Method for removing dithionate radical by controlling oxidation-reduction potential in two-stage leaching

Through the two-stage leaching process, the redox potential decomposition of manganese disulfate is controlled, which solves the problem of manganese disulfate generation in SO2 wet reduction manganese ore, and improves the purity of manganese sulfate and the industrial feasibility of the process.

CN119040669APending Publication Date: 2024-11-29GUANGXI ESOKE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411149537.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the SO2 wet reduction process of manganese ore, the formation of manganese disulfate affects the purity of the manganese sulfate leaching liquid and the corrosion of the equipment, limiting the industrial application of the process, and it is difficult for the prior art to effectively remove and reduce its impact on subsequent processes.

Method used

The two-stage leaching process is adopted. The first stage inhibits the formation of manganese disulfate through control conditions, and the second stage controls the redox potential to decompose the produced manganese disulfate to reduce its impact on the subsequent process.

Benefits of technology

It effectively reduces the concentration of manganese disulfate in the manganese sulfate leaching solution, improves the purity of manganese sulfate, simplifies process conditions, reduces energy consumption and operating costs, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040669A_ABST
    Figure CN119040669A_ABST
Patent Text Reader

Abstract

The invention discloses a method for removing dithionate radicals by controlling oxidation-reduction potential in two-stage leaching, and discloses a method for removing dithionate radicals by two-stage leaching in a process of reducing pyrolusite by SO2 wet process. The method comprises the following steps: firstly, realizing high-efficiency extraction of manganese element and high-efficiency absorption of SO2 by utilizing a first-stage leaching process, and reducing the generation of a byproduct S2O62-by controlling process conditions; and then, in the second-stage leaching process, the decomposition of the impurity S2O62-is promoted by controlling the oxidation-reduction potential of a reaction system, so that the influence of the S2O62-on the quality of the high-purity manganese sulfate is reduced. In the second-stage leaching process, the oxidation-reduction potential of the reaction system is controlled to be larger than or equal to 590 mV by controlling the temperature of the reaction system, the acidity of the solution, the type and dosage of an oxidizing agent and other process parameters, and therefore dithionate radicals in the leaching solution are efficiently decomposed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention relates to the technical fields of environmental protection and metallurgy, and relates to a method for removing dithionate by controlling the redox potential in two-stage leaching, and also relates to a method for removing dithionate by utilizing two-stage leaching in a SO2 wet reduction process of pyrolusite. [Background technology]

[0002] The main component of pyrolusite is MnO2. Since it can stably exist in acid or alkaline solution, in the process of processing pyrolusite by hydrometallurgical process, insoluble Mn(IV) must first be reduced to acid-soluble Mn(II). The commonly used reduction roasting method currently has large investment, high energy consumption, and large pollution to the environment. The non-roasting two-ore method (wet reduction process of pyrolusite and pyrite) has the disadvantages of low metal recovery rate, large amount of waste residue, and pollution to the environment.

[0003] SO2 can directly undergo redox reaction with manganese dioxide in pyrolusite in the liquid phase to generate manganese sulfate. Compared with the traditional reduction roasting method, this process simplifies and shortens the production process, saves investment and site, saves a lot of energy consumption in the roasting process, and avoids the pollution of the environment by CO2 and CO waste gas generated in the roasting reduction process. At the same time, this technology can be combined with the sulfuric acid production process, can be used for the treatment of tail gas in the process, and can also use the heat generated by combustion to achieve comprehensive industrial recycling, which has good development prospects. However, because there will be a side reaction in the leaching reaction process to produce manganese dithionate (MnS2O6).

[0004] The formation of MnS2O6 will affect the purity of manganese sulfate in the pyrolusite leaching solution, increasing the difficulty of utilizing the pyrolusite leaching solution. Excessive MnS2O6 content will seriously affect the manganese sulfate crystallization production process and product quality. 2- During the high temperature process, it will decompose and release SO2, which has the risk of corroding equipment and causing secondary pollution, thus limiting the large-scale industrial application of this process. In order to prepare manganese sulfate by wet leaching manganese from manganese ore using SO2 in flue gas, the problem of manganese dithionate in the manganese sulfate leaching solution must be solved.

