Bearing surface heat treatment device and method

Through the bearing surface heat treatment device and method, electromagnetic impact, carburizing and tempering processes are used to solve the failure problem of tapered roller bearings in harsh environments, improve its wear resistance and fatigue life, extend the service life and reduce the service life Heat treatment costs.

CN119040608APending Publication Date: 2024-11-29刘娇娇
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411245175.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Tapered roller bearings are prone to failure due to fatigue, fracture, wear and so on in harsh marine environments, and it is necessary to improve its wear resistance and fatigue life to extend its service life.

Method used

The bearing surface heat treatment device and method are adopted, including vacuum air atmosphere furnace, water bath furnace, electromagnetic impact device and coating device. Through electromagnetic impact, carburizing, bainite quenching and tempering, stress and structural structure are regulated and bearing rings are added. hardness and toughness reduce holes and crack rates.

Benefits of technology

It effectively improves the wear resistance and impact toughness of the bearing ring, extends the service life, reduces the cost and energy consumption of heat treatment, and enhances the tensile strength and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040608A_ABST
    Figure CN119040608A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of bearing heat treatment, in particular to a bearing surface heat treatment device and method.The bearing surface heat treatment device comprises a plurality of bearing rings, a heating device, an electromagnetic device, a coating device and a controller, the heating device comprises a vacuum atmosphere furnace, a water bath furnace and a tempering furnace, and the electromagnetic device comprises an electromagnetic impact device and a vacuum magnetic field heating furnace; the vacuum atmosphere furnace, the water bath furnace, the tempering furnace, the electromagnetic impact device and the vacuum magnetic field heating furnace are all in communication connection with the controller, and the coating device comprises a flame spraying gun and induction remelting equipment. The method has the beneficial effects that the austenite phase transformation temperature is relatively low, the process time and energy consumption are reduced, the martensite pre-quenching process is introduced between austenitizing and bainite isothermal quenching and tempering, dislocation is generated in supercooled austenite around martensite by generating part of pre-quenched martensite, the effect of promoting bainite transformation can be achieved, and the yield of the bainite is improved. And the heat treatment efficiency is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of bearing heat treatment, and in particular to a bearing surface heat treatment device and method. Background Art

[0002] The ocean is a vast and diverse landscape that plays a vital role in the global economy, and one of the environmental challenges is the ever-present risk of corrosion, which can affect even the smallest mechanical components, such as bearings.

[0003] Tapered roller bearings in the bearing classification can carry large radial loads and axial loads at the same time, and can ensure efficient and smooth output of the cutter ring power. The inner and outer rings of tapered roller bearings are the main load-bearing components of the bearings. They are prone to early failure when serving in harsh marine environments and need to withstand frequent and large impact loads and marine corrosion for a long time. Therefore, fatigue, fracture and wear are the main failure forms of most tapered roller bearings. It is necessary to improve the wear resistance and fatigue life of the tapered roller bearing rings, thereby improving the bearing performance and extending the service life of the equipment. Summary of the invention

[0004] In order to improve the wear resistance and fatigue life of tapered roller bearing rings and enhance the performance of the bearings, the present invention provides a bearing surface heat treatment device and method.

[0005] The present invention provides a bearing surface heat treatment device and method using the following technical solutions: A bearing surface heat treatment device and method, including several bearing rings, a heating device, an electromagnetic device, a coating device and a controller, the heating device includes a vacuum atmosphere furnace, a water bath furnace and a tempering furnace, the electromagnetic device includes an electromagnetic impact device and a vacuum magnetic field heating furnace, and the vacuum atmosphere furnace, water bath furnace, tempering furnace, electromagnetic impact device and vacuum magnetic field heating furnace are all communicatively connected to the controller.

[0006] By adopting the above technical solution, the heating device, the electromagnetic device, and the coating device are controlled by a controller, and the control data during the heat treatment process is recorded.

[0007] Preferably, the electromagnetic impact device includes a thermal imager, a power supply, a converter, a primary induction coil and a secondary induction coil, an iron core is arranged between the primary induction coil and the secondary induction coil, copper electrodes are fixedly connected to both ends of the secondary induction coil, an oscilloscope is electrically connected to the secondary induction coil, the converter is electrically connected to the primary induction coil, and one of the bearing rings is clamped between the two copper electrodes.

[0008] By adopting the above technical solution, the magnitude of participating stresses is regulated by electromagnetic impact, the stress relief annealing process of the bearing after cold rolling is omitted, and excessive power consumption is reduced, which is beneficial to reducing the cost of heat treatment of the bearing ring, and reducing the time and energy consumption of heat treatment of the bearing ring.

