dynamic disulfide bond with the prepolymer, performing a first stirring, adding the self-healing agent 2 containing a hydrazide group and mixing, performing a second stirring, adding the polymer containing an aldehyde group and mixing, performing a third stirring, and finally adding an antioxidant and mixing, performing a fourth stirring to complete the reaction, and obtaining a self-healing prepolymer;

[0010] S4, mixing and stirring the pretreated polydimethylsiloxane and the self-healing prepolymer, and after curing, obtaining a self-healing polymer elastomer material.

[0011] In a preferred embodiment of the present invention, in step S1, the heating condition is: at a temperature of 60-80° C. for 1-4 hours.

[0012] In a preferred embodiment of the present invention, in the step S2, the mass ratio of the polyethylene glycol to the pentamethylene diisocyanate is 1:1-2.

[0013] In a preferred embodiment of the present invention, in step S2, the organic bismuth catalyst accounts for 0.1-0.5% of the total mass of the polyethylene glycol, and the organic bismuth catalyst is bismuth neodecanoate.

[0014] In a preferred embodiment of the present invention, in the step S2, the reaction conditions are: at a temperature of 50-80° C. for 2-3 h.

[0015] In a preferred embodiment of the present invention, in the step S3, the self-healing agent 1 accounts for 5-10% of the total mass of the prepolymer, and the self-healing agent 1 is one of dibenzothiazole disulfide, 4,4'-dithiodiphenol or dimethylthiuram disulfide; the self-healing agent 2 accounts for 5-10% of the total mass of the prepolymer, and the self-healing agent 2 is one of adipic acid dihydrazide, succinic acid dihydrazide or isocyanuric acid trihydrazide; the polymer accounts for 5-8% of the total mass of the prepolymer polyvinyl formal; the antioxidant is pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate accounting for 0.5-1% of the total mass of the prepolymer.

[0016] In a preferred embodiment of the present invention, in the step S3, the conditions for the first stirring are: the stirring temperature is -5-10°C, and the stirring time is 1-2h; the conditions for the second stirring are: the stirring temperature is -5-10°C, and the stirring time is 1-2h; the conditions for the third stirring are: the stirring temperature is 30-50°C, and the stirring time is 4-8h; the conditions for the fourth stirring are: the stirring temperature is 80-120°C, and the stirring time is 1-3h.

[0017] In a preferred embodiment of the present invention, in the step S4, the mass ratio of the pretreated polydimethylsiloxane to the self-healing prepolymer is 1:0.8-1.5; the stirring conditions are: the stirring temperature is room temperature, and the stirring time is 30-60 minutes.

[0018] In a preferred embodiment of the present invention, in the step S4, the curing conditions are: a fixed temperature of 60-80° C. and a curing time of 4-6 hours.

[0019] The present invention provides an application of a self-healing polymer elastomer material. The self-healing polymer elastomer material is obtained by the aforementioned preparation method and is used to make a contact layer of a triboelectric pressure sensor.

[0020] The present invention solves the defects existing in the background technology and has the following beneficial effects:

[0021] (1) The present invention provides a self-healing polymer elastomer material and its application in a pressure sensor. By introducing a double reversible bond containing a dynamic disulfide bond and an acylhydrazone bond, the material can respond quickly and self-repair when damaged. The dynamic disulfide bond can be broken and reorganized under appropriate conditions to achieve physical crosslinking and de-crosslinking of the material, thereby restoring its original performance. The introduction of an aldehyde-containing polymer allows the aldehyde group to react with the hydrazide group to form a stable acylhydrazone bond. The acylhydrazone bond can enhance the chemical crosslinking ability of the material, making the self-healing process more efficient and stable. The synergistic effect of the double reversible bond enables the material to quickly restore its integrity when damaged by the outside world, greatly improving its service life and reliability.