[0005] The chemical properties of manganese dithionate are very stable and difficult to remove or oxidize. Therefore, on the one hand, it is necessary to consider inhibiting the formation of manganese dithionate during the sulfur dioxide leaching of manganese oxide ore, thereby reducing the content of manganese dithionate in the desulfurization solution; on the other hand, it is necessary to decompose the produced manganese dithionate to completely reduce the impact of the by-product manganese dithionate on the subsequent process. Studies have pointed out that the redox potential, acidity, reaction temperature and reaction time of the reaction system have a great influence on the formation of manganese dithionate.

[0006] In the prior art, by adding 0.2 to 100 g of granular activated carbon to 1 L of pyrolusite slurry and simultaneously blowing in air or oxygen, the pH value of the slurry in the entire manganese ore leaching process is made lower than 3.5, which can effectively inhibit the generation of manganese dithionate; however, in order to inhibit the generation of manganese dithionate in the flue gas desulfurization manganese leaching process by this method, additional activated carbon particles need to be added, which not only increases the process cost, but also increases the difficulty of subsequent solid-liquid separation and affects the electrolysis process; on the other hand, this method requires continuous blowing in of oxygen or air during the sulfur dioxide leaching process of manganese ore, which will cause a large amount of energy consumption and increase the difficulty of industrial operation. [Summary of the invention]

[0007] In order to solve the problem of excessive manganese dithionate content in the desulfurization liquid of manganese oxide ore affecting the purity of manganese sulfate in the prior art, the present invention proposes a method for controlling the redox potential in two-stage leaching to remove dithionate, and also a method for removing dithionate by two-stage leaching in a SO2 wet reduction process of pyrolusite. It is necessary to consider both the effective reduction of the content of manganese dithionate in the desulfurization liquid of manganese oxide ore and the industrial operability of the implementation process and the avoidance of increased operating costs, so as to ensure the advantages of manganese oxide ore desulfurization and manganese production technology compared with the traditional "reduction roasting-SO2 acid production-sulfuric acid leaching manganese" process. The present invention adopts a two-stage leaching process. In the first leaching process, under the premise of ensuring the efficient leaching rate of manganese and the efficient absorption of sulfur dioxide, the generation of manganese dithionate is suppressed to the maximum extent; in the second leaching process, the generated manganese dithionate is decomposed by controlling the redox potential. Thereby, the influence of manganese dithionate on the subsequent process and the quality of the final product is completely reduced.

[0008] The purpose of the present invention is achieved through the following technical solutions:

[0009] A method for removing dithionate by controlling the redox potential in a two-stage leaching process comprises the following steps: a first stage leaching process and a second stage leaching process;

[0010] The first stage leaching process includes the following steps:

[0011] S1-1, preparing pyrolusite powder into pyrolusite slurry and adjusting the pH value to 0.5-2.0 with sulfuric acid; preparing alkaline solution as tail gas absorption liquid;

[0012] The pyrolusite powder is selected from manganese dioxide powder with a manganese content of 10wt% to 40wt%, and is sieved through a 100-mesh sieve; the mass-to-volume ratio of the pyrolusite powder to water is 1Kg:(3-6)L;

[0013] S1-2, adding the slurry prepared in step S1-1 to a reaction leaching device, and introducing SO2 into the reaction leaching device under heating and stirring conditions, wherein the reaction parameters are leaching temperature of 40-90°C, leaching time of 60-300min, SO2 ratio concentration of 10%-20%, and stirring rate of 200-600rpm;

