Anti-fogdrop surfactant for film and preparation method of anti-fogdrop surfactant
By using specific proportion mixing and microencapsulation technology of modified surfactants and other components in film anti-fog agents, the problem of insufficient anti-fog performance of film anti-fog agents in low and high temperature environments is solved, and the waterproof and washing performance is improved and stability, extends service life and achieves long-lasting antioxidant properties.
Patent Information
- Application Number
- CN202411169731.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-25
- Publication Date
- 2024-11-29
AI Technical Summary
It is difficult for existing film anti-fog agents to maintain excellent anti-fog performance in low and high temperature environments, and their stability and durability are insufficient, so they cannot improve anti-oxidation performance and purity without affecting the anti-fog effect.
Modified surfactants, tetraalkoxysilanes, silane coupling agents, propellants, antibacterial agents, ultraviolet absorbers and microencapsulated antioxidants are mixed in a specific proportion, and antioxidants are encapsulated through microencapsulation technology and combined with Nanofiltration technology is used to filtration and purification to prepare film-specific anti-fog agents with more comprehensive anti-fog performance and better durability.
Maintain the best anti-fog effect at different temperatures, improve waterproof and wash performance, extend service life, enhance the stability and durability of anti-fog agents, prevent oxidation and degradation, and achieve long-term anti-oxidation performance.
Smart Images

Figure BDA0005008904950000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of antifogging agent preparation, in particular to an antifogging surfactant for a film and a preparation method thereof. Background Art
[0002] Anti-fog agents are mainly used to prevent the surface of transparent materials from fogging due to condensation of water vapor or other gases. Thin-film anti-fog agents are specifically used to prevent condensation on the surface of plastic films. Existing thin-film anti-fog agents are difficult to have excellent anti-fog properties at both low and high temperatures.
[0003] The defects of the existing anti-droplet surfactant preparation are:
[0004] 1. Patent document CN116144198B discloses a special antifogging agent for transparent polyolefin film, which mainly considers how to produce an antifogging agent with a long-lasting antifogging effect and good reinforcement and toughening effect, but does not consider how to prepare an antifogging agent with a comprehensive antifogging effect and good durability;
[0005] 2. Patent document CN110724494B discloses a long-lasting low-temperature resistant antifogging agent and its preparation method and use. It mainly considers how to prepare an antifogging agent with stronger hydrophilicity, low-temperature resistance and high light transmittance, but does not consider how to improve the long-term antioxidant performance of the antifogging agent without affecting the normal performance of the antifogging agent;
[0006] 3. Patent document CN109021759B discloses an antifogging agent and a preparation method thereof, which mainly considers how to make the antifogging agent more hydrophilic and have a better antifogging effect, but does not consider how to enhance the stability and durability of the antifogging agent and have a comprehensive antifogging effect;
[0007] 4. Patent document CN111363425B discloses an anti-fogging agent, a preparation method and its application. It mainly considers how to improve the anti-fogging effect of the anti-fogging agent on glass while avoiding the influence of the anti-fogging agent on the light transmittance of the glass. It does not consider how to improve the purity and stability of the atomizing agent. Summary of the invention
[0008] The object of the present invention is to provide an anti-fogging surfactant for a film and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0009] To achieve the above object, the present invention provides the following technical solution: an anti-fog droplet surfactant for film, characterized in that: the raw materials thereof include the following components by weight: 20-25 parts of modified surfactant, 3-7 parts of tetraalkoxysilane, 1-2 parts of silane coupling agent, 0.1-2 parts of propellant, 1-3 parts of antibacterial agent, 2-5 parts of ultraviolet absorber, 2 parts of antistatic agent and 2-4 parts of microencapsulated antioxidant;
[0010] The modified surfactant, tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber, antistatic agent and microencapsulated antioxidant are mixed in proportion to prepare a special antifog agent for thin films. Compared with traditional antifog agents, the prepared special antifog agent for thin films has more comprehensive antifog performance and better durability.
[0011] Preferably, the modified surfactant is prepared by compounding glycerol monooleate, sorbitan monooleate and ethanol in a mass ratio of (1-3):2:2.
