NV4-4 steel plate with high uniform elongation and good low-temperature fracture toughness and manufacturing method
Through reasonable composition design and new TMCP rolling process, the problem that low-temperature steel plates in the existing technology is difficult to meet high uniform elongation and low-temperature fracture performance, and the NV4-4 steel plate with high strength and good tissue performance is achieved to meet marine equipment harsh environmental demands.
Patent Information
- Application Number
- CN202410852020.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The existing technology is difficult to meet the needs of high uniform elongation and low-temperature fracture indicators while ensuring low-temperature toughness and welding performance. Especially when manufacturing low-temperature steel plates, production is difficult, and the existing steel plate thickness and low-temperature fracture performance cannot meet the ocean. The equipment has strict environmental requirements.
Through reasonable composition design and the new TMCP rolling process, two-stage control rolling and control are carried out using chemical components such as C: 0.05%-0.15%, Si: 0.06%-0.25%, Mn: 1.10%-1.75% and two-stage control rolling and control The cooling process forms ferrite + bainite structure, achieving high uniform elongation and excellent low-temperature fracture performance.
The obtained NV4-4 steel plate has high strength, good uniformity of tissue performance, tear resistance and low temperature fracture resistance, and meets the technical requirements of harsh marine environment. The maximum thickness is 60mm, the characteristic value of low temperature fracture is > 0.2mm, and the mechanics The performance is still good after simulated welding and heat treatment.
Smart Images

Figure CN119040766A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ship steel preparation, and in particular to a TMCP state NV4-4 high-strength low-temperature steel plate with high uniform elongation and good low-temperature fracture toughness and a manufacturing method thereof. Background Art
[0002] Fully refrigerated liquefied petroleum gas (LPG) ships can carry a variety of liquefied petroleum gases (LPG) below -50°C. They are the largest type of liquefied petroleum gas ship family and are recognized by the international shipbuilding industry as being the most difficult to design and build. LPG ships are the main type of ship for long-distance transportation of bulk liquefied petroleum gas products. They have the advantages of large carrying capacity, high safety factor, standardized operating procedures, and high added value, so they have good development prospects.
[0003] With the increase in global energy trade activities and shale gas exports, the demand for LPG carriers has further increased. The ultra-large fully refrigerated LPG carriers independently developed, designed and built by China are mainly built with cryogenic steel plates, and the demand for cryogenic steel plates for each ship is about 10,000 tons. Due to the high requirements for the comprehensive performance of steel plates (not only high strength, but also high toughness while ensuring excellent welding performance, and low-temperature impact toughness below -50°C), the manufacturing difficulty of low-temperature steel is greatly increased. In particular, the NV2-4 low-temperature steel proposed for downstream users must meet the requirements of high uniform elongation and low-temperature fracture indicators of steel plates while ensuring excellent low-temperature toughness. It is necessary to strictly control the heating temperature, rolling temperature and rapid cooling process of the billet after rolling, and the production difficulty is extremely difficult.
[0004] The Chinese invention patent with application number CN 202110031192.2 discloses "a wear-resistant steel with high uniform elongation and a method for manufacturing the same". The chemical elements in the steel are as follows: 0.75%≤C≤2.2%, 0<Si≤0.2%, 0<Mn≤0.2%, 0.1%≤Al≤0.5%; the matrix of the wear-resistant steel is ferrite, and cementite particles are evenly distributed in the crystals and on the grain boundaries of the ferrite. The method for manufacturing wear-resistant steel includes the following steps: (1) smelting and casting; (2) heating; (3) rolling; (4) cooling: cooling to room temperature at a cooling rate of ≤5°C / s. It belongs to medium-high carbon steel grades, which is essentially different from the low-carbon medium and thick plate products involved in the present invention.