[0022] (2) In the present invention, pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)benzene propionate is introduced as an antioxidant to form a self-healing prepolymer. The presence of the benzene ring in the molecular structure makes the antioxidant molecule similar to the aromatic structure in the polymer chain, thereby enhancing the interaction. The pentaerythritol ester portion has multiple hydroxyl groups and can form hydrogen bonds with the polar groups in the polymer chain, thereby having good compatibility. At the same time, the phenolic hydroxyl functional group in pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)benzene propionate has high reactivity and can undergo hydrogen atom transfer reaction with free radicals. During the aging process of the material, when the polymer chain generates free radicals, the phenolic hydroxyl group can provide a hydrogen atom to the free radical, thereby converting it into a stable molecule and interrupting the free radical chain reaction. In addition, the tert-butyl group, a group with a large steric hindrance, can effectively protect the phenolic hydroxyl group from further oxidation, thereby effectively inhibiting the thermal oxidation aging process of the material and improving the antioxidant performance of the material.

[0023] (3) The self-healing polymer elastomer material of the present invention is not only suitable for the contact layer of the triboelectric pressure sensor, but can also be widely used in fields such as electronic packaging, medical devices, flexible electronics, etc. Its unique self-healing and anti-oxidation properties make the material have a wide range of application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.

[0025] Figure 1 It is a flow chart of a method for preparing a self-healing polymer elastomer material according to a preferred embodiment of the present invention; DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0028] It should be noted that the raw materials, equipment and reagents used in the present invention can be purchased from the market or obtained through the preparation methods of existing technologies.

[0029] like Figure 1 As shown, a method for preparing a self-healing polymer elastomer material comprises the following steps:

[0030] S1, placing polydimethylsiloxane in a vacuum drying oven, evacuating and heating, to complete the pretreatment of polydimethylsiloxane;

[0031] S2. In a nitrogen environment, polyethylene glycol and pentamethylene diisocyanate are uniformly mixed, an organic bismuth catalyst is added, and the mixture is reacted at a certain temperature to obtain a prepolymer;

[0032] S3, mixing the self-healing agent 1 containing a dynamic disulfide bond with the prepolymer, performing a first stirring, adding the self-healing agent 2 containing a hydrazide group and mixing, performing a second stirring, adding the polymer containing an aldehyde group and mixing, performing a third stirring, and finally adding an antioxidant and mixing, performing a fourth stirring to complete the reaction, and obtaining a self-healing prepolymer;

[0033] S4, mixing and stirring the pretreated polydimethylsiloxane and the self-healing prepolymer, and after curing, obtaining a self-healing polymer elastomer material.

[0034] In step S1, the heating condition is: at a temperature of 60-80° C. for 1-4 hours.

[0035] It should be noted that the water and volatile impurities in the polydimethylsiloxane can be removed by heating.

[0036] In step S2, the mass ratio of polyethylene glycol to pentamethylene diisocyanate is 1:1-2; the organic bismuth catalyst accounts for 0.1-0.5% of the total mass of polyethylene glycol, and the organic bismuth catalyst is bismuth neodecanoate.

[0037] It should be noted that bismuth neodecanoate, as an organic bismuth catalyst, can effectively catalyze the reaction between isocyanate groups and polyethylene glycol hydroxyl groups, improve the interaction between reactant molecules, promote the formation of hydrogen bonds between isocyanate groups and hydroxyl groups, and thus enhance the interaction between reactant molecules, accelerate the formation of prepolymers, increase the reaction rate, thereby shortening the preparation time and improving production efficiency. It also helps to form a stable polymer network structure, which is the key to achieving the self-healing properties of the material and can repair the material by breaking and reconnecting reversible bonds after damage.

[0038] In step S2, the reaction conditions are: at a temperature of 50-80° C. for 2-3 h.

[0039] In step S3, the self-healing agent 1 accounts for 5-10% of the total mass of the prepolymer, and the self-healing agent 1 is one of dibenzothiazole disulfide, 4,4'-disulfide diphenol or dimethylthiuram disulfide; the self-healing agent 2 accounts for 5-10% of the total mass of the prepolymer, and the self-healing agent 2 is one of adipic acid dihydrazide, succinic acid dihydrazide or isocyanuric acid trihydrazide; the polymer accounts for 5-8% of the total mass of the prepolymer, and the polyvinyl formal accounts for 5-8% of the total mass of the prepolymer; the antioxidant is pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate, and accounts for 0.5-1% of the total mass of the prepolymer.