[0012] Preferably, the propellant is one of dimethyl ether, compressed carbon dioxide and compressed nitrogen.
[0013] Preferably, the antibacterial agent is one or more of alkyl monophenol, alkyl polyphenol and thiopolyphenol.
[0014] Preferably, the preparation method of the anti-fog droplet surfactant for the film is as follows:
[0015] Step S1: preparing microencapsulated antioxidants: using microencapsulation technology to encapsulate antioxidants in microparticles to prepare microencapsulated antioxidants for use;
[0016] Step S2: preparing a modified surfactant: compounding a modified surfactant with glycerol monooleate, sorbitan monooleate and ethanol in a mass ratio of (1-3):2:(3-5);
[0017] Step S3: Mixing raw materials: adding the modified surfactant obtained in step S2, tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber and antistatic agent into a reaction kettle in proportion for mixing reaction to obtain a mixed solution A;
[0018] Step S4: post-treatment process: filtering and purifying the mixed solution A prepared in step S3, and stabilizing it with the microencapsulated antioxidant prepared in step S1;
[0019] Step S5: Performance test: Performing a performance test on the film-specific antifogging agent obtained in step S4;
[0020] Step S6: Packaging and storage: Packaging the qualified anti-fogging agent for thin films, and storing the packaged anti-fogging agent for thin films in a dry, cool and well-ventilated environment.
[0021] Preferably, the step S1 further includes the following steps:
[0022] Step S11: dissolving an antioxidant in ethanol to obtain an antioxidant solution, wherein the mass ratio of the antioxidant to the ethanol is 1:1;
[0023] Step S12: dissolving gelatin in hot water at 70° C. to form a wall material solution, wherein the mass ratio of gelatin to hot water is 2:1;
[0024] Step S13: adding the antioxidant solution obtained in step S11 and the wall material solution prepared in step S12 to a high shear emulsifier at a mass ratio of 1:1.5 for emulsification, stirring for 20-30 minutes at a stirring speed of 35-40 rpm to form tiny antioxidant droplets;
[0025] Step S14: placing the antioxidant beads and the cross-linking agent in step S13 in a reaction kettle at a mass ratio of 1:0.3, stirring for 25 minutes at a stirring speed of 30 rpm to solidify the wall material and form a stable microcapsule structure;
[0026] Step S15: The microcapsules solidified in step S14 are then filtered and centrifuged to obtain microencapsulated antioxidants.
[0027] Preferably, the step S2 further includes the following steps:
[0028] Step S21: adding glycerol monooleate and sorbitan monooleate to ethanol respectively, and stirring with a stirrer until completely dissolved to form a glycerol monooleate solution and a sorbitan monooleate solution, wherein the stirring speed of the stirrer is 20 rpm, and the mass ratios of glycerol monooleate to ethanol and sorbitan monooleate to ethanol are both 1:1;
[0029] Step S22: slowly pouring the glycerol monooleate solution obtained in step S21 into the sorbitan monooleate solution, and rapidly stirring with a stirrer to fully mix the two to form a mixed solution, wherein the stirring speed of the stirrer is 40-50 rpm, and the mass ratio of the glycerol monooleate solution to the sorbitan monooleate solution is (1-3):2;
[0030] Step S23: then placing the mixed solution in step S22 in a constant temperature water bath at 40° C. and stirring at a speed of 30-40 rpm for 1.5 h;
[0031] Step S24: The mixed solution is then taken out from the water bath, left to cool to room temperature, and then unreacted impurities are filtered out with filter paper to obtain a pure modified surfactant.
[0032] Preferably, the step S3 further includes the following steps:
[0033] Step S31: adding deionized water into the reaction kettle for preheating to 50° C.;
[0034] Step S32: then adding the modified surfactant into the reaction kettle and stirring at a speed of 35 rpm for 15 min;
[0035] Step S33: The mixed solution in step S32 is then cooled to 30°C, and tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber and antistatic agent are added to the reactor in sequence, and stirred at 35 rpm for 45 minutes under a constant temperature environment to obtain a mixed solution A.
