Heat insulation foam rubber material for air conditioner air pipe and preparation method of heat insulation foam rubber material
Through the blending of ethylene propylene ternary rubber and neoprene rubber and the combination of modifier, combined with slag wool and polytetrafluoroethylene fine particle resin, the problem of insufficient thermal insulation performance and mechanical strength of air conditioning duct materials is solved, and the problem of insufficient thermal insulation performance and mechanical strength of air conditioning duct materials is realized. More efficient insulation and insulation effects.
Patent Information
- Application Number
- CN202411400309.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The thermal insulation and mechanical strength of existing air conditioning duct materials are insufficient and cannot be maintained for long-term use, resulting in reduced efficiency and energy-saving effects of the air conditioning system.
Foam rubber materials are prepared by blending ethylene propylene rubber and neoprene rubber, and a combination of modifiers such as polyvinyl alcohol-loaded hydroxy polypropylene microspheres and graphene aerogels are formed to form a three-dimensional mesh structure to enhance heat insulation. and mechanical properties, and slag wool and polytetrafluoroethylene fine particle resin can be used to enhance the insulation performance and stability of the material.
It significantly improves the thermal insulation and mechanical strength of air conditioning duct materials, improves flame retardant performance and aging resistance, extends the service life of the material, reduces heat conduction and gas convection, and improves the overall insulation effect.
Abstract
Description
Technical Field
[0001] The present application relates to the field of rubber materials, and more specifically, to a heat insulating foam rubber material for air ducts of air conditioners and a preparation method thereof. Background Art
[0002] Air ducts are an important part of the air conditioning system, used to deliver cold or heated air to various rooms or areas. Choosing the right duct material and designing a reasonable duct system are essential to ensure efficient operation, energy saving and comfort of the air conditioning system.
[0003] In the related art, a duct material includes the following raw materials: 90 kg high-density polyethylene, 3 kg linear low-density polyethylene, 3 kg tert-butyl perbenzoate, 2 kg talcum powder, and 2 kg sodium bicarbonate as a foaming agent.
[0004] The preparation method comprises the following steps: taking raw materials according to a ratio, stirring and mixing for 3 minutes, granulating in a twin-screw extruder at a temperature of 180°C and a screw speed of 300 r / min to obtain a polyethylene composite material, and then blow-molding the polyethylene composite material.
[0005] The above-mentioned duct materials are light in weight and low in cost, but their thermal insulation performance is average and their mechanical strength is also low, so they cannot maintain long-term use, thereby reducing the use effect of the air conditioning duct. Summary of the invention
[0006] In order to improve the thermal insulation performance and mechanical strength of air duct materials for air conditioners, the present application provides a thermal insulation foam rubber material for air ducts for air conditioners and a preparation method thereof.
[0007] In a first aspect, the present application provides a thermal insulation foam rubber material for air ducts of air conditioners, which adopts the following technical solution: A heat-insulating foam rubber material for air-conditioning ducts, comprising the following raw materials in parts by weight: 70 parts of EPDM rubber masterbatch; 30 parts of chloroprene rubber masterbatch; Antiaging agent 4010-NA 0.5-2 parts; 3-7 parts of zinc oxide; Accelerator DM 1 to 1.5 parts; Accelerator Na-22 0.5-1.5 parts; Accelerator TMTD 3-5 parts; 1-2 parts of sulfur; Foaming agent AC 7-11 parts; Modifier 6-10 parts; The modifier includes polyvinyl alcohol, hydroxy polypropylene microspheres and graphene aerogel, the polyvinyl alcohol is loaded inside the hydroxy polypropylene microspheres, the graphene aerogel is loaded outside the hydroxy polypropylene microspheres, and the weight ratio of the polyvinyl alcohol, the hydroxy polypropylene microspheres and the graphene aerogel is 5:8:1.
[0008] By adopting the above technical solutions, both chloroprene rubber (CR) and ethylene propylene diene monomer rubber (EPDM) have good aging resistance and are rubber materials with excellent performance. Ethylene propylene diene monomer rubber (EPDM) also has excellent electrical insulation and low-temperature flexibility, and its foamed materials are often used as heat insulation and insulating materials. However, EPDM has poor flame retardant properties, self-adhesion, and mutual adhesion, which to a certain extent limits the application of EPDM. Chloroprene rubber (CR) has excellent flame retardant properties, and has large initial adhesion and high bonding strength. The foam rubber material prepared by blending CR and EPDM not only has the characteristics of heat insulation and aging resistance, but also has greatly improved flame retardant properties.
[0009] The modifier is made of polyvinyl alcohol, hydroxy polypropylene microspheres and graphene aerogel. The polyvinyl alcohol is loaded inside the hydroxy polypropylene microspheres, and the graphene aerogel is loaded outside the hydroxy polypropylene microspheres. The graphene aerogel is gradually separated from the hydroxy polypropylene microspheres. As the mixed rubber is vulcanized and foamed, the temperature gradually increases, the foaming agent AC decomposes faster, and the pores begin to nucleate and grow. During the pore nucleation process, the graphene aerogel is gradually separated from the hydroxy polypropylene microspheres and dispersed between the pores to form a three-dimensional network structure for stabilizing the pores, reducing surface tension, and maintaining a high nucleation density and a stable pore growth rate. In the pore growth stage, the polyvinyl alcohol inside the hydroxy polypropylene microspheres is gradually released, increasing the surface tension, thereby inhibiting the expansion of the formed pores, and tending to keep the bubbles in a regular spherical shape, thereby improving the stability of the material; when the pores merge, the merging between the pores is inhibited, so that the pores are more evenly distributed and smaller in size, thereby improving the consistency of the overall thermal insulation performance and mechanical properties of the material. Graphene aerogel can also adjust the surface tension not to increase too much, thereby reducing the situation of pore rupture to form perforations or openings, and making the pores as closed-cell structure as possible. The closed-cell structure can better prevent gas convection and reduce heat conduction, thus having better thermal insulation performance. In addition to playing a load role, hydroxy polypropylene microspheres are also dispersed between the foams to disperse stress, thereby improving the mechanical strength of the material. Therefore, the effect of improving the thermal insulation performance and mechanical strength of the air conditioning duct material is obtained.