[0040] It should be noted that by introducing a double reversible bond containing a dynamic disulfide bond and an acylhydrazone bond, the material can respond quickly and self-repair when damaged. The dynamic disulfide bond can be broken and reorganized under appropriate conditions to achieve physical cross-linking and de-cross-linking of the material, thereby restoring its original performance. With the introduction of aldehyde-containing polymers, the aldehyde group can react with the hydrazide group to form a stable acylhydrazone bond. The acylhydrazone bond can enhance the chemical cross-linking ability of the material, making the self-healing process more efficient and stable. The synergistic effect of this double reversible bond enables the material to quickly restore its integrity when damaged by the outside world, greatly improving its service life and reliability.

[0041] In step S3, the conditions for the first stirring are: stirring temperature of -5-10°C, stirring time of 1-2h; the conditions for the second stirring are: stirring temperature of -5-10°C, stirring time of 1-2h; the conditions for the third stirring are: stirring temperature of 30-50°C, stirring time of 4-8h; the conditions for the fourth stirring are: stirring temperature of 80-120°C, stirring time of 1-3h.

[0042] In step S4, the mass ratio of the pretreated polydimethylsiloxane to the self-healing prepolymer is 1:0.8-1.5; the stirring conditions are: the stirring temperature is room temperature, and the stirring time is 30-60 minutes; the curing conditions are: the fixing temperature is 60-80°C, and the curing time is 4-6 hours.

[0043] The present invention provides an application of a self-healing polymer elastomer material. The self-healing polymer elastomer material prepared by the above-mentioned preparation method is used to make a contact layer of a triboelectric pressure sensor.

[0044] Example 1

[0045] A method for preparing a self-healing polymer elastomer material comprises the following steps:

[0046] S1. Place polydimethylsiloxane in a vacuum drying oven, evacuate the oven, and treat at 60° C. for 2 h to complete the pretreatment of polydimethylsiloxane.

[0047] S2. In a nitrogen environment, polyethylene glycol and pentamethylene diisocyanate in a mass ratio of 1:2 are uniformly mixed, bismuth neodecanoate accounting for 0.3% of the total mass of polyethylene glycol is added, and the mixture is treated at a temperature of 80° C. for 2 h to obtain a prepolymer;

[0048] S3, mixing 8% of the total mass of the prepolymer with dibenzothiazole disulfide and the prepolymer, stirring at a temperature of -5°C for 2h, adding 8% of the total mass of the prepolymer with adipic acid dihydrazide, stirring at a temperature of -5°C for 2h, adding 5% of the total mass of the prepolymer with polyvinyl formal, stirring at a temperature of 35°C for 7h, and finally adding 0.7% of the total mass of the prepolymer with pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)benzene propionate, stirring at a temperature of 110°C for 2h to complete the reaction, and obtaining a self-healing prepolymer;

[0049] S4. The pretreated polydimethylsiloxane and the self-healing prepolymer in a mass ratio of 1:1 are stirred and mixed at room temperature for 45 minutes, and dried at 80° C. for 5 hours to complete curing, thereby obtaining a self-healing polymer elastomer material.

[0050] Example 2

[0051] This embodiment is basically the same as Embodiment 1, except that: Step S3 is as follows: 8% of the total mass of the prepolymer is mixed with 4,4'-dithiodiphenol and the prepolymer, stirred at -5°C for 2h, 8% of the total mass of the prepolymer is added with succinic acid dihydrazide, stirred at -5°C for 2h, 5% of the total mass of the prepolymer is added with polyvinyl formal, stirred at 35°C for 7h, and finally 0.7% of the total mass of the prepolymer is added with pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate, stirred at 110°C for 2h to complete the reaction, and obtain a self-healing prepolymer.