[0036] Preferably, the step S4 further includes the following steps:
[0037] Step S41: filtration and purification: using nanofiltration technology to filter the prepared mixed solution A to remove unreacted raw materials and by-products;
[0038] Step S42: Stabilization treatment: add microencapsulated antioxidant to the mixed solution A, and stir at a speed of 30-35 rpm for 30-40 min to allow the microencapsulated antioxidant to be fully mixed in the mixed solution A to obtain a special anti-fogging agent for thin films.
[0039] Preferably, the step S5 further includes the following steps:
[0040] Step S51: Anti-fog performance test: Take a 1*1m film and evenly spray the film surface with a special anti-fog agent for the film, let it stand for 1 day, and then test it in the environment of -20℃, -10℃ and 0℃ according to the water bath hot fog method in GB / T31726-2015 "Test method for anti-fog property of plastic film". Test it in the environment of 20℃, 30℃, 50℃ and 70℃ according to the cold fog method in GB / T31726-2015 "Test method for anti-fog property of plastic film". Comprehensively evaluate it according to the anti-fog grade comparison table in GB / T31726-2015 "Test method for anti-fog property of plastic film" to obtain the anti-fog grade;
[0041] Step S52: Durability test: Take a 1*1m film, spray the film-specific anti-fog agent evenly on the film surface, let it stand for one day, and on the second day, perform an anti-fog performance test on the film according to the rapid hot fog method in GB / T31726-2015 "Test Method for Anti-fog Performance of Plastic Film". Then, on the eighth day and the thirty-first day, perform the anti-fog performance test again using the same method, and make a comprehensive durability evaluation based on the obtained anti-fog grade.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] 1. The special anti-fog agent for thin films prepared according to the ratio of the present invention can maintain the best anti-fog droplet effect under different temperature conditions, and at the same time improve the water-proof and washable performance of the anti-fog agent, so that the film still has a good anti-fog effect even after rainy days, and the anti-fog effect of the anti-fog agent will not be reduced due to rain erosion.
[0044] 2. The present invention can prevent the anti-fogging agent from aging and degradation through the antioxidant, which can effectively extend the service life of the anti-fogging agent, help to improve the stability of the storage performance of the prepared film-specific anti-fogging agent, and at the same time prevent the film from oxidative degradation during use, thereby extending the service life of the film. The antioxidant is encapsulated in microparticles using microencapsulation technology, which can achieve slow release of the antioxidant without affecting the normal performance of the anti-fogging agent, thereby improving the long-term effectiveness of the antioxidant performance.
[0045] 3. The present invention has good initial anti-fog properties and low-temperature anti-fog properties through glycerol monooleate, and sorbitan monooleate belongs to sorbitan fatty acid esters, which has a long-lasting anti-fog effect, a short-term quick effect and a high-temperature anti-fog effect. The two are compounded to produce a synergistic effect between the two surfactants, enhance the stability and durability of the anti-fog agent, so that the anti-fog agent can not only provide good anti-fog properties at low temperatures, but also maintain its effectiveness in high temperature environments, and has a more comprehensive anti-fog effect.
