Special resin for biaxially oriented polypropylene lithium battery diaphragm and preparation method thereof

By mixing polypropylene resin and additives in a twin-screw extruder, special resin for bidirectional stretched lithium battery separator is prepared, which solves the problems of low β crystal content and uneven pore size distribution, and achieves a more uniform pore size distribution and simplified Process flow.

CN119039696APending Publication Date: 2024-11-29NORTH HUAJIN CHEM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411070930.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing dry bidirectional stretched lithium battery separators have low β crystal content and uneven pore size distribution, making the preparation process complex.

Method used

A twin-screw extruder is used to mix polypropylene resin, nucleating agent, main antioxidant, auxiliary antioxidant and acid absorbent to prepare a two-way stretched polypropylene lithium battery separator special resin powder, by controlling the temperature and rotation speed A uniform pore size distribution is obtained.

Benefits of technology

It improves the uniformity of β crystal content and pore size distribution, simplifies the preparation process, and improves the performance of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039696A_ABST
    Figure CN119039696A_ABST
Patent Text Reader

Abstract

The invention provides resin special for a biaxially oriented polypropylene lithium battery diaphragm and a preparation method of the resin. The preparation method comprises the following steps: mixing polypropylene resin, a nucleating agent, a main antioxidant, an auxiliary antioxidant and an acid acceptor; and after mixing, extruding and granulating by a double-screw extruder to obtain the special resin powder for the biaxially oriented polypropylene lithium battery diaphragm. The invention focuses on research on the formula of the resin aid for the biaxially oriented polypropylene lithium battery diaphragm, and can solve the problems of low beta crystal content and non-uniform pore size distribution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyolefin applications, and in particular relates to a biaxially oriented polypropylene lithium battery diaphragm special resin and a preparation method thereof. Background Art

[0002] As an important component of lithium batteries, the separator plays the role of separating the positive and negative electrodes, preventing direct contact short circuits, allowing lithium ion transmission, and storing electrolytes. At present, the development of base membranes is mainly based on dry polypropylene separators and wet polyethylene separators. Dry polypropylene separators are also divided into dry uniaxial stretching and dry biaxial stretching. Their main features are low cost, safety and environmental protection. Dry biaxial stretching polypropylene can effectively improve the transverse strength and has attracted much attention. However, the problem of uniform pore formation still needs to be solved.

[0003] Chinese patent application CN 108346764A discloses a method for preparing a dry biaxially stretched lithium battery separator. Although a lithium battery microporous membrane with a high content of β crystals can be prepared, the pore size distribution is poor and the preparation process is complicated. Chinese patent application CN104513424A discloses a polypropylene resin for dry-stretched lithium battery separator and a preparation method thereof. Through process control, a polypropylene resin with a wide molecular weight distribution is produced for dry-stretched film formation to manufacture lithium battery separators. However, this method has a low β crystal content.

[0004] At present, although research on dry-stretched lithium battery separators has been carried out at home and abroad, the preparation process is complicated, the product β-crystal content is low, and the pore size distribution is uneven. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] The invention provides a biaxially oriented polypropylene lithium battery separator resin and a preparation method thereof, so as to solve the technical problems of low β-crystal content and uneven pore size distribution.

[0007] (II) Technical solution

[0008] In order to solve the above technical problems, the present invention provides a method for preparing a biaxially oriented polypropylene lithium battery separator resin, the preparation method comprising the following steps:

[0009] S1. Mixing polypropylene resin, nucleating agent, primary antioxidant, secondary antioxidant and acid absorbent;

[0010] S2. After mixing, the mixture is extruded and granulated by a twin-screw extruder to obtain a biaxially oriented polypropylene lithium battery separator resin powder.

[0011] Furthermore, the preparation method comprises the following steps:

[0012] S1. By weight, 100 parts of polypropylene resin, 0.01 to 0.02 parts of nucleating agent, 0.02 to 0.04 parts of primary antioxidant, 0.02 to 0.03 parts of secondary antioxidant, 0.01 to 0.02 parts of acid absorbent are mixed;

[0013] S2. After mixing, the mixture is extruded and granulated through a twin-screw extruder to obtain a biaxially oriented polypropylene lithium battery separator resin powder. The temperatures of each section of the screw are 180-200°C, 190-210°C, 190-220°C, 200-230°C, 190-220°C, 90-210°C, the die temperature is 180-220°C, and the screw speed is 160-220rpm.