[0014] S1-3, when the manganese leaching rate in the manganese ore reaches more than 95%, stop the first stage reaction, and after the first stage reaction is completed, close and exhaust the SO2 in the reaction system;

[0015] The second stage leaching process includes the following steps:

[0016] S2-1. After the first stage of leaching reaction is completed, under heating conditions, the feed port is opened, sulfuric acid is added to adjust the pH value of the reaction system to 0.05-1.0, and an oxidant is added to adjust the redox potential to ≥590mV. The amount of oxidant pyrolusite added is 1-3 times the theoretical amount required for the content of dithionate produced in the oxidative decomposition solution, and is calculated based on the content of manganese dioxide, the effective ingredient in pyrolusite; the second stage leaching time is 0.5-5h; the leaching temperature is 40-100°C;

[0017] The oxidant is selected from pyrolusite, manganese dioxide, and hydrogen peroxide;

[0018] S2-2. Determine the concentration of dithionate and the redox potential in the solution until the concentration of dithionate and the redox potential reach equilibrium and then terminate the reaction. The concentration of manganese dithionate in the obtained leaching solution is less than 0.5 g / L.

[0019] In the present invention:

[0020] The main reactions in the first leaching process are:

[0021] SO2+H2O=H2SO3

[0022] SO2+MnO2=MnSO4

[0023] MnO2+H2SO3=MnSO4+H2O

[0024] MnO2+2SO2=MnS2O6

[0025] MnO2+2H2SO3=MnS2O6+2H2O

[0026] The main reactions in the second leaching process are:

[0027] MnS2O6=SO2↑+MnSO4

[0028] SO2+MnO2=MnSO4

[0029] MnO2+MnS2O6=2MnSO4

[0030] Furthermore, in step S1-1, the alkali solution is selected from sodium hydroxide solution, potassium hydroxide solution, and sodium carbonate solution, and the mass concentration of the alkali solution is 10% to 50%; it is loaded into the tail gas absorption device, and during the reaction process, the condition for replacing the tail gas absorption liquid is pH>9.

[0031] Furthermore, in step S1-2, the reaction leaching device is equipped with a condenser and a circulation heater, and the gas supply device is an air compressor and a dynamic gas dilution gas distributor; the N2 gas circuit switch of the dynamic gas dilution gas distributor is turned on; the main gas valve of the SO2 gas cylinder is opened, the SO2 gas cylinder pressure reducing valve is adjusted, the pressure is adjusted to 0.05-0.1MPa, the SO2 gas circuit switch of the dynamic gas dilution gas distributor is opened, and SO2 gas is supplied to the reaction system.

[0032] Further, in step 1-3), after the reaction is completed, first close the main gas valve of the sulfur dioxide cylinder and the pressure reducing valve, wait for 1 to 2 minutes for the sulfur dioxide in the air pipe to be exhausted, and then close the SO2 gas circuit switch; wait for another 5 to 10 minutes to exhaust the SO2 in the system with compressed air, then close the N2 gas circuit switch, turn off the air compressor, and turn off the power of the dilution proportioning machine.

[0033] Furthermore, in the above steps, the sulfuric acid used to adjust the pH is 98% sulfuric acid.

[0034] Compared with the prior art, the present invention has the following advantages:

[0035] 1. The method for removing dithionate by controlling the redox potential in a two-stage leaching process of the present invention comprises: firstly, utilizing the first stage leaching process to mainly realize efficient extraction of manganese and efficient absorption of SO2, and at the same time controlling the process conditions to reduce the byproduct S2O6 2- Then, the second leaching process mainly controls the redox potential of the reaction system to promote the removal of impurities S2O6 2- decomposition, thereby reducing S2O6 2- Impact on the quality of high-purity manganese sulfate. In the second stage leaching process, the redox potential of the reaction system is controlled to be greater than or equal to 590mV by controlling the process parameters such as the temperature of the reaction system, the acidity of the solution, and the type and amount of the oxidant, thereby efficiently decomposing the dithionate in the leachate. The two-stage leaching method provided by the present invention for removing manganese dithionate from the solution can effectively improve the purity of the manganese sulfate mother liquor. The concentration of manganese dithionate in the leachate obtained by the present invention can be reduced to less than 0.5g / L, effectively improving the purity of the manganese sulfate mother liquor, and the process conditions are simple and mild, the operability is strong, and it is easy to realize industrial application.