[0046] 4. The present invention utilizes nanofiltration technology to filter the mixed solution, simplifies the operation steps of filtration and purification, improves the purity and stability of the product, can effectively remove the unreacted raw materials and by-products in the reaction, and then performs stabilization treatment to improve the stability of the antifogging agent, and avoid the antifogging agent being too sensitive to air and affecting the normal antifogging performance of the antifogging agent. DETAILED DESCRIPTION
[0047] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] The present invention provides an anti-fogging surfactant for a film and a preparation method thereof. The preparation method of the anti-fogging surfactant for a film is as follows:
[0049] Step S1: preparing microencapsulated antioxidant: dissolving an antioxidant in ethanol to obtain an antioxidant solution, wherein the mass ratio of the antioxidant to the ethanol is 1:1, then dissolving gelatin in hot water at 70°C to form a wall material solution, wherein the mass ratio of gelatin to the hot water is 2:1, then adding the obtained antioxidant solution and the prepared wall material solution to a high shear emulsifier at a mass ratio of 1:1.5 for emulsification, stirring for 20-30 minutes at a stirring speed of 35-40rpm to form tiny antioxidant droplets, then placing the antioxidant droplets and the cross-linking agent in a reaction kettle at a mass ratio of 1:0.3, stirring for 25 minutes at a stirring speed of 30rpm to solidify the wall material and form a stable microcapsule structure, then filtering and centrifuging the solidified microcapsules to obtain microencapsulated antioxidant;
[0050] Step S2: preparing a modified surfactant: adding glycerol monooleate and sorbitan monooleate to ethanol respectively, and stirring with a stirrer until completely dissolved to form a glycerol monooleate solution and a sorbitan monooleate solution, wherein the stirring speed of the stirrer is 20 rpm, and the mass ratios of glycerol monooleate to ethanol and sorbitan monooleate to ethanol are both 1:1, then slowly pouring the obtained glycerol monooleate solution into the sorbitan monooleate solution, and stirring rapidly with a stirrer at the same time, so that the two are fully mixed to form a mixed solution, wherein the stirring speed of the stirrer is 40-50 rpm, and then placing the mixed solution in a constant temperature water bath at 40°C and stirring at a speed of 30-40 rpm for 1.5 hours, then taking out the mixed solution from the water bath, standing and cooling to room temperature, and then filtering out unreacted impurities with filter paper to obtain a pure modified surfactant, wherein the mass ratio of glycerol monooleate solution to sorbitan monooleate solution is (1-3):2;
[0051] Step S3: Mixing raw materials: first add deionized water into a reactor for preheating treatment, heating to a temperature of 50°C, then add a modified surfactant into the reactor, stir for 15 minutes at a speed of 35rpm, then cool the mixed solution to 30°C, and then add tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber and antistatic agent into the reactor in sequence, and continue to stir at a speed of 35rpm for 45 minutes under a constant temperature environment to obtain a mixed solution A, wherein the mass ratio of the modified surfactant, tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber and antistatic agent is (20-25): (3-7): (1-2): (0.1-2): (1-3): (2-5): 2;
[0052] Step S4: post-treatment process: the prepared mixed solution A is filtered by nanofiltration technology to remove unreacted raw materials and by-products, and then the microencapsulated antioxidant is added to the mixed solution A, and stirred at a speed of 30-35 rpm for 30-40 minutes to make the microencapsulated antioxidant fully mixed in the mixed solution A to obtain a special antifogging agent for thin films;
[0053] Step S5: Performance test: Take a 1*1m film and spray the film-specific anti-fog agent evenly on the film surface, let it stand for 1 day, and then test it at -20℃, -10℃ and 0℃ respectively according to the water bath hot fog method in GB / T31726-2015 "Test method for anti-fog of plastic film". Test it at 20℃, 30℃, 50℃ and 70℃ respectively according to the cold fog method in GB / T31726-2015 "Test method for anti-fog of plastic film". Comprehensively evaluate the anti-fog grade comparison table in the 2015 "Test Method for Anti-fog Property of Plastic Film" to obtain the anti-fog grade. In addition, take a 1*1m film and evenly spray the film surface with a special anti-fog agent for the film. Let it stand for one day. On the second day, the film is tested for anti-fog performance according to the rapid hot fog method in GB / T31726-2015 "Test Method for Anti-fog Property of Plastic Film". Then, on the eighth day and the thirty-first day, the anti-fog performance test is carried out again in the same way, and a comprehensive durability evaluation is obtained based on the obtained anti-fog grade.
[0054] Step S6: Packaging and storage: Packaging the qualified anti-fogging agent for thin films, and storing the packaged anti-fogging agent for thin films in a dry, cool and well-ventilated environment.
