Kombucha cellulose film and preparation method thereof

By enzymatically lyticking and microwaveing ​​of kohlc cellulose, a uniform microstructure was formed, and the problem of insufficient performance of traditional biodegradable films was solved, and a high mechanical strength and rapid degradation of kohlc cellulose film was achieved, showing a green and environmentally friendly Production process.

CN119039635AInactive Publication Date: 2024-11-29ZHEJIANG OCEAN UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411533378.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional biodegradable films have defects in performance and quality, which are difficult to compare with petrochemical polymers, and the performance of biodegradable materials is insufficient, resulting in insufficient films in terms of mechanical strength and environmental friendliness.

Method used

After enzymatic treatment with kombucha cellulose, it is mixed with thickener and crosslinker under microwave action to form a uniform, single-stranded, short string microstructure, which improves the mechanical strength of the film while maintaining biodegradable properties.

Benefits of technology

Through microwave processing, the mechanical strength of the Kombucha cellulose film is greatly improved, and the biodegradable performance is maintained, achieving a green and environmentally friendly production process. The film is completely degraded within 5 days and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039635A_ABST
    Figure CN119039635A_ABST
Patent Text Reader

Abstract

The invention relates to the field of degradable films, and provides a kombucha cellulose film and a preparation method thereof.The method comprises the steps that kombucha cellulose is subjected to enzymolysis with cellulase, meanwhile, homogenization is conducted, and a cellulose hydrolysate is obtained; dispersing the cellulose hydrolysate, a thickening agent and a cross-linking agent in a solvent, and mixing under the action of microwaves to obtain turbid liquid; the microwave power is 70-90 W, the mixing temperature is 50-70 DEG C, and the mixing time is 10-20 min; the microstructure of the cellulose hydrolysate in the turbid liquid is a sphere with the particle size of 0.5-1 [mu] m; and preparing the turbid liquid into a film. Kombucha cellulose is purified and subjected to enzymolysis and then mixed with a thickening agent and a cross-linking agent under the action of microwaves, the particle size of the Kombucha cellulose is reduced, the structure of the Kombucha cellulose is round, uniform, single-chain and short-chain Kombucha cellulose hydrolysate is doped in the microstructure level of the prepared film, and the mechanical strength of the film is greatly improved; meanwhile, the biodegradable performance of the film is not reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of biodegradable films, in particular to a kombucha cellulose film and a preparation method thereof. Background Art

[0002] Biodegradable films undergo bacterial decomposition after fulfilling their original purpose, ultimately decomposing into water, minerals, CO2, and N2. These films are usually formed by condensation and ring-opening polymerization and are mainly composed of esters, amides, and ethers. Degradable polymers such as polysaccharides and proteins have received extensive attention in the preparation of films.

[0003] Traditional biodegradable films are prepared by selecting biodegradable materials and then producing the required films by selecting a suitable method. For example, patent CN104725652B discloses a method for preparing a degradable composite pullulan film, which uses edible pullulan as a raw material, is non-toxic and safe, and can be degraded and utilized by microorganisms in nature without causing environmental pollution. However, compared with petrochemical polymers, it is necessary to improve processing technology to improve the performance and quality of biodegradable films. However, due to the shortcomings in the performance of biodegradable materials themselves, biodegradable films have certain defects in performance and quality. Therefore, an ideal solution is needed. Summary of the invention

[0004] The invention provides a kombucha cellulose film and a preparation method thereof. The kombucha cellulose is purified and enzymatically hydrolyzed, and then mixed with a thickener and a cross-linking agent under the action of microwaves. The particle size of the kombucha cellulose is reduced and the structure becomes round. The prepared film has uniform, single-chain, and short-string kombucha cellulose hydrolyzate incorporated at the microstructure level. The mechanical strength of the film is greatly improved, and the biodegradability of the film is not reduced.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: A method for preparing a kombucha cellulose film comprises the following steps: (1) enzymatically hydrolyzing kombucha cellulose with cellulase and simultaneously homogenizing the cellulose to obtain a cellulose hydrolyzate; (2) The cellulose hydrolysate, thickener and cross-linking agent are dispersed in a solvent and mixed under the action of microwaves to obtain a suspension; the microwave power is 70-90 W, the mixing temperature is 50-70 °C, and the mixing time is 10-20 min; the microstructure of the cellulose hydrolysate in the suspension is spherical with a particle size of 0.5-1 μm; (3) Form the suspension into a thin film.