[0010] Optionally, the EPDM rubber masterbatch includes the following raw materials: EPDM rubber, carbon black, zinc oxide, stearic acid, hollow glass microspheres, and the weight ratio of the EPDM rubber, carbon black, zinc oxide, stearic acid and hollow glass microspheres is 100:20:5:3:2.
[0011] By adopting the above technical scheme, the EPDM rubber masterbatch of this formula has excellent mechanical strength, especially the addition of hollow glass microspheres has a lubricating effect, which can effectively improve the mixing effect of various raw materials in the EPDM rubber masterbatch and improve the thermal insulation performance of the thermal insulation foam rubber material.
[0012] Optionally, the preparation method of the EPDM rubber masterbatch is: take each raw material in sequence according to the amount, plasticize the EPDM rubber at 100-120°C for 4-6 minutes, then add zinc oxide, stearic acid, carbon black and hollow glass microbeads in sequence, maintain the temperature and continue mixing for 4-6 minutes to obtain the EPDM rubber masterbatch.
[0013] Optionally, the chloroprene rubber masterbatch comprises the following raw materials: chloroprene rubber, magnesium oxide, stearic acid and calcium carbonate, and the weight ratio of the chloroprene rubber, magnesium oxide, stearic acid and calcium carbonate is 100:4:3:1.
[0014] By adopting the above technical solution, the chloroprene rubber masterbatch of this formula can contribute excellent mechanical strength to the thermal insulation foam rubber material, especially the addition of calcium carbonate has a good reinforcing effect on the chloroprene rubber masterbatch.
[0015] Optionally, the preparation method of the chloroprene rubber masterbatch is: take each raw material in order according to the amount, plasticize the chloroprene rubber at 60-90° C. for 4-6 minutes, then add magnesium oxide, stearic acid and calcium carbonate in order while maintaining the temperature, and continue mixing for 4-6 minutes to obtain the chloroprene rubber masterbatch.
[0016] Optionally, the preparation method of the modifier is: Dissolving polyvinyl alcohol in water to form a polyvinyl alcohol solution, dissolving hydroxy polypropylene microspheres in dichloromethane to form a hydroxy polypropylene microsphere solution, and dropping the polyvinyl alcohol solution into the hydroxy polypropylene microsphere solution, stirring to make it evenly dispersed; The mixed solution is added to the aqueous phase containing gelatin to form a stable emulsion, and the organic solvent is gradually evaporated by stirring and heating to embed the polyvinyl alcohol inside the hydroxy polypropylene microspheres, and the hydroxy polypropylene microspheres loaded with polyvinyl alcohol are prepared by washing and drying. The graphene aerogel powder is evenly dispersed in water to form a suspension, a silane coupling agent is added to the suspension, and the mixture is stirred until uniform. Then, hydroxyl polypropylene microspheres loaded with polyvinyl alcohol are added to the suspension, and the mixture is stirred sufficiently to make the surface of the microspheres evenly covered with graphene aerogel. The mixture is reacted for 24 hours, and the microspheres loaded with graphene aerogel are separated by centrifugation and dried to obtain a modifier.
[0017] By adopting the above technical scheme, the prepared modifier can effectively improve the pore structure and size of the thermal insulation foam rubber material, thereby improving the thermal insulation performance and mechanical strength of the thermal insulation foam rubber material.
[0018] Optionally, the thermal insulation foam rubber material also includes slag wool and polytetrafluoroethylene fine particle resin, the weight portion of slag wool is 3 to 5 parts, and the weight portion of polytetrafluoroethylene fine particle resin is 4 to 6 parts.
[0019] By adopting the above technical scheme, slag wool and polytetrafluoroethylene fine particle resin are compounded, the slag wool contains a large number of micropores and macropores, the fibers are interwoven to form a dense porous grid, and the polytetrafluoroethylene fine particle resin is entangled between the slag wool fibers, which can not only synergistically improve the mechanical strength of the thermal insulation foam rubber material, but also effectively reduce the damage of the slender ends of the fibers to the internal pores of the thermal insulation foam rubber material, thereby effectively exerting the thermal insulation effect of the slag wool.
[0020] In a second aspect, the present application provides a method for preparing a heat insulating foam rubber material for an air conditioning duct, using the following technical solution: A method for preparing a heat-insulating foam rubber material for an air duct of an air conditioner comprises the following steps: (1) Prepare modifier, EPDM rubber masterbatch and chloroprene rubber masterbatch respectively, weigh each raw material according to the amount used and set aside; (2) Mix EPDM rubber masterbatch, chloroprene rubber masterbatch, antioxidant 4010-NA and modifier at 60-90° C. for 4-6 minutes to prepare a rubber mixture; (3) Add zinc oxide, accelerator DM, accelerator Na-22 and accelerator TMTD to the mixed rubber in sequence and mix evenly, then add sulfur and foaming agent AC in sequence, mix evenly, form sheets, and let stand at room temperature for 24 hours; (4) The mixed rubber is subjected to compression vulcanization foaming with the following process parameters: temperature 180-220°C, pressure 6-8 MPa, time 3-5 min, to obtain a heat insulating foam rubber material.
[0021] By adopting the above technical scheme, through step-by-step mixing and vulcanization, the heat insulating foam rubber material obtained has excellent heat insulating performance and mechanical strength.
[0022] In a third aspect, the present application provides a method for preparing a heat insulating foam rubber material for an air duct of an air conditioner, using the following technical solution: A method for preparing a heat-insulating foam rubber material for an air duct of an air conditioner comprises the following steps: (1) Prepare modifier, EPDM rubber masterbatch and chloroprene rubber masterbatch respectively, weigh each raw material according to the amount used and set aside; (2) Mix EPDM rubber masterbatch, chloroprene rubber masterbatch, antioxidant 4010-NA, modifier, slag wool and polytetrafluoroethylene fine particle resin at 60-90° C. for 4-6 minutes to prepare a mixed rubber; (3) Add zinc oxide, accelerator DM, accelerator Na-22 and accelerator TMTD to the mixed rubber in sequence and mix evenly, then add sulfur and foaming agent AC in sequence, mix evenly, form sheets, and let stand at room temperature for 24 hours; (4) The mixed rubber is subjected to compression vulcanization foaming with the following process parameters: temperature 180-220°C, pressure 6-8 MPa, time 3-5 min, to obtain a heat insulating foam rubber material.