[0055] Furthermore, the antioxidant in the antifogging agent can prevent the antifogging agent from aging and degradation, can effectively extend the service life of the antifogging agent, and help to improve the stability of the storage performance of the prepared antifogging agent for thin films. At the same time, it can prevent the film from oxidative degradation during use, thereby extending the service life of the film. The use of microencapsulation technology to encapsulate the antioxidant in microparticles can achieve slow release of the antioxidant without affecting the normal performance of the antifogging agent, improve the long-term antioxidant performance, and further extend the antifogging effect of the film. Gelatin enables the natural polymer to have good encapsulation performance as a wall material to collect oil;
[0056] Glycerol monooleate belongs to the glycerol fatty acid ester surfactant, and has good initial anti-fogging properties and low-temperature anti-fogging properties, while sorbitan monooleate belongs to the sorbitan fatty acid ester, and has a long-lasting anti-fogging effect, a short-term quick-acting property, and a high-temperature anti-fogging effect. The two are compounded to produce a synergistic effect between the two surfactants, enhance the stability and durability of the anti-fogging agent, and make the subsequently prepared anti-fogging agent combine the advantages of the two, so that the anti-fogging agent can not only provide good anti-fogging properties at low temperatures, but also maintain its effectiveness in high temperature environments, and has a more comprehensive anti-fogging effect;
[0057] The film-specific anti-fog agent prepared according to this ratio can maintain the best anti-fog droplet effect under different temperature conditions, and at the same time improves the water-proof and washable performance of the anti-fog agent, so that the film still has a good anti-fog effect even after rainy days, and the anti-fog effect of the anti-fog agent will not be reduced due to rain erosion. The tetraalkoxysilane therein is an organic silicon compound, which can form a hydrophilic siloxane film on the surface of the plastic film. This hydrophilic layer can automatically absorb water vapor, reduce the contact angle between water molecules and the surface of the substrate, and make the water vapor wet and diffuse on the surface of the substrate to form an ultra-thin transparent water film to avoid the formation of water droplets. At the same time, in order to improve the bonding between the anti-fog agent and the film In addition to the strength, silane coupling agents need to be added. These coupling agents can form chemical bonds between silane and the film to enhance the durability and water wash resistance of the coating. Propellants can help spray out the active ingredients and evenly distribute them on the treated surface, which helps to evenly distribute the anti-fogging agent on the film surface when using the anti-fogging agent. In addition, ultraviolet absorbers can absorb ultraviolet rays to prevent plastics from aging due to ultraviolet radiation, improve weather resistance, and thus extend the service life of the film. Antistatic agents reduce the accumulation of static electricity on the film, improve the electrical properties of the plastic film surface, and avoid affecting transparency due to static dust absorption. Antibacterial agents help inhibit the growth of bacteria in the anti-fogging agent and help extend the storage time of the anti-fogging agent.
[0058] The mixed solution is filtered by nanofiltration technology, which simplifies the operation steps of filtration and purification, improves the purity and stability of the product, and after the preparation is completed, the performance of the prepared film-specific antifogging agent is tested, and finally the film-specific antifogging agent with qualified performance is packaged;
[0059] The value in step S2-3 is changed, and steps S1 and S4-6 are performed to test the anti-fogging effect of the prepared anti-fogging agent for thin film under different environments, and to test its durability and water-proof performance.
[0060] Embodiment 1:
[0061] Step S2: preparing a modified surfactant: adding glycerol monooleate and sorbitan monooleate to ethanol respectively, and stirring with a stirrer until completely dissolved to form a glycerol monooleate solution and a sorbitan monooleate solution, wherein the stirring speed of the stirrer is 20 rpm, and the mass ratios of glycerol monooleate to ethanol and sorbitan monooleate to ethanol are both 1:1, then slowly pouring the obtained glycerol monooleate solution into the sorbitan monooleate solution, and stirring rapidly with a stirrer at the same time, so that the two are fully mixed to form a mixed solution, wherein the stirring speed of the stirrer is 45 rpm, and then placing the mixed solution in a constant temperature water bath at 40°C and stirring at a speed of 30 rpm for 1.5 hours, then taking out the mixed solution from the water bath, standing and cooling to room temperature, and then filtering out unreacted impurities with filter paper to obtain a pure modified surfactant, wherein the mass ratio of glycerol monooleate solution to sorbitan monooleate solution is 1:2;
[0062] Step S3: Mixing raw materials: first add deionized water into the reactor for preheating treatment, heat to a temperature of 50°C, then add the modified surfactant into the reactor, stir at a speed of 35rpm for 15min, then cool the mixed solution to 30°C, and then add tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber and antistatic agent into the reactor in sequence, and continue to stir at a speed of 35rpm for 45min under a constant temperature environment to obtain a mixed solution A, wherein the mass ratio of the modified surfactant, tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber and antistatic agent is 23:4:1:0.5:1.5:2:2.