[0006] Preferably, the kombucha cellulose is purified before enzymatic hydrolysis, and the purification steps are: dispersing the kombucha cellulose in water, first treating it with alkali, then treating it with acid, and washing it with water.

[0007] Preferably, the water is sterilized purified water, which is heated to 100°C and kept warm for more than 30 minutes.

[0008] Preferably, the alkali treatment step is: treating with 0.5-2 mol / L NaOH solution at 48-53°C for 10-12 h; the acid treatment step is: treating with 1-2% mass concentration glacial acetic acid for 1-2 h; washing with water until neutral, and freeze-drying.

[0009] Preferably, the enzymatic hydrolysis conditions are: the mass ratio of enzyme to substrate is 1-3%, the enzymatic hydrolysis is performed at 30-50°C for 8-30 min, and the homogenization speed is 8000-12000 rpm.

[0010] Preferably, the mass concentration of kombucha cellulose enzymatic hydrolysis is 5-7%.

[0011] Preferably, after the enzymatic hydrolysis is completed, the enzyme is inactivated by heating at 90-95°C for 10-20 min, and the cellulose hydrolysate in the upper layer is collected by centrifugation and freeze-dried.

[0012] Preferably, the solvent in step (2) is water, the concentration of the cellulose hydrolysate is 0.04-0.5 g / mL, the mass of the thickener is 12-17% of the cellulose hydrolysate, and the mass of the cross-linking agent is 6-10% of the cellulose hydrolysate.

[0013] Preferably, the thickener is selected from sodium carboxymethyl cellulose or alginate, and the cross-linking agent is selected from one or two of gelatin, agar, and pectin.

[0014] As further preferred, the thickener is sodium alginate and the cross-linking agent is agar.

[0015] Preferably, the suspension is sterilized at high temperature and dried to obtain a film.

[0016] Preferably, the temperature for high temperature sterilization is 110-130°C, and the time is 20-40 min; the temperature for drying is 40-50°C, and the time is 15-25 h.

[0017] The invention also provides a kombucha cellulose film, which is prepared by the preparation method.

[0018] Preferably, nanoparticles and stripe structures are evenly dispersed on the surface of the kombucha cellulose film, wherein the nanoparticles are spherical kombucha cellulose with a particle size of 0.5-1 μm, and the stripe structures are string structures of kombucha cellulose extending and incorporated into the film, showing multiple stripe edges.

[0019] Preferably, the kombucha cellulose film has a tensile strength of ≥ 18 MPa, and a degradation performance of starting to degrade from the first day and completely degrading within 5 days.

[0020] Therefore, the beneficial effects of the present invention are: (1) Thickeners and cross-linking agents were added to the cellulose hydrolysate of kombucha, and microwave processing was used to assist mixing. The strong micro-mixing and high shear stress of microwave processing not only reduced the particle size of kombucha cellulose from about 2 μm to 1 μm, but also changed its structure from irregular to round. The microstructure of the prepared film was uniform, with single-chain, short strings of kombucha cellulose hydrolysate, which greatly improved the mechanical strength of the film. At the same time, the biodegradability of the film generated by microwave processing did not decrease compared with traditional biodegradable films.

[0021] (2) After the cellulose hydrolysate suspension is sterilized, the film can be obtained by directly cooling and drying without using an organic solvent, thereby avoiding the high production cost caused by the use of organic solvents and the impact on the environment caused by the recovery and treatment of organic solvents. Therefore, the preparation method of the present invention is green and environmentally friendly, and the process is simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a scanning electron microscope image of the film of comparative example 1; in the image, a-1 is the front side of the film, and a-2 is the side side of the film.

[0023] Figure 2 This is a scanning electron microscope image of the film of comparative example 2; b-1 in the image is the front side of the film, and b-2 is the side side of the film.

[0024] Figure 3 is a scanning electron microscope image of the film of Example 1; in the image, c-1 is the front side of the film, and c-2 is the side side of the film.

[0025] Figure 4 This is a scanning electron microscope image of the film of comparative example 3; in the image, d-1 is the front side of the film, and d-2 is the side side of the film. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is further described below through specific embodiments.