[0023] By adopting the above technical solution, the obtained heat insulating foam rubber material has better heat insulating performance and mechanical strength.
[0024] In summary, this application has the following beneficial effects: 1. Since the foam rubber material prepared by blending CR and EPDM in this application not only has the characteristics of heat insulation and aging resistance, but also has greatly improved flame retardant properties. The modifier can effectively improve the pore structure, thereby achieving the effect of improving the heat insulation and mechanical strength of the air conditioning duct material.
[0025] 2. In the present application, slag wool and polytetrafluoroethylene fine-particle resin are preferably used in combination. The polytetrafluoroethylene fine-particle resin is entangled between the slag wool fibers, which can not only synergistically improve the mechanical strength of the thermal insulation foam rubber material, but also effectively reduce the damage of the slender ends of the fibers to the internal pores of the thermal insulation foam rubber material, thereby effectively exerting the thermal insulation effect of the slag wool.
[0026] 3. The method of the present application, through step-by-step mixing and vulcanization, obtains a thermal insulation foam rubber material having excellent thermal insulation performance and mechanical strength. DETAILED DESCRIPTION
[0027] The present application is further described in detail with reference to the following examples. It is specially noted that if no specific conditions are specified in the following examples, the conventional conditions or the conditions recommended by the manufacturer are followed, and the raw materials used in the following examples can be obtained from common commercial sources unless otherwise specified.
[0028] EPDM rubber, industrial grade, brand EP 35.
[0029] Carbon black, type N-330.
[0030] Hollow glass microspheres, particle size 30μm.
[0031] Neoprene, technical grade, grade CR 126.
[0032] Foaming agent AC, industrial grade, Shanghai Xiangyang Chemical Co., Ltd.
[0033] Polyvinyl alcohol, type 1799, CAS number: 9002-89-5.
[0034] Hydroxypropylene microspheres were purchased from Beijing Zhongke Keyou Technology Co., Ltd. with a particle size of 50 nm.
[0035] Graphene aerogel was purchased from Xi’an Qiyue Biotechnology Co., Ltd.
[0036] Polytetrafluoroethylene fine particle resin was purchased from Shandong Huafu Chemical Co., Ltd., model 4S02-C. Example Example 1
[0037] A heat-insulating foam rubber material for air-conditioning ducts, comprising the following raw materials in the following amounts: EPDM masterbatch 70kg; Neoprene masterbatch 30kg; Anti-aging agent 4010-NA 0.5kg; Zinc oxide 3kg; Accelerator DM 1kg; Accelerator Na-22 0.5kg; Accelerator TMTD 3kg; Sulfur 1kg; Foaming agent AC 7kg; Modifier 6kg.
[0038] The EPDM rubber masterbatch includes the following raw materials: EPDM rubber, carbon black, zinc oxide, stearic acid, and hollow glass microspheres. The usage ratio of the EPDM rubber, carbon black, zinc oxide, stearic acid, and hollow glass microspheres is 100:20:5:3:2.
[0039] The chloroprene rubber masterbatch includes the following raw materials: chloroprene rubber, magnesium oxide, stearic acid and calcium carbonate, and the usage ratio of chloroprene rubber, magnesium oxide, stearic acid and calcium carbonate is 100:4:3:1.
[0040] The modifier includes polyvinyl alcohol, hydroxy polypropylene microspheres and graphene aerogel, the polyvinyl alcohol is loaded inside the hydroxy polypropylene microspheres, the graphene aerogel is loaded outside the hydroxy polypropylene microspheres, and the usage ratio of polyvinyl alcohol, hydroxy polypropylene microspheres and graphene aerogel is 5:8:1.
[0041] A method for preparing a heat-insulating foam rubber material for an air duct of an air conditioner comprises the following steps: (1) Preparation of modifier: 5 kg of polyvinyl alcohol was dissolved in water to form a polyvinyl alcohol solution, 8 kg of hydroxy polypropylene microspheres were dissolved in dichloromethane to form a hydroxy polypropylene microsphere solution, the polyvinyl alcohol solution was added dropwise to the hydroxy polypropylene microsphere solution, and stirred to make it evenly dispersed.
[0042] The mixed solution is added to the aqueous phase containing gelatin to form a stable emulsion, and the amount of gelatin used is 2% of the total mass of the emulsion. The organic solvent is gradually evaporated by stirring and heating, so that the polyvinyl alcohol is embedded in the hydroxy polypropylene microspheres, and the hydroxy polypropylene microspheres loaded with polyvinyl alcohol are obtained by washing and drying.
[0043] 1 kg of graphene aerogel powder was evenly dispersed in water and ultrasonically treated to form a suspension. An appropriate amount of 0.02 kg of silane coupling agent was added to the suspension and stirred until uniform. Then, hydroxy polypropylene microspheres loaded with polyvinyl alcohol were added to the suspension, stirred thoroughly, and ultrasonically treated for 30 minutes to make the surface of the microspheres evenly covered with graphene aerogel. The reaction was carried out for 24 hours, and the microspheres loaded with graphene aerogel were separated by centrifugation and dried to obtain a modifier.
[0044] Preparation of EPDM rubber masterbatch: 100 kg of EPDM rubber was plasticized at 100°C for 6 min, and then 5 kg of zinc oxide, 3 kg of stearic acid, 20 kg of carbon black and 2 kg of hollow glass microspheres were added in sequence, and the temperature was maintained and the mixing was continued for 6 min to obtain the EPDM rubber masterbatch.
[0045] Preparation of chloroprene rubber masterbatch: 100 kg of chloroprene rubber was plasticized at 60°C for 6 min, and then 4 kg of magnesium oxide, 3 kg of stearic acid and 1 kg of calcium carbonate were added in sequence while maintaining the temperature, and mixing was continued for 6 min to obtain a chloroprene rubber masterbatch.
[0046] Weigh each raw material of the thermal insulation foam rubber material according to the required amount and set aside.