[0014] Furthermore, the grade of the polypropylene resin is T30S, and the melt mass flow rate is 3.0 g / 10 min.

[0015] Furthermore, the nucleating agent is TMB-5, SiO 2 , NP-328, NAB-82 or more.

[0016] Furthermore, the main antioxidant is one or more of 1010, 1076, 697, and 3114.

[0017] Furthermore, the secondary antioxidant is one of 168, 626, and 686.

[0018] Furthermore, the acid absorbent is calcium stearate or synthetic hydrotalcite.

[0019] In addition, the present invention also provides a biaxially oriented polypropylene lithium battery separator special resin, which is prepared by the above method.

[0020] (III) Beneficial effects

[0021] The present invention provides a biaxially oriented polypropylene lithium battery separator resin and a preparation method thereof, comprising mixing polypropylene resin, a nucleating agent, a primary antioxidant, a secondary antioxidant, and an acid absorbent; after mixing, extruding and granulating through a twin-screw extruder to obtain a biaxially oriented polypropylene lithium battery separator resin powder. The present invention focuses on the research of the formula of the resin additive for the biaxially oriented polypropylene lithium battery separator, which can solve the problems of low β-crystal content and uneven pore size distribution. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Graph showing the pore size distribution of the embodiments of the present invention and the comparative example. DETAILED DESCRIPTION

[0023] In order to make the purpose, content and advantages of the present invention more clear, the specific implementation methods of the present invention are further described in detail below in conjunction with the drawings and examples.

[0024] Example 1

[0025] By weight, 100 parts of polypropylene resin, 0.01 parts of β-nucleating agent TMB-5, 0.03 parts of primary antioxidant 1010, 0.02 parts of auxiliary antioxidant 686, and 0.01 parts of acid absorber synthetic hydrotalcite are mixed at high speed and extruded into granules through a twin-screw extruder. The temperatures of the screw sections are 190°C, 200°C, 210°C, 220°C, 220°C, and 205°C, respectively. The die temperature is 195°C and the screw speed is 170rpm.

[0026] Example 2

[0027] By weight, 100 parts of polypropylene resin, 0.015 parts of β-nucleating agent NP-328, 0.04 parts of primary antioxidant 1076, 0.02 parts of auxiliary antioxidant 168, and 0.01 parts of acid absorber calcium stearate are mixed at high speed and then extruded into granules through a twin-screw extruder. The temperatures of the screw sections are 195°C, 205°C, 215°C, 225°C, 225°C, and 215°C, respectively. The die temperature is 190°C and the screw speed is 180rpm.

[0028] Example 3

[0029] By weight, 100 parts of polypropylene resin, 0.01 parts by weight of β-nucleating agent NAB-82, 0.03 parts of primary antioxidant 1010, 0.02 parts of auxiliary antioxidant 686, and 0.01 parts of acid absorber synthetic hydrotalcite are mixed at high speed and extruded into granules through a twin-screw extruder. The temperatures of the screw sections are 190°C, 200°C, 210°C, 220°C, 220°C, and 205°C, respectively. The die temperature is 195°C and the screw speed is 170rpm.

[0030] Example 4

[0031] By weight, 100 parts of polypropylene resin, 0.015 parts by weight of β-nucleating agent NP-328, 0.01 parts of primary antioxidant 3114, 0.02 parts of primary antioxidant 697, 0.02 parts of auxiliary antioxidant 626, and 0.01 parts of acid absorber calcium stearate are mixed at high speed and then extruded into granules through a twin-screw extruder. The temperatures of the screw sections are 195°C, 205°C, 215°C, 225°C, 225°C, and 215°C, respectively. The die temperature is 190°C and the screw speed is 180rpm.