[0063] Furthermore, the anti-fog level at -20°C is: 4, the anti-fog level at -10°C is: 3, the anti-fog level at 0°C is: 2, the anti-fog level at 20°C is: 1, the anti-fog level at 30°C is: 1, the anti-fog level at 50°C is: 2, the anti-fog level at 70°C is: 3, the anti-fog level on the second day is 1, the anti-fog level on the eighth day is 2, the anti-fog level on the thirty-first day is 3, and the durability evaluation is: good.
[0064] Embodiment 2:
[0065] Step S2: preparing a modified surfactant: adding glycerol monooleate and sorbitan monooleate to ethanol respectively, and stirring with a stirrer until completely dissolved to form a glycerol monooleate solution and a sorbitan monooleate solution, wherein the stirring speed of the stirrer is 20 rpm, and the mass ratios of glycerol monooleate to ethanol and sorbitan monooleate to ethanol are both 1:1, then slowly pouring the obtained glycerol monooleate solution into the sorbitan monooleate solution, and stirring rapidly with a stirrer at the same time, so that the two are fully mixed to form a mixed solution, wherein the stirring speed of the stirrer is 45 rpm, and then placing the mixed solution in a constant temperature water bath at 40°C and stirring at a speed of 30 rpm for 1.5 hours, then taking out the mixed solution from the water bath, standing and cooling to room temperature, and then filtering out unreacted impurities with filter paper to obtain a pure modified surfactant, wherein the mass ratio of glycerol monooleate solution to sorbitan monooleate solution is 2:2;
[0066] Step S3: Mixing raw materials: first add deionized water into the reactor for preheating treatment, heat to a temperature of 50°C, then add the modified surfactant into the reactor, stir at a speed of 35rpm for 15min, then cool the mixed solution to 30°C, and then add tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber and antistatic agent into the reactor in sequence, and continue to stir at a speed of 35rpm for 45min under a constant temperature environment to obtain a mixed solution A, wherein the mass ratio of the modified surfactant, tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber and antistatic agent is 23:5:1:0.5:1.5:3:2.
[0067] Furthermore, the anti-fog level at -20°C is 3, the anti-fog level at -10°C is 2, the anti-fog level at 0°C is 2, the anti-fog level at 20°C is 1, the anti-fog level at 30°C is 1, the anti-fog level at 50°C is 2, the anti-fog level at 70°C is 3, the anti-fog level on the second day is 1, the anti-fog level on the eighth day is 1, the anti-fog level on the thirty-first day is 3, and the durability evaluation is good.
[0068] Embodiment three:
[0069] Step S2: preparing a modified surfactant: adding glycerol monooleate and sorbitan monooleate to ethanol respectively, and stirring with a stirrer until completely dissolved to form a glycerol monooleate solution and a sorbitan monooleate solution, wherein the stirring speed of the stirrer is 20 rpm, and the mass ratios of glycerol monooleate to ethanol and sorbitan monooleate to ethanol are both 1:1, then slowly pouring the obtained glycerol monooleate solution into the sorbitan monooleate solution, and stirring rapidly with a stirrer at the same time, so that the two are fully mixed to form a mixed solution, wherein the stirring speed of the stirrer is 45 rpm, and then placing the mixed solution in a constant temperature water bath at 40°C and stirring at a speed of 30 rpm for 1.5 hours, then taking out the mixed solution from the water bath, standing and cooling to room temperature, and then filtering out unreacted impurities with filter paper to obtain a pure modified surfactant, wherein the mass ratio of glycerol monooleate solution to sorbitan monooleate solution is 2:2;
[0070] Step S3: Mixing raw materials: first add deionized water into the reactor for preheating treatment, heat to a temperature of 50°C, then add the modified surfactant into the reactor, stir at a speed of 35rpm for 15min, then cool the mixed solution to 30°C, and then add tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber and antistatic agent into the reactor in sequence, and continue to stir at a speed of 35rpm for 45min under a constant temperature environment to obtain a mixed solution A, wherein the mass ratio of the modified surfactant, tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber and antistatic agent is 23:7:1:0.5:1.5:3:2.