[0047] (2) Mixing EPDM rubber masterbatch, chloroprene rubber masterbatch, antioxidant 4010-NA and modifier at 60°C for 6 minutes to prepare a rubber mixture; (3) Add zinc oxide, accelerator DM, accelerator Na-22 and accelerator TMTD to the mixed rubber in sequence and mix evenly, then add sulfur and foaming agent AC in sequence, mix evenly, form sheets, and let stand at room temperature for 24 hours; (4) The rubber mixture is subjected to compression vulcanization foaming with the following process parameters: temperature 180°C, pressure 6 MPa, time 5 min, to obtain a thermal insulation foam rubber material. Example 2
[0048] A heat-insulating foam rubber material for air-conditioning ducts, comprising the following raw materials in the following amounts: EPDM masterbatch 70kg; Neoprene masterbatch 30kg; Anti-aging agent 4010-NA 1kg; Zinc oxide 5kg; Accelerator DM 1.2kg; Accelerator Na-22 1kg; Accelerator TMTD 4kg; Sulfur 1.5kg; Foaming agent AC 9kg; Modifier 8kg.
[0049] The EPDM rubber masterbatch includes the following raw materials: EPDM rubber, carbon black, zinc oxide, stearic acid, and hollow glass microspheres. The usage ratio of the EPDM rubber, carbon black, zinc oxide, stearic acid, and hollow glass microspheres is 100:20:5:3:2.
[0050] The chloroprene rubber masterbatch includes the following raw materials: chloroprene rubber, magnesium oxide, stearic acid and calcium carbonate, and the usage ratio of chloroprene rubber, magnesium oxide, stearic acid and calcium carbonate is 100:4:3:1.
[0051] The modifier includes polyvinyl alcohol, hydroxy polypropylene microspheres and graphene aerogel, the polyvinyl alcohol is loaded inside the hydroxy polypropylene microspheres, the graphene aerogel is loaded outside the hydroxy polypropylene microspheres, and the usage ratio of polyvinyl alcohol, hydroxy polypropylene microspheres and graphene aerogel is 5:8:1.
[0052] A method for preparing a heat-insulating foam rubber material for an air duct of an air conditioner comprises the following steps: (1) Preparation of modifier: 5 kg of polyvinyl alcohol was dissolved in water to form a polyvinyl alcohol solution, 8 kg of hydroxy polypropylene microspheres were dissolved in dichloromethane to form a hydroxy polypropylene microsphere solution, the polyvinyl alcohol solution was added dropwise to the hydroxy polypropylene microsphere solution, and stirred to make it evenly dispersed.
[0053] The mixed solution is added to the aqueous phase containing gelatin to form a stable emulsion, and the amount of gelatin used is 2% of the total mass of the emulsion. The organic solvent is gradually evaporated by stirring and heating, so that the polyvinyl alcohol is embedded in the hydroxy polypropylene microspheres, and the hydroxy polypropylene microspheres loaded with polyvinyl alcohol are obtained by washing and drying.
[0054] 1 kg of graphene aerogel powder was evenly dispersed in water and ultrasonically treated to form a suspension. An appropriate amount of 0.02 kg of silane coupling agent was added to the suspension and stirred until uniform. Then, hydroxy polypropylene microspheres loaded with polyvinyl alcohol were added to the suspension, stirred thoroughly, and ultrasonically treated for 30 minutes to make the surface of the microspheres evenly covered with graphene aerogel. The reaction was carried out for 24 hours, and the microspheres loaded with graphene aerogel were separated by centrifugation and dried to obtain a modifier.
[0055] Preparation of EPDM rubber masterbatch: 100 kg of EPDM rubber was plasticized at 110°C for 5 min, and then 5 kg of zinc oxide, 3 kg of stearic acid, 20 kg of carbon black and 2 kg of hollow glass microspheres were added in sequence, and the temperature was maintained and the mixing was continued for 5 min to obtain the EPDM rubber masterbatch.
[0056] Preparation of chloroprene rubber masterbatch: 100 kg of chloroprene rubber was plasticized at 75°C for 5 minutes, and then 4 kg of magnesium oxide, 3 kg of stearic acid and 1 kg of calcium carbonate were added in sequence while maintaining the temperature, and the mixing was continued for 5 minutes to obtain the chloroprene rubber masterbatch.
[0057] Weigh each raw material of the thermal insulation foam rubber material according to the required amount and set aside.
[0058] (2) Mixing EPDM rubber masterbatch, chloroprene rubber masterbatch, antioxidant 4010-NA and modifier at 80°C for 5 minutes to prepare a rubber mixture; (3) Add zinc oxide, accelerator DM, accelerator Na-22 and accelerator TMTD to the mixed rubber in sequence and mix evenly, then add sulfur and foaming agent AC in sequence, mix evenly, form sheets, and let stand at room temperature for 24 hours; (4) The rubber mixture is subjected to compression vulcanization foaming with the following process parameters: temperature 200°C, pressure 7 MPa, time 4 min, to obtain a thermal insulation foam rubber material. Example 3
[0059] A heat-insulating foam rubber material for air-conditioning ducts, comprising the following raw materials in the following amounts: EPDM masterbatch 70kg; Neoprene masterbatch 30kg; Anti-aging agent 4010-NA 2kg; Zinc oxide 7kg; Accelerator DM 1.5kg; Accelerator Na-22 1.5kg; Accelerator TMTD 5kg; Sulfur 2kg; Foaming agent AC 11kg; Modifier 10kg.
[0060] The EPDM rubber masterbatch includes the following raw materials: EPDM rubber, carbon black, zinc oxide, stearic acid, and hollow glass microspheres. The usage ratio of the EPDM rubber, carbon black, zinc oxide, stearic acid, and hollow glass microspheres is 100:20:5:3:2.
[0061] The chloroprene rubber masterbatch includes the following raw materials: chloroprene rubber, magnesium oxide, stearic acid and calcium carbonate, and the usage ratio of chloroprene rubber, magnesium oxide, stearic acid and calcium carbonate is 100:4:3:1.
[0062] The modifier includes polyvinyl alcohol, hydroxy polypropylene microspheres and graphene aerogel, the polyvinyl alcohol is loaded inside the hydroxy polypropylene microspheres, the graphene aerogel is loaded outside the hydroxy polypropylene microspheres, and the usage ratio of polyvinyl alcohol, hydroxy polypropylene microspheres and graphene aerogel is 5:8:1.
[0063] A method for preparing a heat-insulating foam rubber material for an air duct of an air conditioner comprises the following steps: (1) Preparation of modifier: 5 kg of polyvinyl alcohol was dissolved in water to form a polyvinyl alcohol solution, 8 kg of hydroxy polypropylene microspheres were dissolved in dichloromethane to form a hydroxy polypropylene microsphere solution, the polyvinyl alcohol solution was added dropwise to the hydroxy polypropylene microsphere solution, and stirred to make it evenly dispersed.