[0027] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the embodiments, unless otherwise specified, are all conventional methods in the art. Unless otherwise specified, parts are by weight, temperatures are expressed in ° C or at ambient temperature, and pressures are atmospheric pressure or near atmospheric pressure. There are many variations and combinations of reaction conditions (such as component concentrations, desired solvents, solvent mixtures, temperatures, pressures, and other reaction ranges) and conditions that can be used to optimize the purity and yield of the product obtained by the method, and only reasonable routine experiments will be required to optimize such method conditions.

[0028] Example A method for preparing a kombucha cellulose film comprises the following steps: S1. Disperse the kombucha cellulose in distilled water, stir and dissolve, and filter. Preferably, the water is sterilized pure water, and the pure water is heated to 100°C and kept warm for more than 30 minutes. Treat with 0.5-2 mol / L NaOH solution at 48-53°C for 10-12 hours. Then treat with glacial acetic acid with a mass concentration of 1-2% for 1-2 hours. Finally, wash the kombucha cellulose with distilled water for multiple times until the pH reaches 7. After neutralization and washing, freeze-dry the kombucha cellulose to obtain freeze-dried kombucha cellulose powder.

[0029] The principle of alkali-first followed by acid purification is mainly based on the difference in solubility and reactivity of different substances under acidic and alkaline conditions. Acid-base treatment is used to remove impurities, effectively remove impurities with large polarity differences (such as inorganic salts, organic acid-base impurities, etc.), and improve the purity of the target substance. The specific process and impurities removed are as follows: Under alkaline conditions, some impurities (such as acidic organic acids, inorganic acid impurities, or compounds that can react with alkali) will dissolve or undergo chemical changes to form soluble salts or other products. This allows the impurities to dissolve in the alkali solution, while the target to be purified, if it is an alkali-insoluble substance, will remain as a solid or be less affected. After the alkali treatment, it is treated with acid. The acid can cause certain impurities dissolved under alkaline conditions to re-precipitate or react with the acid to form other forms of products (such as precipitates or gases), thereby further removing impurities such as amine compounds and alkaline metal impurities. At the same time, the acid treatment will also allow the target substance to reach a suitable solubility or purity.

[0030] S2. The freeze-dried powder of kombucha cellulose obtained in S1 is dissolved in distilled water at a mass ratio of 6%, and cellulase is added at the same time, and the mass ratio of enzyme / substrate is 1-3%. The temperature of the mixture of kombucha cellulose and distilled water is set at 45-55 °C to ensure the optimal activity of cellulase. The enzyme treatment is carried out in a water bath at 45-55 °C for 8-30 min, while homogenizing at a speed of 8000-12000 rpm, and then heated at 90-95 °C for 10-20 min to inactivate the enzyme. The solution is centrifuged into two layers, the bottom layer is unhydrolyzed, insoluble cellulose precipitate, and the top layer is hydrolyzed, soluble cellulose hydrolysate liquid. The soluble cellulose hydrolysate in the upper layer is collected, freeze-dried and stored.

[0031] S3. Disperse the cellulose hydrolysate, thickener and cross-linking agent in solvent water, wherein the mass concentration of the cellulose hydrolysate is 0.04-0.5 g / mL, the mass of the thickener is 12-17% of the cellulose hydrolysate, and the mass of the cross-linking agent is 6-10% of the cellulose hydrolysate. Preferably, the thickener is selected from sodium carboxymethyl cellulose or alginate, and the cross-linking agent is selected from one or two of gelatin, agar, and pectin. Further preferably, the thickener is sodium alginate and the cross-linking agent is agar. Mix under the action of microwaves to obtain a suspension; the microwave power is 70-90 W, the mixing temperature is 50-70 °C, and the mixing time is 10-20 min; the microstructure of the cellulose hydrolysate in the suspension is spherical with a particle size of 0.5-1 μm; S4. After collecting enough suspension, sterilize and dry the suspension at high temperature to obtain a film. Autoclave at 110-130°C for 20-40 minutes, pour into a tray, and dry at 40-50°C for 15-25 hours to obtain a film.