[0071] Furthermore, the anti-fog level at -20°C is: 3, the anti-fog level at -10°C is: 2, the anti-fog level at 0°C is: 2, the anti-fog level at 20°C is: 1, the anti-fog level at 30°C is: 1, the anti-fog level at 50°C is: 2, the anti-fog level at 70°C is: 3, the anti-fog level on the second day is 1, the anti-fog level on the eighth day is 1, the anti-fog level on the thirty-first day is 2, and the durability evaluation is: good.
[0072] Comparative Example:
[0073] Take the anti-fog agent sold on the market as a comparative example, where the anti-fog level at -20°C is: 5, the anti-fog level at -10°C is: 4, the anti-fog level at 0°C is: 4, the anti-fog level at 20°C is: 2, the anti-fog level at 30°C is: 2, the anti-fog level at 50°C is: 4, the anti-fog level at 70°C is: 5, the anti-fog level on the second day is 2, the anti-fog level on the eighth day is 3, and the anti-fog level on the thirty-first day is 5. Durability evaluation:
[0074] generally.
[0075] The test results of anti-fog performance and durability of the film-specific anti-fog agent are as follows:
[0076]
[0077] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
Claims
1. An anti-fogging surfactant for a film, characterized in that: The raw materials include the following components by weight: 20-25 parts of modified surfactant, 3-7 parts of tetraalkoxysilane, 1-2 parts of silane coupling agent, 0.1-2 parts of propellant, 1-3 parts of antibacterial agent, 2-5 parts of ultraviolet absorber, 2 parts of antistatic agent and 2-4 parts of microencapsulated antioxidant; The modified surfactant, tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber, antistatic agent and microencapsulated antioxidant are mixed in proportion to prepare a special antifog agent for thin films. Compared with traditional antifog agents, the prepared special antifog agent for thin films has more comprehensive antifog performance and better durability.
2. The anti-fogging surfactant for film according to claim 1, characterized in that: The modified surfactant is prepared by compounding glycerol monooleate, sorbitan monooleate and ethanol in a mass ratio of (1-3):2:
2.
3. The anti-fogging surfactant for film according to claim 1, characterized in that: The propellant is one of dimethyl ether, compressed carbon dioxide and compressed nitrogen.
4. The anti-fogging surfactant for film according to claim 1, characterized in that: The antibacterial agent is one or more of alkyl monophenol, alkyl polyphenol and thiopolyphenol.
5. A method for preparing an anti-fogging surfactant for a film, applicable to the anti-fogging surfactant for a film according to any one of claims 1 to 4, characterized in that: The preparation method of the anti-fogging surfactant for the film is as follows: Step S1: preparing microencapsulated antioxidants: using microencapsulation technology to encapsulate antioxidants in microparticles to prepare microencapsulated antioxidants for use; Step S2: preparing a modified surfactant: compounding a modified surfactant with glycerol monooleate, sorbitan monooleate and ethanol in a mass ratio of (1-3):2:(3-5); Step S3: Mixing raw materials: adding the modified surfactant obtained in step S2, tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber and antistatic agent into a reaction kettle in proportion for mixing reaction to obtain a mixed solution A; Step S4: post-treatment process: filtering and purifying the mixed solution A prepared in step S3, and stabilizing it with the microencapsulated antioxidant prepared in step S1; Step S5: Performance test: Performing a performance test on the film-specific antifogging agent obtained in step S4; Step S6: Packaging and storage: Packaging the qualified anti-fogging agent for thin films, and storing the packaged anti-fogging agent for thin films in a dry, cool and well-ventilated environment.
