High-damping heat-resistant rubber material and preparation method thereof

By adding modified filler and petroleum hydrogenation resin to butyl rubber, high-damping heat-resistant rubber materials are prepared, which solves the problem of improving damping performance at high temperatures and achieves high damping and heat-resistant performance in high temperature environments , suitable for high temperature application scenarios.

CN119039713APending Publication Date: 2024-11-29NINGGUO ZOYE PLASTIC & RUBBER CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411252783.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art cannot meet the high damping requirements at high temperatures, especially the damping performance of butyl rubber is limited in high temperature conditions and cannot be suitable for high temperature application scenarios.

Method used

The components such as brominated butyl rubber, petroleum hydrogenation resin, modified filler, stearic acid, indirect zinc oxide, internal mold release agent MH-610, S-80, K-805 were prepared through refining and vulcanization. High damping heat-resistant rubber material is produced. The modified filler is treated with synthetic mica powder and carbon black through calcium bicarbonate solution to enhance dispersion and compatibility, and improve the mechanical and thermal stability of the rubber.

Benefits of technology

Maintaining high damping performance at high temperatures provides good heat resistance and shock absorption performance. It is suitable for products such as engine base, automobile shock absorbers and elevator shock absorbers in high temperature environments. The damping coefficient is stable at more than 1.2, and the material is After high temperature treatment, there is no bubble peeling and bubbling phenomenon, and the heat resistance is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005032946950000061
    Figure BDA0005032946950000061
  • Figure BDA0005032946950000071
    Figure BDA0005032946950000071
Patent Text Reader

Abstract

The invention discloses a high-damping heat-resistant rubber material and a preparation method thereof.The preparation method comprises the following steps that 1, brominated butyl rubber, petroleum hydrogenated resin, modified filler, stearic acid, aliphatic resin, indirect method zinc oxide and internal release agents MH-610, S-80 and K-805 are sequentially fed into an internal mixer to be internally mixed, and synthetic rubber is obtained; 2, performing open milling on the synthetic rubber, and performing vulcanization treatment to obtain the high-damping heat-resistant rubber material, the high-damping heat-resistant rubber material prepared according to the formula and the preparation method can stabilize the damping at 1.2 or above at a high temperature, has good heat resistance and shock absorption performance, and is especially suitable for the fields of engine seats, automobile shock absorbers, elevator shock absorption piece products and the like with high requirements on buffer performance and high working temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rubber materials, relates to the technical field of damping rubber materials, and specifically relates to a high-damping heat-resistant rubber material and a manufacturing method thereof. Background Art

[0002] Butyl rubber is a linear gel-free copolymer with good shock absorption performance, low temperature flexural resistance, ozone resistance and heat resistance. It is particularly suitable for engine seats, automobile shock absorbers and elevator shock absorbers with high buffering performance requirements. With the progress and development of society, the requirements for shock absorption and noise reduction of the natural rubber shock-absorbing seals that were originally widely used are becoming higher and higher, and butyl rubber with high damping requirements and good heat resistance has emerged.

[0003] Patent CN109320861A discloses a wide temperature range high damping halogenated butyl rubber material and a preparation method thereof. By adding a damping agent terpene resin and / or its modified products to the halogenated butyl rubber, the glass transition temperature difference is increased, so that the damping peak value is shifted to the right, the damping performance of the rubber at room temperature and high temperature is improved, and the effective damping temperature range of the rubber is further broadened. However, this solution is based on the influence of metal adhesion and the effective damping temperature range, and the damping of butyl rubber is not greatly improved, and it cannot meet the application scenarios with high damping requirements.

[0004] Patent CN105906956A discloses a high-damping chlorobutyl damping rubber and a preparation method thereof. By modifying the chlorobutyl rubber with octyl triazone masterbatch, a chlorobutyl rubber material with excellent damping and mechanical properties and a wide damping temperature range is obtained; however, the maximum damping temperature range is -60-40°C, which cannot meet the high damping requirements under high temperatures. Summary of the invention

[0005] The purpose of the present invention is to solve the problem of a rubber material that can maintain high damping performance at high temperatures, and to provide a high-damping heat-resistant rubber material and a manufacturing method thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for manufacturing a high-damping heat-resistant rubber material comprises the following steps:

[0008] Step 1, bromobutyl rubber, petroleum hydrogenated resin, modified filler, stearic acid, aliphatic resin, indirect zinc oxide, internal release agents MH-610, S-80, K-805 are sequentially sent to a banbury mixer for 8-10 minutes each time at a banbury temperature of 50-60°C to obtain synthetic rubber;

[0009] Step 2: The synthetic rubber is subjected to vulcanization treatment after being refined to obtain a high damping heat-resistant rubber material.