[0009] Preferably, the vacuum magnetic field heating furnace comprises an outer shell, an inner shell and a thermocouple, the outer surface of the inner shell is fixedly connected to a magnet, the interior of the inner shell is fixedly connected to an insulating layer, the inner surface of the insulating layer is fixedly connected to a resistance wire, the interior of the insulating layer is fixedly connected to a crucible, the probe of the thermocouple is overlapped on the outer surface of the crucible, and one of the bearing rings is placed inside the crucible.

[0010] By adopting the above technical solution, the martensite is induced to expand by a strong magnetic field, thereby generating compressive stress on the surrounding austenite structure, inhibiting the initiation and expansion of cracks in the bearing ring, which is beneficial to improving the wear resistance of the bearing ring.

[0011] Preferably, the coating device comprises a flame spraying gun and an induction remelting device, and the flame spraying gun and the induction remelting device are both communicatively connected to the controller.

[0012] By adopting the above technical solution, the flame spraying gun is controlled by the controller to have a pre-spray coating thickness of 1 mm.

[0013] A bearing surface heat treatment method includes the following specific operation steps: step S1, cold rolling to form a bearing ring, and the bearing ring is subjected to composite treatment; step S2, the bearing ring 5 is carburized and austenitized in a vacuum atmosphere furnace; step S3, the bearing ring 5 is bainite quenched in a vacuum atmosphere furnace; step S4, the bearing ring 5 is cooled in a water bath furnace; step S5, the bearing ring 5 is tempered in a tempering furnace.

[0014] Preferably, in step S1, the specific operation steps of the composite treatment of the bearing ring include operating the controller to adjust the current size and the number of impacts, the electromagnetic impact device generates electromagnetic impulses to continuously impact the bearing ring, the primary uses an industrial frequency power supply, and the primary current range is 0~300A.

[0015] By adopting the above technical solution, electromagnetic punching is used to generate thermal effect and atomic migration in a short time to repair the holes and cracks caused by cold rolling and reduce the porosity of the bearing ring.

[0016] Preferably, in step S1, the specific operating steps of the composite treatment of the bearing ring include operating a flame spray gun to pre-spray the outer surface of the bearing ring, the thickness of the pre-spray coating of the bearing ring is 1 mm, and the pre-spray coating of the bearing ring is induction remelted, the remelting temperature is not lower than 1000°C, the time is not less than 25s, and the pre-spray coating material is made of high-hardness nickel-chromium-borosilicate alloy powder.

[0017] By adopting the above technical solution, the impact resistance and hardness of the bearing ring are improved through coating, and the toughness and corrosion resistance of the coating are improved through high-hardness nickel-chromium-boron-silicon alloy powder, so that the bearing has a longer service life in harsh marine environments.

[0018] Preferably, in step S2, the specific operation steps of carburizing include: step S21, the bearing ring after step S1 is placed in a vacuum atmosphere furnace for carburizing heating and austenitizing, the bearing ring is heated to 900°C and then carburized, after heating to 945°C, the bearing ring enters the strong carburizing and diffusion stage, the heating time of the strong carburizing and diffusion stage is 8h40min and 4h20min respectively, and the environmental carbon content of the strong carburizing and diffusion stage is 1.20% and 1.00% respectively; step S22, the austenitizing includes, the bearing ring after step S21 is heated to 840°C in a vacuum atmosphere furnace for 20min.

[0019] By adopting the above technical solution, by increasing the carburizing temperature, shortening the carburizing time, and reducing the concentration of ambient carbon, a higher surface carbon content is obtained, so that during subsequent heating of the bearing ring, the content of martensite and ferrite on the surface is increased and the content of non-martensite is reduced, thereby improving the hardness and toughness of the surface of the bearing ring.

[0020] Preferably, in step S3, the specific operating steps of the bainite quenching include: step S31, heating the bearing ring after step S2 to 200°C in a vacuum atmosphere furnace for 5 minutes; step S32, heating the bearing ring after step S31 to 240°C in a vacuum atmosphere furnace for 20 minutes; in step S4, the specific operating steps of cooling the bearing ring through a water bath furnace include: placing the bearing ring after step S3 in a water bath furnace, immersing it in an aqueous quenching medium and cooling it to 70°C.