[0052] Example 3

[0053] This embodiment is basically the same as Embodiment 1, except that: Step S3 is as follows: 8% of the total mass of the prepolymer is mixed with dimethylthiuram disulfide and the prepolymer, stirred at a temperature of -5°C for 2h, 8% of the total mass of the prepolymer is added with isocyanuric acid trihydrazide and mixed, stirred at a temperature of -5°C for 2h, 5% of the total mass of the prepolymer is added with polyvinyl formal and mixed, stirred at a temperature of 35°C for 7h, and finally 0.7% of the total mass of the prepolymer is added with pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate and mixed, stirred at a temperature of 110°C for 2h to complete the reaction, and obtain a self-healing prepolymer.

[0054] Example 4

[0055] This embodiment is basically the same as Embodiment 1, except that: Step S3 is as follows: 8% of the total mass of the prepolymer is mixed with dibenzothiazole disulfide and the prepolymer, stirred at -5°C for 2h, 8% of the total mass of the prepolymer is added with succinic acid dihydrazide, stirred at -5°C for 2h, 5% of the total mass of the prepolymer is added with polyvinyl formal, stirred at 35°C for 7h, and finally 0.7% of the total mass of the prepolymer is added with pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)benzenepropionate, stirred at 110°C for 2h to complete the reaction, and obtain a self-healing prepolymer.

[0056] Example 5

[0057] This embodiment is basically the same as Embodiment 1, except that: Step S3 is as follows: 8% of the total mass of the prepolymer is mixed with dibenzothiazole disulfide and the prepolymer, stirred at -5°C for 2h, 8% of the total mass of the prepolymer is added and mixed with isocyanuric acid trihydrazide, stirred at -5°C for 2h, 5% of the total mass of the prepolymer is added and mixed with polyvinyl formal, stirred at 35°C for 7h, and finally 0.7% of the total mass of the prepolymer is added with pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate, stirred at 110°C for 2h to complete the reaction, and obtain a self-healing prepolymer.

[0058] Example 6

[0059] This embodiment is basically the same as Embodiment 1, except that: Step S3 is as follows: 8% of the total mass of the prepolymer is mixed with 4,4'-dithiodiphenol and the prepolymer, stirred at -5°C for 2h, 8% of the total mass of the prepolymer is added with adipic acid dihydrazide and mixed, stirred at -5°C for 2h, 5% of the total mass of the prepolymer is added with polyvinyl formal and mixed, stirred at 35°C for 7h, and finally 0.7% of the total mass of the prepolymer is added with pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate and mixed, stirred at 110°C for 2h to complete the reaction, and obtain a self-healing prepolymer.

[0060] Example 7

[0061] This embodiment is basically the same as Embodiment 1, except that: Step S3 is as follows: 8% of the total mass of the prepolymer is mixed with 4,4'-dithiodiphenol and the prepolymer, stirred at -5°C for 2h, 8% of the total mass of the prepolymer is added with isocyanuric acid trihydrazide and mixed, stirred at -5°C for 2h, 5% of the total mass of the prepolymer is added with polyvinyl formal and mixed, stirred at 35°C for 7h, and finally 0.7% of the total mass of the prepolymer is added with pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate and mixed, stirred at 110°C for 2h to complete the reaction, and obtain a self-healing prepolymer.

[0062] Example 8

[0063] This embodiment is basically the same as Embodiment 1, except that: Step S3 is as follows: 8% of the total mass of the prepolymer is mixed with dimethylthiuram disulfide and the prepolymer, stirred at a temperature of -5°C for 2h, 8% of the total mass of the prepolymer is added with adipic acid dihydrazide and mixed, stirred at a temperature of -5°C for 2h, 5% of the total mass of the prepolymer is added with polyvinyl formal and mixed, stirred at a temperature of 35°C for 7h, and finally 0.7% of the total mass of the prepolymer is added with pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate and mixed, stirred at a temperature of 110°C for 2h to complete the reaction, and obtain a self-healing prepolymer.