[0064] The mixed solution is added to the aqueous phase containing gelatin to form a stable emulsion, and the amount of gelatin used is 2% of the total mass of the emulsion. The organic solvent is gradually evaporated by stirring and heating, so that the polyvinyl alcohol is embedded in the hydroxy polypropylene microspheres, and the hydroxy polypropylene microspheres loaded with polyvinyl alcohol are obtained by washing and drying.
[0065] 1 kg of graphene aerogel powder was evenly dispersed in water and ultrasonically treated to form a suspension. An appropriate amount of 0.02 kg of silane coupling agent was added to the suspension and stirred until uniform. Then, hydroxy polypropylene microspheres loaded with polyvinyl alcohol were added to the suspension, stirred thoroughly, and ultrasonically treated for 30 minutes to make the surface of the microspheres evenly covered with graphene aerogel. The reaction was carried out for 24 hours, and the microspheres loaded with graphene aerogel were separated by centrifugation and dried to obtain a modifier.
[0066] Preparation of EPDM rubber masterbatch: 100 kg of EPDM rubber was plasticized at 120°C for 4 min, and then 5 kg of zinc oxide, 3 kg of stearic acid, 20 kg of carbon black and 2 kg of hollow glass microspheres were added in sequence, and the temperature was maintained and the mixing was continued for 4 min to obtain the EPDM rubber masterbatch.
[0067] Preparation of chloroprene rubber masterbatch: 100 kg of chloroprene rubber was plasticized at 90°C for 4 min, and then 4 kg of magnesium oxide, 3 kg of stearic acid and 1 kg of calcium carbonate were added in sequence while maintaining the temperature, and mixing was continued for 4 min to obtain a chloroprene rubber masterbatch.
[0068] Weigh each raw material of the thermal insulation foam rubber material according to the required amount and set aside.
[0069] (2) Mixing EPDM rubber masterbatch, chloroprene rubber masterbatch, antioxidant 4010-NA and modifier at 90°C for 4 minutes to prepare a rubber mixture; (3) Add zinc oxide, accelerator DM, accelerator Na-22 and accelerator TMTD to the mixed rubber in sequence and mix evenly, then add sulfur and foaming agent AC in sequence, mix evenly, form sheets, and let stand at room temperature for 24 hours; (4) The rubber mixture is subjected to compression vulcanization foaming with the following process parameters: temperature 220°C, pressure 8 MPa, time 3 min, to obtain a thermal insulation foam rubber material. Example 4
[0070] The difference between this embodiment and embodiment 2 is that the EPDM rubber masterbatch of this embodiment does not contain hollow glass microbeads. Example 5
[0071] The difference between this embodiment and embodiment 2 is that the chloroprene rubber masterbatch of this embodiment does not contain calcium carbonate. Example 6
[0072] The difference between this embodiment and embodiment 2 is that the EPDM rubber masterbatch of this embodiment does not contain hollow glass microbeads, and the chloroprene rubber masterbatch does not contain calcium carbonate. Example 7
[0073] The difference between this embodiment and embodiment 2 is that the heat insulating foam rubber material of this embodiment further includes slag wool and polytetrafluoroethylene fine granular resin, the amount of slag wool used is 3 kg, and the amount of polytetrafluoroethylene fine granular resin used is 4 kg.
[0074] A method for preparing a heat-insulating foam rubber material for an air duct of an air conditioner comprises the following steps: (1) Preparation of modifier, EPDM rubber masterbatch and chloroprene rubber masterbatch: same as in Example 2.
[0075] Weigh each raw material of the thermal insulation foam rubber material according to the required amount and set aside.
[0076] (2) Mixing EPDM rubber masterbatch, chloroprene rubber masterbatch, antioxidant 4010-NA, modifier, slag wool and polytetrafluoroethylene fine particle resin at 60° C. for 6 minutes to prepare a mixed rubber; (3) Add zinc oxide, accelerator DM, accelerator Na-22 and accelerator TMTD to the mixed rubber in sequence and mix evenly, then add sulfur and foaming agent AC in sequence, mix evenly, form sheets, and let stand at room temperature for 24 hours; (4) The rubber mixture is subjected to compression vulcanization foaming with the following process parameters: temperature 180°C, pressure 6 MPa, time 5 min, to obtain a thermal insulation foam rubber material. Example 8
[0077] The difference between this embodiment and embodiment 2 is that the heat insulating foam rubber material of this embodiment further includes slag wool and polytetrafluoroethylene fine granular resin, the amount of slag wool used is 4 kg, and the amount of polytetrafluoroethylene fine granular resin used is 5 kg.
[0078] A method for preparing a heat-insulating foam rubber material for an air duct of an air conditioner comprises the following steps: (1) Preparation of modifier, EPDM rubber masterbatch and chloroprene rubber masterbatch: same as in Example 2.
[0079] Weigh each raw material of the thermal insulation foam rubber material according to the required amount and set aside.
[0080] (2) Mix EPDM rubber masterbatch, chloroprene rubber masterbatch, antioxidant 4010-NA, modifier, slag wool and polytetrafluoroethylene fine particle resin at 80° C. for 5 minutes to prepare a mixed rubber; (3) Add zinc oxide, accelerator DM, accelerator Na-22 and accelerator TMTD to the mixed rubber in sequence and mix evenly, then add sulfur and foaming agent AC in sequence, mix evenly, form sheets, and let stand at room temperature for 24 hours; (4) The rubber mixture is subjected to compression vulcanization foaming with the following process parameters: temperature 200°C, pressure 7 MPa, time 4 min, to obtain a thermal insulation foam rubber material. Example 9
[0081] The difference between this embodiment and embodiment 2 is that the heat insulating foam rubber material of this embodiment further includes slag wool and polytetrafluoroethylene fine granular resin, the amount of slag wool used is 5 kg, and the amount of polytetrafluoroethylene fine granular resin used is 6 kg.
[0082] A method for preparing a heat-insulating foam rubber material for an air duct of an air conditioner comprises the following steps: (1) Preparation of modifier, EPDM rubber masterbatch and chloroprene rubber masterbatch: same as in Example 2.