[0032] The present invention also provides a kombucha cellulose film, which is prepared by the above preparation method. Nanoparticles and stripe structures are evenly dispersed on the surface of the kombucha cellulose film, the nanoparticles are spherical kombucha cellulose with a particle size of 0.5-1 μm, and the stripe structures are string structures of kombucha cellulose extending and incorporated into the film, showing multiple stripe edges. The kombucha cellulose film has a tensile strength of ≥ 18MPa, and the degradation performance is that it starts to degrade from the first day and is completely degraded within 5 days.

[0033] The advantages of kombucha cellulose in film preparation, especially compared with other bio-based materials, come from its unique mechanical strength and processability. This is mainly related to its following properties: 1. High mechanical strength: By hydrolyzing kombucha cellulose, the cellulose hydrolysate generated can form a striped structure in the film, which greatly improves the mechanical strength of the film. 2. Improved particle size and structure: After hydrolysis and microwave treatment, the particle size of kombucha cellulose is reduced from 2 μm to 1 μm, and the shape is changed from irregular to round. This improvement in microstructure improves the uniformity of the distribution of cellulose hydrolysate in the film, thereby enhancing the overall performance of the film. 3. Good biodegradability: Despite the improvement in mechanical strength, the film made with kombucha cellulose hydrolysate does not sacrifice its biodegradability. Compared with other bio-based materials, kombucha cellulose film can be completely degraded in a short time, meeting environmental protection requirements.

[0034] In summary, kombucha cellulose has become a more ideal bio-based film material due to its superior mechanical properties, microstructural controllability and good biodegradability.

[0035] Example 1 A method for preparing a kombucha cellulose film, comprising the following steps: S1. Select kombucha cellulose and dissolve it in distilled water and stir it for 48 h, filter it, heat it with 1 mol / L NaOH solution at 50 °C for 12 h, and then treat it with 1% glacial acetic acid for 1 h. Finally, wash the kombucha cellulose with distilled water several times until the pH reaches 7. After neutralization and washing, freeze-dry the kombucha cellulose.

[0036] S2. The freeze-dried powder of kombucha cellulose obtained from S1 was dissolved in distilled water at a ratio of 6%, and cellulase was added at a mass ratio of 2% of enzyme / substrate. The temperature of the mixture of kombucha cellulose and distilled water was set at 50 °C to ensure the optimal activity of cellulase. The enzyme treatment was carried out in a water bath at 50 °C for 30 min, while homogenizing at a speed of 10,000 rpm. Then, the enzyme was inactivated by heating at 95 °C for 20 min. The solution was centrifuged into two layers, the bottom layer was unhydrolyzed, insoluble cellulose precipitate, and the top layer was hydrolyzed, soluble cellulose hydrolysate liquid. The soluble cellulose hydrolysate in the upper layer was collected, freeze-dried and stored.

[0037] S3. Dissolve 30 g of the soluble cellulose hydrolysate obtained in S2 in 750 mL of water, add 2.5 g of agar and 5 g of sodium alginate, and mix under microwave assistance to obtain a suspension. The microwave power is 80 W, the mixing temperature is 60 ℃, and the mixing time is 15 min. The microstructure of the cellulose hydrolysate in the suspension is spherical with a particle size of 0.5-1 μm.

[0038] S4. Collect 300 mL of the suspension, autoclave the suspension at 120 °C for 30 minutes, pour it into a tray (20 × 30 cm), and dry it at 45 °C for 20 hours to obtain a film.

[0039] Example 2 The difference from Example 1 is that the amounts of agar and sodium alginate in step S3 are not within the preferred range, specifically: agar is reduced to 1.5 g, and sodium alginate is increased to 6 g.

[0040] Example 3 The difference from Example 1 is that the mass ratio of enzyme / substrate in step S2 is reduced to 0.5%, which is not within the preferred range of 1-2%.

[0041] Example 4 The difference from Example 1 is that in step S3, 30 g of the soluble cellulose hydrolysate obtained in S2 is dissolved in 30 mL of water.

[0042] Example 5 A method for preparing a kombucha cellulose film, comprising the following steps: S1. Select kombucha cellulose and dissolve it in distilled water and stir it for 48 hours, filter it, heat it with 0.5 mol / L NaOH solution at 50 ℃ for 12 hours, and then treat it with 2% glacial acetic acid for 1 hour. Finally, wash the kombucha cellulose with distilled water several times until the pH reaches 7. After neutralization and washing, freeze-dry the kombucha cellulose.