6. The method for preparing an anti-fogging surfactant for a film according to claim 5, characterized in that: The step S1 further includes the following steps: Step S11: dissolving an antioxidant in ethanol to obtain an antioxidant solution, wherein the mass ratio of the antioxidant to the ethanol is 1:1; Step S12: dissolving gelatin in hot water at 70° C. to form a wall material solution, wherein the mass ratio of gelatin to hot water is 2:1; Step S13: adding the antioxidant solution obtained in step S11 and the wall material solution prepared in step S12 to a high shear emulsifier at a mass ratio of 1:1.5 for emulsification, stirring for 20-30 minutes at a stirring speed of 35-40 rpm to form tiny antioxidant droplets; Step S14: placing the antioxidant beads and the cross-linking agent in step S13 in a reaction kettle at a mass ratio of 1:0.3, stirring for 25 minutes at a stirring speed of 30 rpm to solidify the wall material and form a stable microcapsule structure; Step S15: The microcapsules solidified in step S14 are then filtered and centrifuged to obtain microencapsulated antioxidants.
7. The method for preparing an anti-fogging surfactant for a film according to claim 5, characterized in that: The step S2 further includes the following steps: Step S21: adding glycerol monooleate and sorbitan monooleate to ethanol respectively, and stirring with a stirrer until completely dissolved to form a glycerol monooleate solution and a sorbitan monooleate solution, wherein the stirring speed of the stirrer is 20 rpm, and the mass ratios of glycerol monooleate to ethanol and sorbitan monooleate to ethanol are both 1:1; Step S22: slowly pouring the glycerol monooleate solution obtained in step S21 into the sorbitan monooleate solution, and rapidly stirring with a stirrer to fully mix the two to form a mixed solution, wherein the stirring speed of the stirrer is 40-50 rpm, and the mass ratio of the glycerol monooleate solution to the sorbitan monooleate solution is (1-3):2; Step S23: then placing the mixed solution in step S22 in a constant temperature water bath at 40° C. and stirring at a speed of 30-40 rpm for 1.5 h; Step S24: The mixed solution is then taken out from the water bath, left to cool to room temperature, and then unreacted impurities are filtered out with filter paper to obtain a pure modified surfactant.
8. The method for preparing an anti-fogging surfactant for a film according to claim 5, characterized in that: The step S3 further includes the following steps: Step S31: adding deionized water into the reaction kettle for preheating to 50° C.; Step S32: then adding the modified surfactant into the reaction kettle and stirring at a speed of 35 rpm for 15 min; Step S33: The mixed solution in step S32 is then cooled to 30°C, and tetraalkoxysilane, silane coupling agent, propellant, antibacterial agent, ultraviolet absorber and antistatic agent are added to the reactor in sequence, and stirred at 35 rpm for 45 minutes under a constant temperature environment to obtain a mixed solution A.
9. The method for preparing an anti-fogging surfactant for a film according to claim 5, characterized in that: The step S4 further includes the following steps: Step S41: filtration and purification: using nanofiltration technology to filter the prepared mixed solution A to remove unreacted raw materials and by-products; Step S42: Stabilization treatment: add microencapsulated antioxidant to the mixed solution A, and stir at a speed of 30-35 rpm for 30-40 min to allow the microencapsulated antioxidant to be fully mixed in the mixed solution A to obtain a special anti-fogging agent for thin films.
10. The method for preparing an anti-fogging surfactant for a film according to claim 5, characterized in that: The step S5 further includes the following steps: Step S51: Anti-fog performance test: Take a 1*1m film and evenly spray the film surface with a special anti-fog agent for the film, let it stand for 1 day, and then test it in the environment of -20℃, -10℃ and 0℃ according to the water bath hot fog method in GB / T31726-2015 "Test method for anti-fog property of plastic film". Test it in the environment of 20℃, 30℃, 50℃ and 70℃ according to the cold fog method in GB / T31726-2015 "Test method for anti-fog property of plastic film". Comprehensively evaluate it according to the anti-fog grade comparison table in GB / T31726-2015 "Test method for anti-fog property of plastic film" to obtain the anti-fog grade; Step S52: Durability test: Take a 1*1m film, spray the film-specific anti-fog agent evenly on the film surface, let it stand for one day, and on the second day, perform an anti-fog performance test on the film according to the rapid hot fog method in GB / T31726-2015 "Test Method for Anti-fog Performance of Plastic Film". Then, on the eighth day and the thirty-first day, perform the anti-fog performance test again using the same method, and make a comprehensive durability evaluation based on the obtained anti-fog grade.