[0021] By adopting the above technical solution, a martensite pre-quenching process is introduced between austenitization and bainite isothermal quenching and tempering. By generating part of the pre-quenched martensite, dislocations are generated in the supercooled austenite around the martensite, which can promote the transformation of bainite and thus improve the heat treatment efficiency. The aqueous quenching medium does not need to clean the bearing ring, which reduces the consumption of water resources and is beneficial to energy saving and green environmental protection.

[0022] Preferably, high temperature tempering is performed, and the bearing ring after step S3 is placed in a crucible of a vacuum magnetic field heating furnace and heated to 530° C. for 2 hours.

[0023] By adopting the above technical solution, high temperature tempering combined with a strong magnetic field can promote the precipitation of carbides, reduce the recovery of dislocation, induce mutation of martensite, and cause the adjacent austenite to move and dislocate, thereby increasing the dislocation density of the martensite, strengthening the dislocation effect, improving the hardness and tensile strength of the bearing ring, and extending the service life of the bearing ring.

[0024] Preferably, low temperature tempering is performed, and the bearing ring after step S3 is placed in a tempering furnace and heated to 160° C. for 2 hours.

[0025] By adopting the above technical solution, under the action of heat and force in the friction process, when the residual austenite in the bearing ring is gradually transformed into martensite, the hardness of the bearing ring is improved, and the plastic deformation and the degree of pear peeling on the surface of the bearing ring are reduced. At the same time, the formed martensite generates compressive stress on the surrounding tissues through volume expansion, inhibiting the initiation and expansion of cracks in the bearing ring, which is beneficial to improving the wear resistance of the bearing ring.

[0026] In summary, the present invention has the following beneficial technical effects: 1. In the present invention, the austenite phase transition temperature is relatively low, which reduces the process time and energy consumption. A martensite pre-quenching process is introduced between austenitization and bainite isothermal quenching and tempering. By generating part of the pre-quenched martensite, dislocations are generated in the supercooled austenite around the martensite, which can promote the transformation of bainite and thus improve the heat treatment efficiency. At the same time, the generated pre-quenched martensite and the final quenched martensite can divide the original austenite grains for many times and refine the structure, thereby improving the impact toughness and wear resistance of the tapered roller bearing ring and improving the bearing performance. 2. In the present invention, a flame spray gun is operated to pre-spray the outer surface of the bearing ring, the thickness of the pre-spray coating of the bearing ring is 1 mm, and the pre-spray coating of the bearing ring is induction remelted, thereby improving the impact performance and hardness of the bearing ring, and at the same time, the toughness of the coating is improved by high-hardness nickel-chromium-boron-silicon alloy powder, thereby improving the toughness of the bearing, improving the wear resistance of the tapered roller bearing ring, and improving the bearing performance; 3. In the present invention, electromagnetic shock is used to generate heat effect and atomic migration in a short time, repair holes and cracks caused by cold rolling, and reduce the porosity of the bearing ring. Electromagnetic shock can also directly regulate the size and analysis of participating stresses, thereby eliminating the stress relief annealing process after cold rolling, reducing excessive power consumption, and helping to reduce the cost of heat treatment of the bearing ring, and reducing the time and energy consumption of heat treatment of the bearing ring; 4. In the present invention, high temperature tempering is combined with a strong magnetic field to promote the precipitation of carbides, reduce the recovery of dislocation, induce mutation of martensite, and make adjacent austenite move and dislocate, so that the dislocation density of the residual austenite is increased, the dislocation effect is strengthened, the hardness and tensile strength of the bearing ring are increased, and the service life of the bearing ring is extended; 5. In the present invention, during low-temperature tempering, the residual austenite in the bearing ring gradually transforms into martensite under the action of heat and force in the friction process, thereby improving the hardness of the bearing ring and reducing the plastic deformation and pear peeling degree of the bearing ring surface. At the same time, the formed martensite generates compressive stress on the surrounding tissues through volume expansion, inhibiting the initiation and expansion of cracks in the bearing ring, which is beneficial to improving the wear resistance of the bearing ring. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a structural schematic diagram of a vacuum magnetic field heating furnace in a bearing surface heat treatment device of the present invention; Figure 2 It is a structural principle diagram of an electromagnetic impact device in a bearing surface heat treatment device of the present invention; Figure 3 It is a process route map of electromagnetic control in a bearing surface heat treatment method of the present invention; Figure 4 The present invention is a process flow chart of a bearing surface heat treatment method.

[0028] Description of reference numerals: 1. Converter; 2. Primary induction coil; 3. Secondary induction coil; 4. Oscilloscope; 5. Bearing ring; 6. Magnet; 7. Insulation layer; 8. Resistance wire; 9. Crucible. DETAILED DESCRIPTION

[0029] The following is combined with Figure 1-Figure 4 The present invention is described in further detail.