[0043] S2. The freeze-dried powder of kombucha cellulose obtained from S1 was dissolved in distilled water at a ratio of 6%, and cellulase was added at a mass ratio of 1% of enzyme / substrate. The temperature of the mixture of kombucha cellulose and distilled water was set at 45 °C. The enzyme treatment was carried out in a water bath at 45 °C for 20 min, while homogenizing at a speed of 8000 rpm. Then, the enzyme was inactivated by heating at 90 °C for 20 min. The solution was centrifuged and separated into two layers, the bottom layer was unhydrolyzed, insoluble cellulose precipitate, and the top layer was hydrolyzed, soluble cellulose hydrolysate liquid. The soluble cellulose hydrolysate in the upper layer was collected, freeze-dried and stored.

[0044] S3. Dissolve 30 g of the soluble cellulose hydrolysate obtained in S2 in 60 mL of water, add 1.8 g of agar and 3.6 g of sodium alginate, and mix under microwave assistance to obtain a suspension. The microwave power is 70 W, the mixing temperature is 50 ℃, and the mixing time is 20 min. The microstructure of the cellulose hydrolysate in the suspension is spherical with a particle size of 0.5-1 μm.

[0045] S4. Collect 300 mL of the suspension, autoclave the suspension at 110 °C for 40 minutes, pour it into a tray (20 × 30 cm), and dry it at 40 °C for 25 hours to obtain a film.

[0046] Example 6 A method for preparing a kombucha cellulose film, comprising the following steps: S1. Select kombucha cellulose and dissolve it in distilled water and stir it for 48 hours, filter it, heat it with 2 mol / L NaOH solution at 50 ℃ for 10 hours, and then treat it with 1% glacial acetic acid for 2 hours. Finally, wash the kombucha cellulose with distilled water several times until the pH reaches 7. After neutralization and washing, freeze-dry the kombucha cellulose.

[0047] S2. The freeze-dried powder of kombucha cellulose obtained from S1 was dissolved in distilled water at a ratio of 6%, and cellulase was added at a mass ratio of 3% for enzyme / substrate. The temperature of the mixture of kombucha cellulose and distilled water was set at 55 °C. The enzyme treatment was carried out in a water bath at 55 °C for 8 min, while homogenizing at a speed of 12,000 rpm. The enzyme was then heated at 95 °C for 10 min to inactivate the enzyme. The solution was centrifuged and separated into two layers, the bottom layer was unhydrolyzed, insoluble cellulose precipitate, and the top layer was hydrolyzed, soluble cellulose hydrolysate liquid. The soluble cellulose hydrolysate in the upper layer was collected, freeze-dried and stored.

[0048] S3. Dissolve 30 g of the soluble cellulose hydrolysate obtained in S2 in 300 mL of water, add 3 g of agar and 5.1 g of sodium alginate, and mix under microwave assistance to obtain a suspension. The microwave power is 90 W, the mixing temperature is 70 ℃, and the mixing time is 10 min. The microstructure of the cellulose hydrolysate in the suspension is spherical with a particle size of 0.5-1 μm.

[0049] S4. Collect 300 mL of the suspension, autoclave the suspension at 130 °C for 20 minutes, pour it into a tray (20 × 30 cm), and dry it at 50 °C for 15 hours to obtain a film.

[0050] Comparative Example Comparative Example 1 The difference from Example 1 is that the kombucha cellulose is not enzymatically hydrolyzed, that is, step S2 is not performed.

[0051] Comparative Example 2 The difference from Example 1 is that in step S3, when the soluble cellulose hydrolysate is mixed with agar and sodium alginate, there is no microwave, but the mixture is homogenized at a speed of 10,000 rpm.

[0052] Comparative Example 3 The difference from Example 1 is that in step S3, no cellulose hydrolysate is added, that is, only agar and sodium alginate are mixed to form the membrane.

[0053] Comparative Example 4 The difference from Example 1 is that the microwave power in step S3 is 110 W, which is higher than the preferred range of 70-90 W.

[0054] Performance Testing The performance tests of the films prepared in the embodiments and comparative examples are as follows.