[0010] Further, the modified filler is prepared by the following steps:

[0011] Add synthetic mica powder and carbon black to a sufficient amount of calcium bicarbonate solution, stir to disperse the synthetic mica powder and carbon black in the calcium bicarbonate solution, add 0.1 mol / L dilute hydrochloric acid until the solution pH is 6.5-6.9, continue stirring for 1-2 hours, filter, wash with anhydrous ethanol, dry, and crush to obtain a modified filler.

[0012] Furthermore, the mass ratio of synthetic mica powder to carbon black is 14-18:10-12.

[0013] Furthermore, the specific steps of step 2 are: the synthetic rubber is preformed by an open mill at 75-80°C, and then the preformed rubber is placed in a mold in a vulcanization equipment at a pressure of 160-170Kgf / cm 2 , the rubber is vulcanized at a temperature of 170-175°C for 390-480 seconds to obtain a high damping heat-resistant rubber material.

[0014] A high damping heat-resistant rubber material contains the following components by mass percentage: 42-46% brominated butyl rubber, 4.2-4.7% indirect zinc oxide, 6.5-7% petroleum hydrogenated resin, 1.5-2% internal mold release agent MH-610, 12-16% aliphatic resin, 24-30% modified filler, 1% stearic acid, 0.15-0.25% S-80, and 1-1.5% K-805.

[0015] Furthermore, the aliphatic resin is a C5 aliphatic resin.

[0016] Beneficial effects of the present invention:

[0017] (1) The high damping heat-resistant rubber material prepared according to the formula and preparation method of the present invention can maintain a stable damping of more than 1.2 at high temperature, has good heat resistance and shock absorption performance, and is particularly suitable for engine seats, automobile shock absorbers, and elevator shock absorption parts with high buffering performance requirements and high operating temperatures.

[0018] (2) The present invention uses synthetic mica powder and carbon black as fillers. The synthetic mica has high surface finish, high whiteness and high purity, and does not contain heavy metals that are harmful to the human body. The present invention increases the dispersibility and compatibility of the synthetic mica powder and carbon black in the brominated butyl rubber by grafting calcium ions on the surface of the synthetic mica powder and carbon black. At the same time, the calcium ions can also synthesize calcium stearate with stearic acid, further increasing the dispersibility of the filler in the rubber, enhancing the mechanical properties and thermal stability of the rubber, and improving the heat resistance of the rubber. During the shock absorption process, the force of the rubber moves along the vertical direction of the vibration and noise propagation, rubbing against the surrounding emulsion polymer chains, synthetic mica powder and other fillers, and quickly converting mechanical energy into heat energy to achieve a high damping effect.

[0019] (3) The present invention forms a coating between the high damping heat-resistant rubber material and the mold by adding petroleum hydrogenated resin to the rubber, thereby preventing adhesion and facilitating demolding. The petroleum hydrogenated resin can form a large number of hydrogen bonds with the rubber to hinder the movement of the polymer chain segments, increase the friction resistance, and enhance the damping performance; and has little effect on the damping temperature range, effectively improving the damping performance of the high damping heat-resistant rubber material at high temperatures, so that the high damping rubber material prepared by the present invention has good heat resistance. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Embodiment 1: A method for preparing a high damping heat-resistant rubber material, comprising the following steps:

[0022] Step 1: Add 14 kg of synthetic mica powder and 10 kg of carbon black to a sufficient amount of calcium bicarbonate solution, stir to disperse the synthetic mica powder and carbon black in the calcium bicarbonate solution, add 0.1 mol / L of dilute hydrochloric acid until the solution pH is 6.5, continue stirring for 1 hour, filter, wash with anhydrous ethanol, dry, and crush to obtain a modified filler.

[0023] Step 2: 42kg of brominated butyl rubber, 6.5kg of petroleum hydrogenated resin, 27.2kg of modified filler, 1kg of stearic acid, 16kg of aliphatic resin, 4.3kg of indirect zinc oxide, 1.5kg of internal release agent MH-610, 0.2kg of S-80 and 1.3kg of K-805 are sequentially sent into a banburying mixer for 8 minutes each time at a banburying temperature of 50°C to obtain a synthetic rubber.

[0024] Step 3: Preform the synthetic rubber by mixing it in an open mill at 75°C, and then put the preformed rubber into the mold in the vulcanization equipment at a pressure of 160Kgf / cm 2 The rubber is vulcanized at a temperature of 170°C for 480 seconds to obtain a high damping heat-resistant rubber material.