[0030] The embodiments of the present invention disclose a bearing surface heat treatment device and method.

[0031] Embodiment 1 discloses a bearing surface heat treatment device.

[0032] Reference Figure 1 , Figure 2 , including several bearing rings 5, a heating device, an electromagnetic device, a coating device and a controller. The heating device includes a vacuum atmosphere furnace, a water bath furnace and a tempering furnace. The electromagnetic device includes an electromagnetic impact device and a vacuum magnetic field heating furnace. The vacuum atmosphere furnace, the water bath furnace, the tempering furnace, the electromagnetic impact device and the vacuum magnetic field heating furnace are all connected to the controller for communication.

[0033] Reference Figure 2 , Figure 3The electromagnetic impact device includes a thermal imager, a power supply, a converter 1, a primary induction coil 2 and a secondary induction coil 3. A Fotric226 non-contact thermal imager is used to monitor the temperature in real time. An iron core is arranged between the primary induction coil 2 and the secondary induction coil 3. Copper electrodes are fixedly connected to both ends of the secondary induction coil 3. An oscilloscope 4 is electrically connected to the secondary induction coil 3. The oscilloscope 4 is used to obtain a waveform diagram of the current size changing with time. The converter 1 is electrically connected to the primary induction coil 2. One of the bearing rings 5 ​​is clamped between the two copper electrodes. The bearing ring 5 is placed between the upper and lower copper electrodes. The current size and the number of impacts are adjusted by a controller.

[0034] Reference Figure 1 , Figure 3 The vacuum magnetic field heating furnace includes an outer shell, an inner shell and a thermocouple. A heat treatment heating furnace is fixed between the inner shell and the outer shell. The vacuum magnetic field heating furnace adopts a 12T superconducting strong magnet, so that the bearing ring 5 is heated as a whole and the insulation process is carried out under the condition of a 12T steady magnetic field and vacuum. The outer surface of the inner shell is fixedly connected with a magnet 6, the inner shell is fixedly connected with an insulating layer 7, the inner surface of the insulating layer 7 is fixedly connected with a resistance wire 8, the inner surface of the insulating layer 7 is fixedly connected with a crucible 9, and the probe of the thermocouple is overlapped with the outer surface of the crucible 9. During the heating process, the thermocouple feeds back the temperature in the crucible 9 in real time, which is convenient for the staff to operate the controller for real-time adjustment. One of the bearing rings 5 ​​is placed inside the crucible 9.

[0035] Reference Figure 4 The coating device includes a flame spraying gun and an induction remelting device, and both the flame spraying gun and the induction remelting device are communicatively connected to the controller.

[0036] The implementation principle of Example 1 is: 1. When the surface of the cold-rolled bearing ring 5 is more damaged, an electromagnetic impact device can be used to continuously impact the cold-rolled bearing ring 5 with electromagnetic impact, and then the bearing ring 5 is placed in a vacuum atmosphere furnace, carbon is released at 905°C, the temperature is raised to 945°C and the temperature is kept isothermal for 13 hours, and then the temperature is kept isothermal at 840°C for 20 minutes, and then the bearing ring is cooled to below the Ms value, and pre-quenched and kept at 200°C for 5 minutes, and then the temperature is raised to 240°C and the temperature is kept isothermal for 20 minutes, and then the bearing ring 5 is placed in a water bath furnace, and the water quenching medium is used to cool the bearing ring 5 to 70°C, and finally the bearing ring 5 is placed in the crucible 9 of the vacuum magnetic field heating furnace, and the temperature is kept isothermal at 530°C for 2 hours; 2. When the surface of the cold-rolled bearing ring 5 is relatively flat, use a flame spray gun to spray a 1mm coating on the surface of the cold-rolled bearing ring 5. After induction remelting, put the bearing ring 5 into a vacuum atmosphere furnace, start carbon release at 905°C, raise the temperature to 945°C and keep isothermal for 13 hours, continue to keep isothermal at 840°C for 20 minutes, cool to below the Ms value, pre-quench and keep warm at 200°C for 5 minutes, then raise the temperature to 240°C and keep isothermal for 20 minutes, then place the bearing ring 5 in a water bath furnace, use an aqueous quenching medium to cool it down to 70°C, and finally place the bearing ring 5 in a tempering furnace and keep isothermal at 160°C for 2 hours.