[0055] (1) Tensile strength Test method: In an environment of 25 ℃, the mechanical strength was tested using an Instron 5960 benchtop tensile tester with a loading unit of 500 N. A crosshead speed of 5 mm / min was used, and the load value was recorded. The results are shown in Table 1.

[0056] Table 1

[0057] From Table 1, the mechanical strength of the film (Example 1) made by mixing with the aid of microwave processing using the hydrolyzate of kombucha cellulose as raw material is 18.18 MPa, which is higher than that of Comparative Example 1, which directly uses the complete kombucha cellulose as raw material, and Comparative Example 3, indicating that the hydrolyzate obtained by enzymatic hydrolysis of kombucha cellulose can be used to make a film to improve the mechanical strength of the film. The mechanical strength of the film (Example 1) made with the aid of microwave processing is better than that of the film (Comparative Example 2) made without the aid of microwave processing, which indicates that microwave processing assistance helps to form a film with higher mechanical strength. In Comparative Example 4, the microwave power is insufficient, which affects the uniformity and structural strength of the film; in Comparative Example 5, the microwave power is too large, the microstructure of the kombucha cellulose particles is destroyed and the film is too dense, and the performance is reduced.

[0058] Comparing the various examples, the film of Example 1 has the highest mechanical strength, which is mainly attributed to the uniform distribution of cellulose hydrolysate and the optimal adjustment of the microstructure. In contrast, the amount of agar and sodium alginate in Example 2 is not within the preferred range, resulting in insufficient cross-linking structure in the film and reduced mechanical strength. The enzymatic efficiency of Example 3 is insufficient, which affects the uniformity and structural strength of the film. In Example 4, the excessively high concentration of cellulose hydrolysate causes the film to be too dense, thereby reducing the mechanical strength and flexibility.

[0059] (2) Biodegradability Test method: Soil was added to a glass container to a height of 60 mm, and a biodegradable film (40 × 40 mm) was buried in the soil to a depth of 20 mm. The glass bottles were stored in a greenhouse and watered twice a day to maintain humidity. The biofilm was removed and weighed on the 1st, 3rd and 5th day, and then reburied. The biodegradability of each film was calculated as the weight percentage of the remaining film relative to the original film. The results are shown in Table 2.

[0060] Table 2

[0061] Example 1 was completely degraded on the 5th day, and the degradation rate was close to that of Comparative Example 3, indicating that the biodegradability of the film of the present invention was not reduced while the mechanical strength was improved. Examples 2-4 had slightly reduced biodegradability due to factors such as the amount of agar and sodium alginate, enzymatic hydrolysis conditions, and microwave power not reaching the optimal state. In particular, Example 3, due to insufficient enzymatic hydrolysis efficiency, the cellulose hydrolysis products in the film were unevenly distributed, and the biodegradability was still not completely degraded on the 5th day.

[0062] (3) Microscopic morphology Test method: The samples were examined using a FEI F50 SEM (PS216) at 5.0 kV and a 2.0 μm spot size. 20 μL of the treated liquid sample was drop-coated on a silicon substrate and air-dried for 12 h. A 2 nm thick layer of platinum was then sputtered on top to avoid charging. The test results are shown in Figure 2. Figure 1-Figure 4 shown.

[0063] Good solubility is the primary prerequisite for cellulose and its derivatives to enhance the mechanical strength of the film. Only when these materials are well dissolved in the liquid formulation can their fibers unfold and integrate into the microstructure of the film, thereby improving its mechanical strength. Figure 4 The surface of the biodegradable film without cellulose added in d-1 (Comparative Example 3) is clear and free of impurities. Figure 3c-1 (Example 1) The surface of the biodegradable film prepared from the Kombucha cellulose hydrolysate is uniformly dispersed with nanoparticles, which is because the Kombucha cellulose hydrolysate evenly dissolves the particles in the film formula. This shows that some cellulose materials on the surface of the biodegradable film prepared from the Kombucha cellulose hydrolysate are well integrated into the film, which is the reason for its improved mechanical strength. Figure 1 As can be seen from a-1 (Comparative Example 1), the particles on the film containing intact kombucha cellulose are relatively large, about 300 μm in size. The uneven structure not only makes the surface rough, but also deforms the surface. Figure 1 A-2 Figure 2 B-2 Figure 3 C-2 Figure 4 D-2, Figure 2 b-2 (Comparative Example 2), Figure 3 c-2 (Example 1) than Figure 1 a-2 (Comparative Example 1), Figure 4 The edges of d-2 (Comparative Example 3) are much neater, and the mechanical strength is also relatively high, indicating that hydrolysis greatly reduces the particle size of intact cellulose and increases solubility, thereby improving the mechanical strength of the resulting film to a certain extent. Figure 2 b-2 (Comparative Example 2) and Figure 3 The stripe-like structure can be observed on c-2 (Example 1). This is because although the kombucha cellulose loses its long strings and cross-linked network structure after hydrolysis, it has better solubility due to the reduced particle size. The remaining string-like structure unfolds and extends to the internal structure of the film, showing multiple stripe edges, which is also the reason why the mechanical strength of the film is significantly improved. Figure 3 It is more obvious in c-2 (Example 1), and Example 1 shows higher mechanical strength, which shows that compared with homogenization, microwave treatment can make the string structure arranged in the film more orderly, so that the film has higher mechanical strength.