[0025] Embodiment 2: A method for preparing a high damping heat-resistant rubber material, comprising the following steps:

[0026] Step 1: Add 16 kg of synthetic mica powder and 11 kg of carbon black to a sufficient amount of calcium bicarbonate solution, stir to disperse the synthetic mica powder and carbon black in the calcium bicarbonate solution, add 0.1 mol / L of dilute hydrochloric acid until the pH of the solution is 6.7, continue stirring for 1.5 hours, filter, wash with anhydrous ethanol, dry, and crush to obtain a modified filler.

[0027] Step 2: 46 kg of brominated butyl rubber, 6.5 kg of petroleum hydrogenated resin, 26 kg of modified filler, 1 kg of stearic acid, 13 kg of aliphatic resin, 4.4 kg of indirect zinc oxide, 1.5 kg of internal release agent MH-610, 0.2 kg of S-80 and 1.4 kg of K-805 are sequentially sent into a banbury mixer for 9 minutes each time at a banbury temperature of 55°C to obtain a synthetic rubber.

[0028] Step 3: Preform the synthetic rubber by mixing it in an open mill at 80°C, and then put the preformed rubber into the mold in the vulcanization equipment at a pressure of 170Kgf / cm 2 The rubber is vulcanized at a temperature of 170°C for 420 seconds to obtain a high damping heat-resistant rubber material.

[0029] Embodiment 3: A method for preparing a high damping heat-resistant rubber material, comprising the following steps:

[0030] Step 1: Add 18 kg of synthetic mica powder and 12 kg of carbon black to a sufficient amount of calcium bicarbonate solution, stir to disperse the synthetic mica powder and carbon black in the calcium bicarbonate solution, add 0.1 mol / L of dilute hydrochloric acid until the pH of the solution is 6.9, continue stirring for 2 hours, filter, wash with anhydrous ethanol, dry, and crush to obtain a modified filler.

[0031] Step 2: 42kg of brominated butyl rubber, 6.5kg of petroleum hydrogenated resin, 30kg of modified filler, 1kg of stearic acid, 13kg of aliphatic resin, 4.4kg of indirect zinc oxide, 1.5kg of internal release agent MH-610, 0.2kg of S-80 and 1.4kg of K-805 are sequentially sent into a banburying mixer for 10min each time at a banburying temperature of 60°C to obtain a synthetic rubber.

[0032] Step 3: Preform the synthetic rubber by mixing it in an open mill at 80°C, and then put the preformed rubber into the mold in the vulcanization equipment at a pressure of 170Kgf / cm 2 The rubber is vulcanized at a temperature of 175°C for 390 seconds to obtain a high damping heat-resistant rubber material.

[0033] The surface of synthetic mica powder can have active sites, which can react with calcium ions in calcium bicarbonate solution to graft calcium ions onto the surface of synthetic mica powder; the surface of carbon black also has acidic sites, which can react with calcium bicarbonate to graft calcium ions onto the surface of carbon black, and under the regulation of dilute hydrochloric acid, the negative charge density on the surface of synthetic mica powder and carbon black is relatively high, which can produce a strong electrostatic attraction with positively charged calcium ions, which not only helps to promote the grafting reaction of calcium ions on the surface of synthetic mica powder and carbon black, but also helps the surface of synthetic mica powder and carbon black to adsorb calcium ions.

[0034] Synthetic mica powder has good stability and can improve the thermal stability of rubber, so that the rubber material maintains a high damping coefficient at different temperatures. However, the surface polarity of synthetic mica powder is large and it is easy to agglomerate in rubber. The surface polarity of the modified filler composed of modified synthetic mica powder and carbon black is more compatible with brominated butyl rubber, and the interaction force between synthetic mica powder and carbon black and brominated butyl rubber is increased, making it easier for synthetic mica powder and carbon black to disperse in brominated butyl rubber. The increase in this interaction force reduces the aggregation of mica powder and carbon black in rubber, which not only improves the thermal stability of rubber materials, but also enhances the mechanical properties of rubber materials. At the same time, stearic acid is added. Stearic acid can react with calcium ions to form calcium stearate. Calcium stearate has the effect of a dispersant and stabilizer on brominated butyl rubber, further helping the mica powder and carbon black grafted with surface calcium ions and the reinforcing agent petroleum hydrogenated resin to be dispersed in brominated butyl rubber, thereby enhancing the thermal stability and mechanical properties of rubber materials.

[0035] Comparative Example 1: The difference from Example 1 is that the modified filler is replaced by equal masses of carbon black and mica powder.

[0036] Comparative Example 2: The difference from Example 1 is that the mass percentage of the modified filler is 10%.

[0037] Comparative Example 3: The difference from Example 1 is that the mass percentage of the modified filler is 40%.