[0036] 2. The method for removing dithionite by controlling the redox potential in a two-stage leaching process described in the present invention can be combined with a sulfuric acid production process and can be used to treat tail gas SO2 in the process. The heat generated by combustion can also be used to achieve comprehensive industrial recycling, and has good development prospects.

[0037] 3. The present invention discloses a method for removing dithionate by controlling the redox potential in a two-stage leaching process, wherein the second stage leaching can utilize the heat and reaction device of the first stage reaction on the basis of the first stage leaching, thereby saving energy consumption and process production costs.

Brief Description of the Drawings

[0038] Figure 1 The present invention is a simplified flow chart of a leaching device for a method of removing dithionate by controlling the redox potential in a two-stage leaching process according to an embodiment of the present invention. [Specific implementation method]

[0039] The present invention is further described below in conjunction with the embodiments, but it should not be understood that the above subject matter of the present invention is limited to the following embodiments. Without departing from the above technical ideas of the present invention, various substitutions and changes are made according to the common technical knowledge and customary means in the art, which should all be included in the protection scope of the present invention.

[0040] Figure 1 The present invention is a simplified flow chart of the leaching device equipment of a method for removing dithionate by controlling the redox potential in a two-stage leaching as described in an embodiment.

[0041] The composition of the pyrolusite used in the examples is shown in Table 1, and the subsequent experiments were all conducted using the pyrolusite.

[0042] Table 1 Main chemical composition of pyrolusite (wt.%)

[0043]

[0044] Embodiment 1:

[0045] A method for removing dithionate by controlling the redox potential in a two-stage leaching process, comprising a first-stage leaching process and a second-stage leaching process;

[0046] The first stage leaching process comprises the following steps:

[0047] Weigh 1kg of pyrolusite powder and 3L of water to make pyrolusite slurry, add it to the reaction leaching device, then add sulfuric acid according to the acid-ore ratio of 75mL / Kg, the reaction temperature is 70℃, the concentration of SO2 introduced is 20%, the total mixed gas (sulfur dioxide and air, the same below) flow rate is 5000mL / min, the stirring rate is 300rpm, and the first leaching time is 3.5h. After analysis and detection, the manganese content in the leachate can reach 119.78g / L, and the leaching rate can reach 95.57%. At this time, S2O6 in the leachate 2- The content is 9.42g / L.

[0048] The second stage leaching process comprises the following steps:

[0049] The pH value of the reaction system was adjusted to 0.09 with sulfuric acid, the temperature was 90°C, 60g of the above-mentioned pyrolusite powder was added, and the redox potential of the reaction system was 590mV. After reacting for 3h, the S2O6 in the solution was measured. 2- The content was reduced to 0.45g / L.

[0050] Embodiment 2:

[0051] A method for removing dithionate by controlling the redox potential in a two-stage leaching process, comprising a first-stage leaching process and a second-stage leaching process;

[0052] The first stage leaching process comprises the following steps:

[0053] Weigh 1kg of pyrolusite powder and 3L of water to make pyrolusite slurry, add it to the reaction leaching device, then add sulfuric acid according to the acid-ore ratio of 75mL / Kg, the reaction temperature is 70°C, the SO2 concentration introduced into the reaction system is 20%, the total mixed gas flow rate is 5000mL / min, the stirring rate is 300rpm, and the first leaching time is 3.5h.