[0037] Embodiment 2 discloses a method for heat treatment of a bearing surface.

[0038] Reference Figure 3 , Figure 4 , including the following specific operation steps: step S1, cold rolling to form the bearing ring 5, the bearing ring 5 is formed by near-net cold rolling ring forming, which can avoid high-temperature heating of the ring blank of the bearing ring 5, thereby avoiding the problems of coarse grains, oxidation decarburization and large size changes of the bearing ring 5 during the high temperature process, and the bearing ring 5 undergoes composite treatment; step S2, the bearing ring 5 is carburized and austenitized in a vacuum atmosphere furnace; step S3, the bearing ring 5 is bainite quenched in a vacuum atmosphere furnace, after austenitization isothermal, it is first pre-quenched below the martensite start transformation temperature, after obtaining a certain pre-quenched martensite, the temperature is raised to the bainite transformation temperature range for isothermal, the lower bainite generated when close to the martensite transformation temperature has a thin lens-like morphology, has good impact toughness and wear resistance, and can improve the toughness and wear resistance of the bearing ring matrix structure; step S4, the bearing ring 5 is cooled in a water bath furnace; step S5, the bearing ring 5 is tempered in a tempering furnace.

[0039] Reference Figure 3In step S1, the specific operation steps of the composite treatment of the bearing ring 5 include: operating the controller to adjust the current size and the number of impacts, the electromagnetic impact device generates electromagnetic impacts to continuously impact the bearing ring 5, the primary uses an industrial frequency power supply of 50HZ, and the primary current range is 0~300A. The electromagnetic field, as an energy carrier with high transmission rate and high energy flow density, can directly transfer energy to the atomic scale of the material, change the atomic arrangement, matching and migration behaviors, thereby realizing the regulation of the material structure and performance. Under the action of temperature rise and compressive stress, the matrix around the cavities on the surface of the bearing ring 5 moves, and there is a resistance difference between the holes, cracks and the surrounding materials. After the electromagnetic impact, the temperature rise occurs at the impacted place of the bearing ring 5, and the holes and cracks will cause the bearing ring 5 to have an uneven temperature rise, thereby generating a higher thermal compression stress near the holes and cracks, driving the flow of the bearing ring 5 matrix and the healing of the holes and cracks, and the electromagnetic impact causes the dislocation around the carbide to rearrange, that is, the atoms diffuse and migrate, so that the electromagnetic impact treatment can effectively repair the cracks and holes on the surface of the cold-rolled bearing ring 5.

[0040] Reference Figure 3 In step S2, the specific operation steps of carburizing include: step S21, the bearing ring 5 after step S1 is placed in a vacuum atmosphere furnace for carburizing heating and austenitization, the bearing ring 5 is heated to 900°C and then carburized, and after being heated to 945°C, the bearing ring 5 enters the strong carburizing and diffusion stage, the heating time of the strong carburizing and diffusion stages are 8h40min and 4h20min respectively, the environmental carbon content of the strong carburizing and diffusion stages is 1.20% and 1.00% respectively, by increasing the carburizing temperature, shortening the carburizing time, and reducing the concentration of environmental carbon, a higher surface carbon content is obtained, so that in the subsequent heating of the bearing ring 5, the content of martensite and ferrite in the surface layer increases, and the content of non-martensite decreases, thereby improving the hardness and toughness of the surface layer of the bearing ring 5, and at the same time, the carburizing time is shortened, which can improve the heat treatment production efficiency of the bearing ring 5; Reference Figure 3, step S22, austenitization includes heating the bearing ring 5 after step S21 to 840°C in a vacuum atmosphere furnace for 20 minutes, cooling to below the Ms value, and a part of the existing austenite needs to be transformed at a high temperature above 900°C, and the cold rolling causes plastic changes such as dislocation and small-angle crystals in the internal structure of the bearing ring 5, which reduces the activation energy of austenite transformation, reduces the heat energy required to generate austenite, and accelerates the austenite phase transformation process. At 840°C, the transformation can begin. At the same time, plastic changes such as dislocation and small-angle crystals The changes increase the austenite nucleation rate, refine the austenite grains, and provide a large number of fast expansion channels for carbon atoms, accelerating the dissolution of carbides during the isothermal austenitization process; as the carbides dissolve, the stress concentration of the bearing ring 5 is relieved, and when the bearing ring 5 is working, the spalling area of ​​the friction layer will also decrease during the wear process, and the wear resistance and strength of the bearing ring 5 will be improved. At the same time, the increase in austenite will increase the residual austenite content in the later period, thereby increasing the crack initiation and expansion resistance, and improving the wear resistance of the bearing ring 5.