[0032] Example 5

[0033] According to weight, 100 parts of polypropylene resin, 0.01 parts of β-nucleating agent NP-328, 0.01 parts of β-nucleating agent SiO 2, 0.015 parts of main antioxidant 1010, 0.01 parts of main antioxidant 1076, 0.02 parts of auxiliary antioxidant 168, and 0.01 parts of acid absorber calcium stearate. After high-speed mixing, they are extruded and granulated through a twin-screw extruder. The temperatures of each section of the screw are 195°C, 205°C, 215°C, 225°C, 225°C, and 215°C respectively. The die temperature is 190°C and the screw speed is 190rpm.

[0034] Comparative Example

[0035] By weight, 100 parts of polypropylene resin, 0.03 parts of primary antioxidant 1010, 0.02 parts of auxiliary antioxidant 168, and 0.01 parts of acid absorber calcium stearate are mixed at high speed and extruded into granules through a twin-screw extruder. The temperatures of the screw sections are 185°C, 200°C, 210°C, 220°C, 220°C, and 210°C, respectively. The die temperature is 190°C and the screw speed is 180rpm.

[0036] The resins prepared in the above examples and comparative examples were subjected to tensile yield stress test, bending strength test and β crystal content determination. The tensile yield stress test was determined using the national standard GB / T 1040.2-2022, the bending strength test was determined using the national standard GB / T9341-2008, and the β crystal content was determined using the DSC method at a heating rate of 20°C / min and a temperature of 23-210°C. The test results are shown in Table 1. The pore size distribution was characterized and statistically analyzed by using ImageJ software on the diaphragm. Figure 1 shown.

[0037] Table 1 Tensile yield stress, flexural strength and β crystal content of the embodiments and comparative examples

[0038]

[0039] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a biaxially oriented polypropylene lithium battery separator resin, characterized in that: The preparation method comprises the following steps: S1. The polypropylene resin, nucleating agent, primary antioxidant, secondary antioxidant, acid scavenger are mixed; S2. After mixing, the mixture is extruded and granulated through a twin-screw extruder to obtain a biaxially oriented polypropylene resin powder specifically for lithium battery separators.

2. The method for preparing a biaxially oriented polypropylene resin for lithium battery separators according to claim 1, wherein: The preparation method comprises the following steps: S1. In parts by weight, 100 parts of polypropylene resin, 0.01 to 0.02 parts of nucleating agent, 0.02 to 0.04 parts of primary antioxidant, 0.02 to 0.03 parts of secondary antioxidant, 0.01 to 0.02 parts of acid scavenger are mixed; S2. After mixing, the mixture is extruded and granulated through a twin-screw extruder to obtain a biaxially oriented polypropylene resin powder for lithium battery separators. The temperatures of each section of the screw are 180-200°C, 190-210°C, 190-220°C, 200-230°C, 190-220°C, and 90-210°C, respectively. The die temperature is 180-220°C, and the screw speed is 160-220rpm.

3. The method for preparing a biaxially oriented polypropylene resin for lithium battery separators according to claim 1 or 2, characterized in that: The polypropylene resin is T30S, and its melt mass flow rate is 3.0 g / 10 min.

4. The method for preparing a biaxially oriented polypropylene resin for lithium battery separators according to claim 1 or 2, characterized in that: The nucleating agent is one or more of TMB-5, SiO2, NP-328, and NAB-82.

5. The method for preparing a biaxially oriented polypropylene resin for lithium battery separators according to claim 1 or 2, characterized in that: The main antioxidant is one or more of 1010, 1076, 697, and 3114.

6. The method for preparing a biaxially oriented polypropylene resin for lithium battery separators according to claim 1 or 2, characterized in that: The secondary antioxidant is one of 168, 626, and 686.

7. The method for preparing a biaxially oriented polypropylene resin for lithium battery separators according to claim 1 or 2, characterized in that: The acid scavenger is calcium stearate or synthetic hydrotalcite.

8. A biaxially oriented polypropylene resin for lithium battery separators, characterized in that: The resin is prepared by the method according to any one of claims 1 to 7.