[0064] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a kombucha cellulose film, characterized in that: The following steps are involved: (1) enzymatically hydrolyzing kombucha cellulose with cellulase and simultaneously homogenizing the cellulose to obtain a cellulose hydrolyzate; (2) The cellulose hydrolysate, thickener and cross-linking agent are dispersed in a solvent and mixed under the action of microwaves to obtain a suspension; the microwave power is 70-90 W, the mixing temperature is 50-70 °C, and the mixing time is 10-20 min; the microstructure of the cellulose hydrolysate in the suspension is spherical with a particle size of 0.5-1 μm; (3) Form the suspension into a thin film.

2. The method for preparing a kombucha cellulose film according to claim 1, characterized in that: The kombucha cellulose is purified before enzymatic hydrolysis, and the purification steps are: dispersing the kombucha cellulose in water, first treating it with alkali, then treating it with acid, and washing it with water.

3. The method for preparing a kombucha cellulose film according to claim 2, characterized in that: The alkali treatment step is: treating with 0.5-2 mol / L NaOH solution at 48-53°C for 10-12 h; the acid treatment step is: treating with 1-2% mass concentration glacial acetic acid for 1-2 h; washing with water until neutral, and freeze-drying.

4. The method for preparing a kombucha cellulose film according to claim 1, characterized in that: The enzymatic hydrolysis conditions are as follows: the mass ratio of enzyme to substrate is 1-3%, the enzymatic hydrolysis is performed at 30-50°C for 8-30 min, and the homogenization speed is 8000-12000 rpm.

5. The method for preparing a kombucha cellulose film according to claim 1 or 4, characterized in that: The mass concentration of Kombucha cellulose enzymatic hydrolysis is 5-7%.

6. The method for preparing a kombucha cellulose film according to claim 1, characterized in that: The concentration of the cellulose hydrolysate is 0.04-0.5 g / mL; the mass of the thickener is 12-17% of the cellulose hydrolysate, and the mass of the cross-linking agent is 6-10% of the cellulose hydrolysate.

7. The method for preparing a kombucha cellulose film according to claim 1, characterized in that: The suspension is sterilized at high temperature and dried to obtain a film.

8. The method for preparing a kombucha cellulose film according to claim 7, characterized in that: The temperature for high temperature sterilization is 110-130 ℃, and the time is 20-40 min; the temperature for drying is 40-50 ℃, and the time is 15-25 h.

9. A kombucha cellulose film, prepared by the preparation method according to any one of claims 1 to 8.

10. The kombucha cellulose film according to claim 9, characterized in that: The tensile strength of the Kombucha cellulose film is ≥ 18MPa, and the degradation performance is that it starts to degrade from the first day and is completely degraded within 5 days.

Citation Information

Patent Citations

  • Transparent reproductive bacterial cellulose reproductive membrane as well as preparation method and application thereof

    CN104587516A

  • Preparation method of orderly nanofiber membrane based on bacterial cellulose

    CN105384957A

  • Preparation method of liquorice root cellulose and composite microporous diaphragm

    CN107012185A

  • Method for preparing hemicellulose film by high-consistency disc refiner

    CN109867803A

  • Biodegradable thin film material based on enteromorpha extract as well as preparation method and application of biodegradable thin film material

    CN114409968A