[0064] Example 9

[0065] This embodiment is basically the same as Embodiment 1, except that: Step S3 is as follows: 8% of the total mass of the prepolymer is mixed with dimethylthiuram disulfide and the prepolymer, stirred at a temperature of -5°C for 2h, 8% of the total mass of the prepolymer is added with succinic acid dihydrazide and mixed, stirred at a temperature of -5°C for 2h, 5% of the total mass of the prepolymer is added with polyvinyl formal and mixed, stirred at a temperature of 35°C for 7h, and finally 0.7% of the total mass of the prepolymer is added with pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate and mixed, stirred at a temperature of 110°C for 2h to complete the reaction, and obtain a self-healing prepolymer.

[0066] Comparative Example 1

[0067] This embodiment is basically the same as Embodiment 1, except that: Step S3 is as follows: 8% of dibenzothiazole disulfide by weight of the prepolymer is mixed with the prepolymer, stirred at -5°C for 2 h, 8% of adipic acid dihydrazide by weight of the prepolymer is added and mixed, stirred at -5°C for 2 h, and finally 5% of polyvinyl formal by weight of the prepolymer is added and mixed, stirred at 35°C for 7 h to complete the reaction, and obtain a self-healing prepolymer.

[0068] Performance testing: The self-healing polymer elastomer materials obtained in the above Examples 1-9 and Comparative Example 1 were tested for self-repairing tensile properties and aging resistance.

[0069] Self-healing tensile properties: Cut the self-healing polymer elastomer material, connect the two cut pieces together, drop water on the cut, and measure the time required for self-healing and the self-healing efficiency of mechanical properties at room temperature and 60°C respectively.

[0070] Aging resistance: Refer to GB / T 14522-2008 "Artificial weathering test method for plastics, coatings and rubber materials for mechanical industrial products - fluorescent ultraviolet lamp".

[0071] The test results of the self-repairing tensile properties and aging resistance of Examples 1-9 and Comparative Example 1 are shown in Table 1.

[0072] Table 1:

[0073]

[0074] It can be seen from Table 1 that:

[0075] By comparing Example 2 with Example 1 and Examples 3-9, it can be learned that by using 4,4'-dithiodiphenol as the first healing agent and succinic acid dihydrazide as the second healing agent, 4,4'-dithiodiphenol can break when the material is damaged, and the breaking of the disulfide bond will release sulfur free radicals, and the reactivity of the hydrazide group in succinic acid dihydrazide will cause the hydrazide group to react rapidly with the aldehyde group, and the nitrogen atom in the hydrazide group will attack the carbon atom of the aldehyde group to form a stable acylhydrazone bond. The reaction is fast, and the generated acylhydrazone bond has high stability. The reaction of the sulfur free radical and the hydrazide group will form a new chemical bond in the damaged area, and the sulfur atom in 4,4'-dithiodiphenol and the nitrogen atom in succinic acid dihydrazide have a suitable electron cloud distribution, which makes it easier to transfer and share electrons between them, thereby giving them stronger connection and repair capabilities.

[0076] By comparing Example 1 with Comparative Example 1, it can be learned that by introducing pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)benzene propionate as an antioxidant to form a self-healing prepolymer, the presence of the benzene ring in the molecular structure makes the antioxidant molecule similar to the aromatic structure in the polymer chain, thereby enhancing the interaction. The pentaerythritol ester portion has multiple hydroxyl groups and can form hydrogen bonds with polar groups in the polymer chain, thereby having good compatibility. At the same time, the phenolic hydroxyl functional group in pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)benzene propionate has high reactivity and can undergo hydrogen atom transfer reaction with free radicals. During the aging process of the material, when the polymer chain generates free radicals, the phenolic hydroxyl group can provide a hydrogen atom to the free radical, thereby converting it into a stable molecule and interrupting the free radical chain reaction. In addition, the tert-butyl group, a group with a large steric hindrance, can effectively protect the phenolic hydroxyl group from further oxidation, thereby effectively inhibiting the thermal oxidation aging process of the material and improving the antioxidant performance of the material.

[0077] The self-healing polymer elastomer material of the present invention is not only suitable for the contact layer of the triboelectric pressure sensor, but also can be widely used in fields such as electronic packaging, medical equipment, flexible electronics, etc. Its unique self-healing and anti-oxidation properties make the material have a wide range of application prospects.