[0038] The sources of some reagents in the embodiments and comparative examples are as follows:

[0039] Bromobutyl rubber was purchased from Shanghai Ren'en Import and Export Trading Co., Ltd.

[0040] Indirect zinc oxide was purchased from Haishun New Materials Co., Ltd.

[0041] Synthetic mica powder was purchased from Guangdong Yufeng Powder Material Co., Ltd.

[0042] The aliphatic resin is C5 aliphatic resin purchased from Shanghai Wandao Chemical Co., Ltd.

[0043] Petroleum hydrogenated resin, brand Exxon, was purchased from Qingdao Oubeli Technology Co., Ltd.

[0044] The high damping heat-resistant rubber materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to performance tests. The tensile stress-strain properties of the high damping heat-resistant rubber materials were tested according to GB / T 528-2009 standard. The damping properties of the high damping heat-resistant rubber materials were tested using a DMA-242 dynamic mechanical analyzer produced by NETZSCH, Germany. The samples were cut into the same size and thickness and then subjected to a high temperature resistance test. After the samples were attached, the steel plates were placed in an environment of 180° C. for 30 minutes, and the shedding and bubbling of the samples were observed. The results are shown in Table 1:

[0045] Table 1

[0046]

[0047]

[0048] It can be seen from Table 1 that the damping coefficients of Examples 1 to 3 prepared in the present invention are above 1.2, and have high damping performance. In addition, no bubbling phenomenon occurs on the surface after high-temperature treatment, and the high-temperature resistance is strong.

[0049] Since Comparative Example 1 is not modified with calcium bicarbonate, it is unevenly dispersed in the high-damping heat-resistant rubber material, and the improvement in the heat resistance of the rubber material is low. Therefore, it falls off after high-temperature treatment and has poor heat resistance; since Comparative Example 2 has a small content of modified filler, the improvement in the heat resistance of the high-damping heat-resistant rubber is small, so bubbling occurs after high-temperature treatment; since Comparative Example 3 has an excessively high content of modified filler and is unevenly dispersed, fillers in some high-damping heat-resistant rubbers are agglomerated, so bubbles occur in the agglomerated part of the fillers after high-temperature treatment and the heat resistance is poor.

[0050] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0051] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for producing a high damping heat-resistant rubber material, characterized in that: The steps include: Step 1, bromobutyl rubber, petroleum hydrogenated resin, modified filler, stearic acid, aliphatic resin, indirect zinc oxide, internal release agents MH-610, S-80, K-805 are sequentially sent to a banbury mixer for 8-10 minutes each time at a banbury temperature of 50-60°C to obtain synthetic rubber; Step 2: The synthetic rubber is subjected to vulcanization treatment after being refined to obtain a high damping heat-resistant rubber material.

2. The method for manufacturing a high damping heat-resistant rubber material according to claim 1, characterized in that: The modified filler is prepared by the following steps: Add synthetic mica powder and carbon black to a sufficient amount of calcium bicarbonate solution, stir to disperse the synthetic mica powder and carbon black in the calcium bicarbonate solution, add 0.1 mol / L dilute hydrochloric acid until the solution pH is 6.5-6.9, continue stirring for 1-2 hours, filter, wash with anhydrous ethanol, dry, and crush to obtain a modified filler.

3. The method for manufacturing a high damping heat-resistant rubber material according to claim 2, characterized in that: The mass ratio of the synthetic mica powder to carbon black is 14-18:10-12.

4. The method for manufacturing a high damping heat-resistant rubber material according to claim 1, characterized in that: The specific steps of step 2 are: the synthetic rubber is preformed by an open mill at 75-80°C, and then the preformed rubber is placed in a mold in a vulcanization equipment at a pressure of 160-170Kgf / cm 2 , the rubber is vulcanized at a temperature of 170-175°C for 390-480 seconds to obtain a high damping heat-resistant rubber material.

5. A high damping heat-resistant rubber material, characterized in that: The composition comprises the following components by mass percentage: 42-46% brominated butyl rubber, 4.2-4.7% indirect zinc oxide, 6.5-7% petroleum hydrogenated resin, 1.5-2% internal mold release agent MH-610, 12-16% aliphatic resin, 24-30% modified filler, 1% stearic acid, 0.15-0.25% S-80 and 1-1.5% K-805.

6. A high damping heat-resistant rubber material according to claim 5, characterized in that: The aliphatic resin is a C5 aliphatic resin.

Citation Information

Patent Citations

  • High-damping chlorinated butyl rubber and method for preparing same

    CN105906956A

  • Wide-temperature-range and high-damping halogenated butyl rubber material and preparation method thereof

    CN109320861A