[0041] Reference Figure 3 In step S3, the specific operation steps of bainite quenching include: step S31, the bearing ring 5 after step S2 is heated to 200°C in a vacuum atmosphere furnace for 5 minutes, and a martensite pre-quenching process is introduced between austenitization and bainite isothermal quenching and tempering. By generating part of the pre-quenched martensite, dislocations are generated in the supercooled austenite around the martensite, which can promote the transformation of bainite and thus improve the heat treatment efficiency. At the same time, the generated pre-quenched martensite and the final quenched martensite can divide the original austenite grains and refine the structure for multiple times, thereby improving the impact toughness and wear resistance of the tapered roller bearing ring 5; Reference Figure 3, step S32, the bearing ring 5 after step S31 is heated to 240°C in a vacuum atmosphere furnace for 20 minutes. The ferrite in the lower bainite has a dislocation substructure and has better toughness than martensite. An appropriate amount of lower bainite is introduced into the bearing ring 5 to improve its toughness. When heated, a complete lower bainite structure needs to be kept at the bainite temperature for a long time. The pre-quenched martensite produced after pre-quenching introduces dislocation into the nearby austenite during phase transformation. The carbide / austenite interface in the bearing ring 5 can be a lower bainite. The austenite provides nucleation sites to promote the transformation of bainite, thereby shortening the incubation period of bainite and the transformation time of lower bainite; similarly, there is a large amount of lower bainite near the carbide of the bearing ring 5. During the transformation process, the bainite distributes carbon to the surrounding austenite, which is beneficial to the formation of film-like residual austenite and to the improvement of the impact toughness and wear resistance of the bearing ring. The bainite refines the matrix of the bearing ring 5 and enhances the plastic deformation of the lower bainite during the stretching process, so that the distribution of the lower bainite becomes uniform, which is beneficial to the improvement of the strength of the bearing ring 5. Reference Figure 4 In step S4, the specific operation steps of cooling the bearing ring 5 through the water bath furnace include placing the bearing ring 5 after step S3 in the water bath furnace, immersing it in the water quenching medium and cooling it to 70°C. The KR9028 quenching medium using water instead of oil has no smoke, and the workpiece does not need to be cleaned after quenching, thereby reducing the loss of water resources.

[0042] Reference Figure 3 In step S5, the specific operation steps of tempering the bearing ring 5 through the tempering furnace include: high temperature tempering, the bearing ring 5 after step S3 is placed in the crucible 9 of the vacuum magnetic field heating furnace, heated to 530°C, and the heating time is 2h. The different magnetic properties of the parent phase and the generated phase in the phase change process are used to affect the thermodynamic and kinetic processes of the phase change through a strong magnetic field, thereby improving the final microstructure. Carbides will also dissolve during the tempering process, and the strong magnetic field will promote the precipitation of carbides. At the same time, in a strong magnetic field, martensite belongs to a ferromagnetic phase and will also undergo mutation and deformation, thereby affecting the movement of adjacent austenite and causing dislocation, thereby increasing the dislocation density of the austenite and improving the hardness and tensile strength of the bearing ring 5.

[0043] Embodiment 3 discloses a method for heat treatment of a bearing surface.

[0044] Reference Figure 4 , including the following specific operation steps: step S1, cold rolling to form a bearing ring 5, the bearing ring 5 is subjected to composite treatment; step S2, the bearing ring 5 is carburized and austenitized in a vacuum atmosphere furnace, and the phase transformation of martensite belongs to the process of volume expansion; step S3, the bearing ring 5 is bainite quenched in a vacuum atmosphere furnace; step S4, the bearing ring 5 is cooled in a water bath furnace; step S5, the bearing ring 5 is tempered in a tempering furnace.

[0045] Reference Figure 4 In step S1, the specific operation steps of the composite treatment of the bearing ring 5 include: operating a flame spray gun to pre-spray the outer surface of the bearing ring 5, the thickness of the pre-spray coating of the bearing ring 5 is 1 mm, and the pre-spray coating of the bearing ring 5 is induction remelted. The bearing ring 5 is pre-sprayed using an HG-FMS-II type oxygen-acetylene high-energy flame spray gun. The remelting temperature is not less than 1000°C, and the time is not less than 25s. The pre-spray coating material uses high-hardness nickel-chromium-borosilicate alloy powder, which can improve the toughness of the coating and improve the hardness of the surface of the bearing ring 5.