[0054] The second stage leaching process comprises the following steps:

[0055] The pH value of the reaction system was adjusted to 0.12 with sulfuric acid, the temperature was 100°C, 60g of the above-mentioned pyrolusite powder was added, and the redox potential of the reaction system was 610mV. After reacting for 3h, the S2O6 in the solution was measured. 2- The content was reduced to 0.07g / L.

[0056] Embodiment 3:

[0057] A method for removing dithionate by controlling the redox potential in a two-stage leaching process, comprising a first-stage leaching process and a second-stage leaching process;

[0058] The first stage leaching process comprises the following steps:

[0059] Weigh 1kg of pyrolusite powder and 3L of water to make pyrolusite slurry, add it to the reaction leaching device, then add sulfuric acid according to the acid-ore ratio of 75mL / Kg, the reaction temperature is 70°C, the SO2 concentration introduced into the reaction system is 20%, the total mixed gas flow rate is 5000mL / min, the stirring rate is 300rpm, and the first leaching time is 3.5h.

[0060] The second stage leaching process comprises the following steps:

[0061] The pH value of the reaction system was adjusted to 0.14 with sulfuric acid, the temperature was 90°C, 60g of the above-mentioned pyrolusite powder was added, and the redox potential of the reaction system was 597mV. After reacting for 3h, the S2O6 in the solution was measured. 2- The content was reduced to 0.13g / L.

[0062] Embodiment 4:

[0063] A method for removing dithionate by controlling the redox potential in a two-stage leaching process, comprising a first-stage leaching process and a second-stage leaching process;

[0064] The first stage leaching process comprises the following steps:

[0065] Weigh 1kg of pyrolusite powder and 3L of water to make pyrolusite slurry, add it to the reaction leaching device, then add sulfuric acid according to the acid-ore ratio of 75mL / Kg, the reaction temperature is 70°C, the SO2 concentration introduced into the reaction system is 20%, the total mixed gas flow rate is 5000mL / min, the stirring rate is 300rpm, and the first leaching time is 3.5h.

[0066] The second stage leaching process comprises the following steps:

[0067] The pH value of the reaction system was adjusted to 0.34 with sulfuric acid, the temperature was 100°C, 60g of the above-mentioned pyrolusite powder was added, and the redox potential of the reaction system was 594mV. After reacting for 3h, the S2O6 in the solution was measured. 2- The content was reduced to 0.16g / L.

[0068] Embodiment 5:

[0069] A method for removing dithionate by controlling the redox potential in a two-stage leaching process, characterized in that it comprises a first-stage leaching process and a second-stage leaching process;

[0070] The first stage leaching process comprises the following steps:

[0071] Weigh 1kg of pyrolusite powder and 3L of water to make pyrolusite slurry, add it to the reaction leaching device, then add sulfuric acid according to the acid-ore ratio of 75mL / Kg, the reaction temperature is 70°C, the SO2 concentration introduced into the reaction system is 20%, the total mixed gas flow rate is 5000mL / min, the stirring rate is 300rpm, and the first leaching time is 3.5h.

[0072] The second stage leaching process comprises the following steps:

[0073] The pH value of the reaction system was adjusted to 0.12 with sulfuric acid, the temperature was 103°C, 60g of the above-mentioned pyrolusite powder was added, and the redox potential of the reaction system was 612mV. After 3h of reaction, the S2O6 in the solution was measured. 2- The content was reduced to 0.03g / L.

[0074] Summarize:

[0075] Through Examples 1-5, it can be seen that by controlling the redox potential in a two-stage leaching method of the present invention to remove dithionate, the concentration of manganese dithionate in the obtained leachate is 0.03-0.45 g / L, which effectively improves the purity of the manganese sulfate mother liquor, and the process conditions are simple and mild, the operability is strong, and it is easy to realize industrial application.

[0076] The above description is only a preferred embodiment of the present invention. It should be pointed out that for those skilled in the art, without departing from the creative concept of the present invention, non-essential improvements and changes are made, which all fall within the protection scope of the present invention.