[0078] The above is based on the ideal embodiment of the present invention. Through the above description, it is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic characteristics of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is limited by the attached claims rather than the above description, and it is intended to include all changes within the meaning and scope of the equivalent elements of the claims. Any figure mark in the claims should not be regarded as limiting the claims involved.

[0079] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing a self-healing polymer elastic material, characterized in that: The following steps are involved: S1, placing polydimethylsiloxane in a vacuum drying oven, evacuating and heating, to complete the pretreatment of polydimethylsiloxane; S2. In a nitrogen environment, polyethylene glycol and pentamethylene diisocyanate are uniformly mixed, an organic bismuth catalyst is added, and the mixture is reacted at a certain temperature to obtain a prepolymer; S3, mixing the self-healing agent 1 containing a dynamic disulfide bond with the prepolymer, performing a first stirring, adding the self-healing agent 2 containing a hydrazide group and mixing, performing a second stirring, adding the polymer containing an aldehyde group and mixing, performing a third stirring, and finally adding an antioxidant and mixing, performing a fourth stirring to complete the reaction, and obtaining a self-healing prepolymer; S4, mixing and stirring the pretreated polydimethylsiloxane and the self-healing prepolymer, and after curing, obtaining a self-healing polymer elastomer material.

2. The method for preparing a self-healing polymer elastic material according to claim 1, characterized in that: In the step S1, the heating condition is: at a temperature of 60-80° C. for 1-4 hours.

3. The method for preparing a self-healing polymer elastic material according to claim 1, characterized in that: In the step S2, the mass ratio of the polyethylene glycol to the pentamethylene diisocyanate is 1:1-2.

4. The method for preparing a self-healing polymer elastic material according to claim 1, characterized in that: In the step S2, the organic bismuth catalyst accounts for 0.1-0.5% of the total mass of the polyethylene glycol, and the organic bismuth catalyst is bismuth neodecanoate.

5. The method for preparing a self-healing polymer elastic material according to claim 1, characterized in that: In the step S2, the reaction conditions are: at a temperature of 50-80° C. for 2-3 hours.

6. The method for preparing a self-healing polymer elastic material according to claim 1, characterized in that: In the step S3, the self-healing agent 1 accounts for 5-10% of the total mass of the prepolymer, and the self-healing agent 1 is one of dibenzothiazole disulfide, 4,4'-dithiodiphenol or dimethylthiuram disulfide; the self-healing agent 2 accounts for 5-10% of the total mass of the prepolymer, and the self-healing agent 2 is one of adipic acid dihydrazide, succinic acid dihydrazide or isocyanuric acid trihydrazide; the polymer accounts for 5-8% of the total mass of the prepolymer. Polyvinyl formal; the antioxidant is pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate, which accounts for 0.5-1% of the total mass of the prepolymer.

7. The method for preparing a self-healing polymer elastic material according to claim 1, characterized in that: In the step S3, the conditions for the first stirring are: stirring temperature of -5-10°C, stirring time of 1-2h; the conditions for the second stirring are: stirring temperature of -5-10°C, stirring time of 1-2h; the conditions for the third stirring are: stirring temperature of 30-50°C, stirring time of 4-8h; the conditions for the fourth stirring are: stirring temperature of 80-120°C, stirring time of 1-3h.

8. The method for preparing a self-healing polymer elastic material according to claim 1, characterized in that: In the step S4, the mass ratio of the pretreated polydimethylsiloxane to the self-healing prepolymer is 1:0.8-1.5; the stirring conditions are: the stirring temperature is room temperature, and the stirring time is 30-60 minutes.

9. The method for preparing a self-healing polymer elastic material according to claim 1, characterized in that: In the step S4, the curing conditions are: a fixing temperature of 60-80° C. and a curing time of 4-6 hours.

10. An application of a self-healing polymer elastic material, characterized in that: The self-healing polymer elastomer material is obtained by the preparation method according to any one of claims 1 to 9 and is used to make a contact layer of a triboelectric pressure sensor.

Citation Information

Cited By

  • Self-healing elastomer as well as preparation method and application thereof

    CN120842530A