[0046] Reference Figure 4 In step S2, the specific operation steps of carburizing include: step S21, the bearing ring 5 after step S1 is placed in a vacuum atmosphere furnace for carburizing heating and austenitization, the bearing ring 5 is heated to 900°C for carburizing, and after heating to 945°C, the bearing ring 5 enters the strong carburizing and diffusion stage, the heating time of the strong carburizing and diffusion stages is 8h40min and 4h20min respectively, and the environmental carbon content of the strong carburizing and diffusion stages is 1.20% and 1.00% respectively; Reference Figure 4 Step S22, austenitizing includes heating the bearing ring 5 after step S21 to 840° C. in a vacuum atmosphere furnace for 20 minutes, and cooling to below the Ms value.

[0047] Reference Figure 4 In step S3, the specific operation steps of bainite quenching include: step S31, the bearing ring 5 after step S2 is heated to 200°C in a vacuum atmosphere furnace for 5 minutes, and the martensite generated during the pre-quenching process divides the original austenite grains during the phase transformation process, which limits the growth space of the subsequently transformed bainite in the grain, plays a role in refining the structure of the bearing ring 5, is conducive to the formation of a dense structure refinement layer on the wear mark sub-surface of the bearing ring 5, and inhibits the occurrence of fatigue spalling; Reference Figure 4 In order to ensure the impact toughness and hardness of the bearing ring 5, the content of pre-quenched martensite + secondary quenched martensite is 50~60%, the pre-quenching temperature is 200℃, and the content of pre-quenched martensite is 25~35%, which can make the bearing ring 5 have sufficient toughness.

[0048] Reference Figure 4 , step S32, the bearing ring 5 after step S31 is heated to 240° C. in a vacuum atmosphere furnace for 20 min. The ferrite in the lower bainite has a dislocation substructure, which can relieve stress concentration during the stretching process through plastic deformation and inhibit the formation of necking, which is beneficial to improving the strength of the bearing ring 5; The martensite finally generated in the bearing ring 5 is composed of the pre-quenched martensite generated in the pre-fire process and the secondary quenched martensite generated in the isothermal cooling process of the bainite. The secondary quenched martensite generated later squeezes the pre-quenched martensite and the lower bainite due to volume expansion, which increases the dislocation density of the lower bainite, thereby improving the strength of the bearing ring 5. The bearing ring 5 is isothermally heated at 240°C for 20 minutes to ensure that the content of lower bainite is not less than 15%, so that the bearing ring 5 has a good hardness.

[0049] Reference Figure 4 In step S4, the specific operation steps of cooling the bearing ring 5 through the water bath furnace include placing the bearing ring 5 after step S3 in the water bath furnace, immersing it in the aqueous quenching medium and cooling it to 70°C.

[0050] Reference Figure 4 In step S5, the specific operation steps of tempering the bearing ring 5 through the tempering furnace include: low-temperature tempering, the bearing ring 5 after step S3 is placed in the tempering furnace and heated to 160°C for 2 hours. In the quenching and low-temperature tempering structure, the residual austenite has good plasticity, so that when the bearing ring 5 is under the heat and force of the friction process, the residual austenite in the bearing ring 5 gradually transforms into martensite, which improves the hardness of the bearing ring 5 and reduces the plastic deformation and pear peeling degree of the surface of the bearing ring 5. At the same time, the formed martensite generates compressive stress on the surrounding tissues through volume expansion, inhibits the initiation and expansion of cracks in the bearing ring, and is conducive to improving the wear resistance of the bearing ring 5; The tempering temperature of the secondary quenched martensite is relatively low, so that the hardness of the secondary quenched martensite is relatively high, thereby improving the hardness of the bearing ring 5.

[0051] The above are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A bearing surface heat treatment device, characterized in that: The invention comprises a plurality of bearing rings (5), a heating device, an electromagnetic device, a coating device and a controller, wherein the heating device comprises a vacuum atmosphere furnace, a water bath furnace and a tempering furnace, the electromagnetic device comprises an electromagnetic impact device and a vacuum magnetic field heating furnace, and the vacuum atmosphere furnace, the water bath furnace, the tempering furnace, the electromagnetic impact device and the vacuum magnetic field heating furnace are all connected to the controller for communication.

2. A bearing surface heat treatment device according to claim 1, characterized in that: The electromagnetic impact device comprises a thermal imager, a power supply, a converter (1), a primary induction coil (2) and a secondary induction coil (3); an iron core is arranged between the primary induction coil (2) and the secondary induction coil (3); copper electrodes are fixedly connected to both ends of the secondary induction coil (3); an oscilloscope (4) is electrically connected to the secondary induction coil (3); the converter (1) is electrically connected to the primary induction coil (2); and one of the bearing rings (5) is clamped between the two copper electrodes.