[0083] Weigh each raw material of the thermal insulation foam rubber material according to the required amount and set aside.
[0084] (2) Mix EPDM rubber masterbatch, chloroprene rubber masterbatch, antioxidant 4010-NA, modifier, slag wool and polytetrafluoroethylene fine particle resin at 90° C. for 4 minutes to prepare a mixed rubber; (3) Add zinc oxide, accelerator DM, accelerator Na-22 and accelerator TMTD to the mixed rubber in sequence and mix evenly, then add sulfur and foaming agent AC in sequence, mix evenly, form sheets, and let stand at room temperature for 24 hours; (4) The rubber mixture is subjected to compression vulcanization foaming with the following process parameters: temperature 220°C, pressure 8 MPa, time 3 min, to obtain a thermal insulation foam rubber material. Example 10
[0085] The difference between this embodiment and embodiment 8 is that there is no polytetrafluoroethylene fine particle resin in this embodiment. Embodiment 11
[0086] The difference between this embodiment and embodiment 8 is that there is no slag wool in this embodiment. Comparative Example
[0087] Comparative Example 1 A duct material comprises the following raw materials: 90 kg of high-density polyethylene, 3 kg of linear low-density polyethylene, 3 kg of tert-butyl perbenzoate, 2 kg of talcum powder, and 2 kg of sodium bicarbonate as a foaming agent.
[0088] The preparation method comprises the following steps: taking raw materials according to a ratio, stirring and mixing for 3 minutes, granulating in a twin-screw extruder at a temperature of 180°C and a screw speed of 300 r / min to obtain a polyethylene composite material, and then blow-molding the polyethylene composite material.
[0089] Comparative Example 2 The difference between this comparative example and Example 2 is that the modifier in this comparative example does not contain graphene aerogel.
[0090] The modifier includes polyvinyl alcohol and hydroxy polypropylene microspheres. The polyvinyl alcohol is loaded inside the hydroxy polypropylene microspheres, with 5 kg of polyvinyl alcohol and 8 kg of hydroxy polypropylene microspheres.
[0091] The preparation method of the modifier is as follows: polyvinyl alcohol is dissolved in water to form a polyvinyl alcohol solution, hydroxy polypropylene microspheres are dissolved in dichloromethane to form a hydroxy polypropylene microsphere solution, the polyvinyl alcohol solution is added dropwise to the hydroxy polypropylene microsphere solution, and stirred to make it uniformly dispersed. The mixed solution is added to the aqueous phase containing gelatin to form a stable emulsion, and the amount of gelatin used is 2% of the total mass of the emulsion. The organic solvent is gradually evaporated by stirring and heating, and the polyvinyl alcohol is embedded in the hydroxy polypropylene microspheres, and the modifier is obtained by washing and drying.
[0092] Comparative Example 3 The difference between this comparative example and Example 2 is that the modifier in this comparative example does not contain hydroxyl polypropylene microspheres.
[0093] The modifiers include polyvinyl alcohol and graphene aerogel, with 10 kg of polyvinyl alcohol and 2 kg of graphene aerogel.
[0094] The preparation method of the modifier is as follows: polyvinyl alcohol and graphene aerogel are taken according to a ratio, and the polyvinyl alcohol is dissolved in water to form a polyvinyl alcohol solution; the graphene aerogel powder is evenly dispersed in water and ultrasonically treated to form a suspension, 0.04 kg of silane coupling agent is added to the suspension, and stirred until uniform to form a graphene aerogel solution, the two solutions are evenly mixed, ultrasonically dispersed for 30 minutes, spray-dried to evaporate the solvent, and dried to obtain the modifier.
[0095] Comparative Example 4 The difference between this comparative example and Example 2 is that the modifier in this comparative example does not contain polyvinyl alcohol.
[0096] The modifier includes hydroxy polypropylene microspheres and graphene aerogel, 8 kg of hydroxy polypropylene microspheres and 1 kg of graphene aerogel.
[0097] The preparation method of the modifier is as follows: graphene aerogel powder is uniformly dispersed in water, ultrasonically treated to form a suspension, 0.02 kg of silane coupling agent is added to the suspension, stirred until uniform, and then hydroxy polypropylene microspheres are added to the suspension, fully stirred, and ultrasonically treated for 30 minutes to make the surface of the microspheres uniformly covered with graphene aerogel, react for 24 hours, centrifugally separate the microspheres loaded with graphene aerogel, and dry to obtain the modifier.
[0098] Comparative Example 5 The difference between this comparative example and Example 2 is that the modifier in this comparative example is graphene aerogel.
[0099] Comparative Example 6 The difference between this comparative example and Example 2 is that the modifier in this comparative example is hydroxy polypropylene microspheres.
[0100] Comparative Example 7 The difference between this comparative example and Example 2 is that the modifier in this comparative example is polyvinyl alcohol.
[0101] Comparative Example 8 The difference between this comparative example and Example 2 is that the modifier in this comparative example includes polyvinyl alcohol, hydroxy polypropylene microspheres and graphene aerogel, 5 kg of polyvinyl alcohol, 8 kg of hydroxy polypropylene microspheres and 1 kg of graphene aerogel.
[0102] The preparation method of the modifier is as follows: polyvinyl alcohol, hydroxy polypropylene microspheres and graphene aerogel are taken and mixed evenly to obtain the modifier.
[0103] Comparative Example 9 The difference between this comparative example and Example 2 is that there is no modifier in this comparative example.
[0104] Comparative Example 10 The difference between this comparative example and Example 2 is that in this comparative example, chloroprene rubber masterbatch is used to completely replace EPDM rubber masterbatch.
[0105] Comparative Example 11 The difference between this comparative example and Example 2 is that in this comparative example, EPDM rubber masterbatch is used to completely replace chloroprene rubber masterbatch. Performance testing Detection Methods
[0106] 1. Mechanical strength: According to "GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber", the materials prepared in each embodiment and comparative example were used to prepare dumbbell-shaped type 1 specimens. The test was carried out at a speed of 500±50mm / min. Five specimens were taken for each material and the results were averaged. The tensile strength and elongation at break were measured as shown in Table 1.
[0107] According to "GB / T 529-2008 Determination of tear strength of vulcanized rubber or thermoplastic rubber", the materials prepared in each embodiment and comparative example were used to prepare rectangular specimens (with cuts) at a speed of 500±50mm / min for testing. Five specimens were taken for each material for testing, and the results were averaged. The measured tear strengths are shown in Table 1.