Claims

1. A method for removing dithionate by controlling the redox potential in a two-stage leaching process, characterized in that: The steps include: It includes a first stage leaching process and a second stage leaching process; The first stage leaching process includes the following steps: S1-1, preparing pyrolusite powder into pyrolusite slurry and adjusting the pH value to 0.5-2.0 with sulfuric acid; preparing alkaline solution as tail gas absorption liquid; The pyrolusite powder is selected from manganese dioxide powder with a manganese content of 10wt% to 40wt%, and is sieved through a 100-mesh sieve; the mass-to-volume ratio of the pyrolusite powder to water is 1Kg:(3-6)L; S1-2, adding the slurry prepared in step S1-1 to a reaction leaching device, and introducing SO2 into the reaction leaching device under heating and stirring conditions, wherein the reaction parameters are leaching temperature of 40-90°C, leaching time of 60-300min, SO2 ratio concentration of 10%-20%, and stirring rate of 200-600rpm; S1-3, when the manganese leaching rate in the manganese ore reaches more than 95%, stop the first stage of reaction, and after the first stage of reaction is completed, close and exhaust the SO2 in the reaction system; The second stage leaching process includes the following steps: S2-1. After the first stage of leaching reaction is completed, under heating conditions, the feed port is opened, sulfuric acid is added to adjust the pH value of the reaction system to 0.05-1.0, and an oxidant is added to adjust the redox potential to ≥590mV. The amount of oxidant pyrolusite added is 1-3 times the theoretical amount required for the content of dithionate generated in the oxidative decomposition solution, and is calculated based on the content of manganese dioxide, an effective ingredient in pyrolusite; the second stage leaching time is 0.5-5h; the leaching temperature is 40-100°C; the oxidant is selected from one of pyrolusite, manganese dioxide, and hydrogen peroxide; S2-2. Determine the concentration of dithionate and the redox potential in the solution until the concentration of dithionate and the redox potential reach equilibrium and then terminate the reaction. The concentration of manganese dithionate in the obtained leaching solution is less than 0.5 g / L.

2. The method for removing dithionate by controlling the redox potential in a two-stage leaching process according to claim 1, characterized in that: In step S1-1, the alkali solution is selected from sodium hydroxide solution, potassium hydroxide solution, and sodium carbonate solution, and the mass concentration of the alkali solution is 10% to 50%; it is loaded into the tail gas absorption device, and during the reaction process, the condition for replacing the tail gas absorption liquid is pH>9.

3. The method for removing dithionate by controlling the redox potential in a two-stage leaching process according to claim 1, characterized in that: In step S1-2, the reaction leaching device is equipped with a condenser and a circulation heater, and the gas supply device is an air compressor and a dynamic gas dilution gas distributor; the N2 gas circuit switch of the dynamic gas dilution gas distributor is turned on; the main gas valve of the SO2 gas cylinder is opened, the SO2 gas cylinder pressure reducing valve is adjusted, the pressure is adjusted to 0.05-0.1MPa, the SO2 gas circuit switch of the dynamic gas dilution gas distributor is opened, and SO2 gas is supplied to the reaction system.

4. The method for removing dithionate by controlling the redox potential in a two-stage leaching process according to claim 1, characterized in that: In step 1-3), after the reaction is completed, first close the main gas valve of the sulfur dioxide cylinder and the pressure reducing valve, wait for 1 to 2 minutes for the sulfur dioxide in the air pipe to be exhausted, and then close the SO2 gas circuit switch; wait for another 5 to 10 minutes to exhaust the SO2 in the system with compressed air, then close the N2 gas circuit switch, turn off the air compressor, and turn off the power of the dilution proportioning machine.

5. The method for removing dithionate by controlling the redox potential in a two-stage leaching process according to claim 1, characterized in that: In the above steps, the sulfuric acid used to adjust the pH is 98% sulfuric acid.