3. A bearing surface heat treatment device according to claim 2, characterized in that: The vacuum magnetic field heating furnace comprises an outer shell, an inner shell and a thermocouple, the outer surface of the inner shell is fixedly connected to a magnet (6), the interior of the inner shell is fixedly connected to an insulating layer (7), the inner surface of the insulating layer (7) is fixedly connected to a resistance wire (8), the interior of the insulating layer (7) is fixedly connected to a crucible (9), a probe of the thermocouple is overlapped on the outer surface of the crucible (9), and one of the bearing rings (5) is placed inside the crucible (9).

4. A bearing surface heat treatment device according to claim 3, characterized in that: The coating device comprises a flame spraying gun and an induction remelting device, and both the flame spraying gun and the induction remelting device are communicatively connected with a controller.

5. A bearing surface heat treatment method, characterized in that: The bearing ring (5) is heat treated by using the bearing surface heat treatment device according to claim 4, comprising the following specific operating steps: Step S1, cold rolling to form a bearing ring (5), and the bearing ring (5) undergoes a composite treatment; Step S2, the bearing ring (5) is carburized and austenitized in a vacuum atmosphere furnace; Step S3, the bearing ring (5) is subjected to bainite quenching in a vacuum atmosphere furnace; Step S4, cooling the bearing ring (5) in a water bath furnace; Step S5: The bearing ring (5) is tempered in a tempering furnace.

6. A bearing surface heat treatment method according to claim 5, characterized in that: In step S1, the specific operation steps of performing composite treatment on the bearing ring (5) include: The controller is operated to adjust the current size and the number of impacts. The electromagnetic impact device generates electromagnetic impacts to continuously impact the bearing ring (5). The primary side adopts industrial frequency power supply, and the primary current range is 0~300A.

7. A bearing surface heat treatment method according to claim 5, characterized in that: In step S1, the specific operation steps of performing composite treatment on the bearing ring (5) include: A flame spray gun is operated to pre-spray the outer surface of the bearing ring 5, wherein the pre-spray coating thickness of the bearing ring (5) is 1 mm. The pre-spray coating of the bearing ring (5) is induction remelted, wherein the remelting temperature is not less than 1000° C. and the time is not less than 25 seconds. The pre-spray coating material is made of high-hardness nickel-chromium-boron-silicon alloy powder.

8. A bearing surface heat treatment method according to claim 6 or 7, characterized in that: In step S2, the specific operation steps of carburizing include: step S21, the bearing ring (5) after step S1 is placed in a vacuum atmosphere furnace for carburizing heating and austenitization, the bearing ring (5) is heated to 900° C. and then carburized, and after being heated to 945° C., the bearing ring (5) enters a strong carburizing and diffusion stage, the heating time of the strong carburizing and diffusion stages is 8 hours and 40 minutes and 4 hours and 20 minutes respectively, and the environmental carbon content of the strong carburizing and diffusion stages is 1.20% and 1.00% respectively; Step S22, the austenitizing comprises heating the bearing ring (5) after step S21 to 840° C. in a vacuum atmosphere furnace for 20 minutes.

9. A bearing surface heat treatment method according to claim 8, characterized in that: In step S3, the specific operation steps of bainite quenching include: step S31, heating the bearing ring (5) after step S2 to 200° C. in a vacuum atmosphere furnace for 5 minutes; Step S32, heating the bearing ring (5) after step S31 to 240° C. in a vacuum atmosphere furnace for 20 minutes; In step S4, the specific operation steps of cooling the bearing ring (5) through the water bath furnace include placing the bearing ring (5) after step S3 in the water bath furnace, immersing it in an aqueous quenching medium and cooling it to 70° C.

10. A bearing surface heat treatment method according to claim 9, characterized in that: In step S5, the bearing ring (5) is tempered in a tempering furnace. The specific operation steps include: High temperature tempering: the bearing ring (5) after step S3 is placed in a crucible (9) of a vacuum magnetic field heating furnace and heated to 530° C. for 2 hours; Low temperature tempering: the bearing ring (5) after step S3 is placed in a tempering furnace and heated to 160° C. for 2 hours.

Citation Information

Cited By

  • Extreme-performance forming and manufacturing method for multiple heterogeneous structures of high-carbon-chromium bearing