[0108] 2. Thermal insulation performance According to "GB / T 10294-2008 Determination of Steady-State Thermal Resistance and Related Properties of Insulating Materials - Guarded Hot Plate Method", samples were prepared from the materials obtained in each embodiment and comparative example. A single specimen vertical device was selected in air to measure the thermal conductivity at room temperature as shown in Table 1.
[0109] 3. Combustion performance According to "GB / T 2406-93 Test Method for Combustion Performance of Plastics", the materials prepared in each embodiment and comparative example were used to prepare type II specimens, and the test was carried out using method A. Five specimens were taken for each material and the results were averaged. The measured oxygen index is shown in Table 1.
[0110] 4. Microscopic morphology of pore structure Take the materials prepared in each embodiment and comparative example, cut a 15mm*15mm*5mm rectangular parallelepiped sample, and observe the cross section of each sample by scanning electron microscope SEM.
[0111] 5. According to "GB / T 3512-2001 Vulcanized rubber or thermoplastic rubber hot air accelerated aging and heat resistance test", take the materials prepared in each embodiment and comparative example, prepare samples, take 5 samples of each material for testing, and observe the morphology of the samples after 168 hours.
[0112] Table 1 Example / Comparative Example Tensile strength / MPa Elongation at break / % Tear strength / (kN / m) Thermal conductivity: W / (m*K) Oxygen index / % Microstructure of pore structure Sample morphology after 168h hot air accelerated aging Example 1 2.5 580 42 0.02 36 Closed cell structure No wrinkles, no cracks, no pinholes, no deformation Example 2 2.8 620 45 0.018 36 Closed cell structure No wrinkles, no cracks, no pinholes, no deformation Example 3 2.6 586 43 0.019 36 Closed cell structure No wrinkles, no cracks, no pinholes, no deformation Example 4 2.2 450 36 0.023 35 Closed cell structure No wrinkles, no cracks, no pinholes, no deformation Example 5 2.3 465 37 0.022 35 Closed cell structure No wrinkles, no cracks, no pinholes, no deformation Example 6 2 413 33 0.023 35 Closed cell structure No wrinkles, no cracks, no pinholes, no deformation Example 7 3.2 690 61 0.013 38 Closed cell structure No wrinkles, no cracks, no pinholes, no deformation Example 8 3.5 750 65 0.012 38 Closed cell structure No wrinkles, no cracks, no pinholes, no deformation Example 9 3.3 710 62 0.013 38 Closed cell structure No wrinkles, no cracks, no pinholes, no deformation Example 10 2.83 626 47 0.021 38 Closed cell structure No wrinkles, no cracks, no pinholes, no deformation Embodiment 11 2.85 631 48 0.022 38 Closed cell structure No wrinkles, no cracks, no pinholes, no deformation Comparative Example 1 0.7 210 23 0.032 33 Contains partially open and perforated structures Wrinkles, cracks, pinholes and deformation Comparative Example 2 1.4 276 30 0.026 36 Contains a small amount of open pore structure Slight pinholes Comparative Example 3 1.21 260 28 0.028 36 Contains a small amount of open pore structure Slight pinholes Comparative Example 4 1.45 280 30 0.025 36 Contains a small amount of open pore structure Slight pinholes Comparative Example 5 1.13 256 27 0.029 36 Contains a small amount of open and perforated structures Wrinkles, pinholes and deformation Comparative Example 6 1.2 261 28 0.028 36 Contains a small amount of open and perforated structures Wrinkles, pinholes and deformation Comparative Example 7 1.15 258 27 0.029 36 Contains a small amount of open and perforated structures Wrinkles, pinholes and deformation Comparative Example 8 1.25 263 28 0 36 Contains a small amount of open and perforated structures Wrinkled, deformed Comparative Example 9 1.1 251 26 0.029 35 Contains a small amount of open and perforated structures Wrinkles, pinholes and deformation Comparative Example 10 1.3 270 29 0.027 36 Contains micro-opening structure Slightly deformed Comparative Example 11 1.5 285 31 0.025 33 Contains micro-opening structure Slightly deformed It can be seen from Example 2 and Comparative Example 1 and Table 1 that the thermal insulation foam rubber material prepared in the present application has excellent thermal insulation performance and mechanical strength.
[0113] It can be seen from Example 2, Comparative Examples 2 to 11 and Table 1 that the foam rubber material prepared by compounding the modifier, EPDM masterbatch and chloroprene rubber masterbatch in this application, and blending CR with EPDM, not only has the characteristics of heat insulation and aging resistance, but also has greatly improved flame retardant properties. The addition of the modifier can effectively improve the pore structure and improve the thermal insulation and mechanical strength properties of the material. And it can be seen from the data that the effect is optimal only when the above raw materials are compounded. In particular, when the modifier is prepared by the method of this application, the modifier has the highest degree of improvement on the thermal insulation and mechanical strength properties of the material.
[0114] Combining Example 2 and Example 4 with Table 1, it can be seen that the addition of hollow glass microspheres can effectively improve the mixing effect of the raw materials in the EPDM rubber masterbatch, and can also improve the thermal insulation performance and mechanical strength of the thermal insulation foam rubber material.
[0115] It can be seen from Example 2 and Example 5 and Table 1 that the addition of calcium carbonate has a good reinforcing effect on the chloroprene rubber masterbatch, and the chloroprene rubber masterbatch can contribute excellent mechanical strength to the thermal insulation foam rubber material.
[0116] It can be seen from Example 2 and Example 8 and Table 1 that by adding slag wool and polytetrafluoroethylene fine particle resin to the compound, the slag wool contains a large number of micropores and macropores, the fibers are interwoven to form a dense porous grid, and the polytetrafluoroethylene fine particle resin is entangled between the slag wool fibers, which can not only synergistically improve the mechanical strength of the thermal insulation foam rubber material, but also effectively reduce the damage of the slender ends of the fibers to the internal pores of the thermal insulation foam rubber material, thereby effectively exerting the thermal insulation effect of the slag wool.
[0117] It can be seen from Example 2, Example 8, Example 10, Example 11 and Table 1 that the performance of the thermal insulation foam rubber material is best improved only when slag wool and polytetrafluoroethylene fine particle resin are compounded and used.
[0118] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A thermal insulation foam rubber material for air ducts of air conditioners, characterized in that: The invention comprises the following raw materials in parts by weight: 70 parts of EPDM rubber masterbatch; 30 parts of chloroprene rubber masterbatch; Antiaging agent 4010-NA 0.5-2 parts; 3-7 parts of zinc oxide; Accelerator DM 1 to 1.5 parts; Accelerator Na-22 0.5-1.5 parts; Accelerator TMTD 3-5 parts; 1-2 parts of sulfur; Foaming agent AC 7-11 parts; Modifier 6-10 parts; The modifier includes polyvinyl alcohol, hydroxy polypropylene microspheres and graphene aerogel, the polyvinyl alcohol is loaded inside the hydroxy polypropylene microspheres, the graphene aerogel is loaded outside the hydroxy polypropylene microspheres, and the weight ratio of the polyvinyl alcohol, the hydroxy polypropylene microspheres and the graphene aerogel is 5:8:
1.
2. The heat-insulating foam rubber material for air-conditioning ducts according to claim 1, characterized in that: The EPDM rubber masterbatch comprises the following raw materials: EPDM rubber, carbon black, zinc oxide, stearic acid, and hollow glass microspheres, and the weight ratio of the EPDM rubber, carbon black, zinc oxide, stearic acid, and hollow glass microspheres is 100:20:5:3:
2.
3. The heat insulating foam rubber material for air ducts of an air conditioner according to claim 2, characterized in that: The preparation method of the EPDM rubber masterbatch is as follows: taking each raw material in order according to the usage, plasticizing the EPDM rubber at 100-120° C. for 4-6 minutes, then adding zinc oxide, stearic acid, carbon black and hollow glass microbeads in order, maintaining the temperature and continuing to mix for 4-6 minutes to obtain the EPDM rubber masterbatch.
4. The heat insulating foam rubber material for air ducts of an air conditioner according to claim 1, characterized in that: The chloroprene rubber masterbatch comprises the following raw materials: chloroprene rubber, magnesium oxide, stearic acid and calcium carbonate, and the weight ratio of the chloroprene rubber, magnesium oxide, stearic acid and calcium carbonate is 100:4:3:
1.
5. The heat insulating foam rubber material for air ducts of an air conditioner according to claim 4, characterized in that: The preparation method of the chloroprene rubber masterbatch is as follows: taking each raw material in order according to the amount, plasticizing the chloroprene rubber at 60-90° C. for 4-6 minutes, then adding magnesium oxide, stearic acid and calcium carbonate in order while maintaining the temperature, and continuing to mix for 4-6 minutes to obtain the chloroprene rubber masterbatch.
6. The heat insulating foam rubber material for air ducts of an air conditioner according to claim 1, characterized in that: The preparation method of the modifier is: Dissolving polyvinyl alcohol in water to form a polyvinyl alcohol solution, dissolving hydroxy polypropylene microspheres in dichloromethane to form a hydroxy polypropylene microsphere solution, and dropping the polyvinyl alcohol solution into the hydroxy polypropylene microsphere solution, stirring to make it evenly dispersed; The mixed solution is added to the aqueous phase containing gelatin to form a stable emulsion, and the organic solvent is gradually evaporated by stirring and heating to embed the polyvinyl alcohol inside the hydroxy polypropylene microspheres, and the hydroxy polypropylene microspheres loaded with polyvinyl alcohol are prepared by washing and drying. The graphene aerogel powder is evenly dispersed in water to form a suspension, a silane coupling agent is added to the suspension, and the mixture is stirred until uniform. Then, hydroxyl polypropylene microspheres loaded with polyvinyl alcohol are added to the suspension, and the mixture is stirred sufficiently to make the surface of the microspheres evenly covered with graphene aerogel. The mixture is reacted for 24 hours, and the microspheres loaded with graphene aerogel are separated by centrifugation and dried to obtain a modifier.
7. The heat insulating foam rubber material for air ducts of an air conditioner according to claim 1, characterized in that: The heat insulating foam rubber material also includes slag wool and polytetrafluoroethylene fine particle resin. The weight portion of the slag wool is 3 to 5 parts, and the weight portion of the polytetrafluoroethylene fine particle resin is 4 to 6 parts.
8. The method for preparing the heat insulating foam rubber material for air ducts of air conditioners according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Prepare modifier, EPDM rubber masterbatch and chloroprene rubber masterbatch respectively, weigh each raw material according to the amount used and set aside; (2) Mix EPDM rubber masterbatch, chloroprene rubber masterbatch, antioxidant 4010-NA and modifier at 60-90° C. for 4-6 minutes to prepare a rubber mixture; (3) Add zinc oxide, accelerator DM, accelerator Na-22 and accelerator TMTD to the mixed rubber in sequence and mix evenly, then add sulfur and foaming agent AC in sequence, mix evenly, form sheets, and let stand at room temperature for 24 hours; (4) The mixed rubber is subjected to compression vulcanization foaming with the following process parameters: temperature 180-220°C, pressure 6-8 MPa, time 3-5 min, to obtain a heat insulating foam rubber material.
9. The method for preparing the heat insulating foam rubber material for air duct of air conditioner according to claim 7, characterized in that: The following steps are involved: (1) Prepare the modifier, EPDM rubber masterbatch and chloroprene rubber masterbatch respectively, weigh each raw material according to the amount used and set aside; (2) Mix EPDM rubber masterbatch, chloroprene rubber masterbatch, antioxidant 4010-NA, modifier, slag wool and polytetrafluoroethylene fine particle resin at 60-90° C. for 4-6 minutes to prepare a mixed rubber; (3) Add zinc oxide, accelerator DM, accelerator Na-22 and accelerator TMTD to the mixed rubber in sequence and mix evenly, then add sulfur and foaming agent AC in sequence, mix evenly, form sheets, and let stand at room temperature for 24 hours; (4) The mixed rubber is subjected to compression vulcanization foaming with the following process parameters: temperature 180-220°C, pressure 6-8 MPa, time 3-5 min, to obtain a heat insulating foam rubber material.
Citation Information
Patent Citations
Method for preparing core-shell structure glycosylated polypropylene and its use
CN101070401A
Coating explosive microspheres prepared through emulsion solidification and preparation method thereof
CN106083495A