[0005] The Chinese invention patent with application number CN 202110086416.X discloses "a hot-dip galvanized steel and its manufacturing method", and its composition is designed as follows: C: 0.15-0.25%, Mn: 1.8-2.4%, Si: 0.3-0.9%, Al: 0.03-0.40%, and also includes at least one of the following chemical components: Ti: 0.005-0.1%, Nb: 0.005-0.1%, Cr: 0.01-0.3%, Mo: 0.02-0.2%, and the balance is Fe and unavoidable impurities, among which the contents of Si, Al and Cr satisfy 0.5%≤Si+Al+Cr≤1.1%, and the contents of C and Si satisfy 4C+Si≤2.0%. It belongs to the hot-dip galvanized cold-rolled series products, which is completely different from the medium and thick plate products involved in the present invention.
[0006] The Chinese invention patent with application number CN 201210327206.6 discloses a "deformation-resistant X80-X100 pipeline steel plate and its manufacturing method". The composition of the steel is designed as follows: C: 0.04%~0.09%, Si: 0.10%~0.50%, Mn: 1.00%~2.00%, P≤0.015%, S≤0.005%, Nb: 0.05%~0.11%, Ti: 0.010%~0.025%, Mo≤0.30%, Cu≤0.40%, Ni≤0.50%, Cr≤0.40%, and the balance is Fe and unavoidable impurities; but the maximum thickness of the finished steel plate is only 26.4mm, and there is no CTOD fracture evaluation, which cannot meet the actual needs of marine equipment for carbon-manganese low-temperature toughness, fracture toughness and thickness.
[0007] The Chinese invention patent with application number CN 202110392421.3 discloses a "VL4-4L shipbuilding steel plate with good low-temperature toughness and its manufacturing method", whose composition is designed as follows: C: 0.04% to 0.09%; Si: 0.05% to 0.14%; Mn: 1.10% to 1.45%; S: ≤0.002%; P: ≤0.008%; Als: 0.015% to 0.045%; N: 0.003% %~0.015%; Nb: 0.01%~0.03%; Cu: 0.05%~0.15%; Cr: 0.05%~0.20%; Ni: 0.25%~0.50%; V: 0%~0.04%; Ti: 0.008%~0.014%; the balance is Fe and inevitable impurities; but it only focuses on low temperature toughness, without uniform elongation and CTOD fracture toughness evaluation, which is essentially different from the present invention.
[0008] The Chinese invention patent with application number CN 202210404964.7 discloses a "500MPa grade crack arrest steel plate and its production method", whose composition is designed as follows: C: 0.04-0.08%, Si: 0.1-0.2%, Mn: 1.5-1.6%, Cr: 0.2-0.3%, Ni: 0.5-0.7%, Mo: 0.2-0.3%, Cu: 0.35-0.50%, Nb: 0. .04~0.06%, V: 0.01~0.03%, Al: 0.02~0.05%, Ti: 0.01~0.02%, B: 0.001~0.002%, Ti / N≥3.4, the remainder is iron and impurities; its carbon equivalent is 0.46~0.51%, the cold crack sensitivity index is ≤0.22, but the low temperature resistance is only -60℃, and there is no product uniform elongation index, which is essentially different from the present invention. Summary of the invention
[0009] The present invention provides an NV4-4 steel plate with high uniform elongation and good low-temperature fracture toughness and a manufacturing method thereof. Through reasonable component design and combination with a novel TMCP rolling process, the obtained steel plate has high uniform elongation and excellent low-temperature fracture performance in the full-thickness section. The prepared high-strength, low-temperature-resistant, uniform elongation-good steel plate with a maximum thickness of 60 mm has the characteristics of good uniformity of organizational properties, tear resistance, low-temperature fracture resistance, etc., and can meet the technical requirements of the harsh and demanding marine environment for marine steel plates.
[0010] In order to achieve the above object, the present invention adopts the following technical solutions:
[0011] The invention discloses an NV4-4 steel plate with high uniform elongation and good low-temperature fracture toughness. The chemical composition of the steel plate is as follows by mass percentage: C: 0.05%-0.15%; Si: 0.06%-0.25%; Mn: 1.10%-1.75%; S: ≤0.002%; P: ≤0.008%; Als: 0.015%-0.045%; N: 0.003%-0.015%; Nb: 0.02%-0.06%; Cu: 0.10%-0.30%; Cr: 0.10%-0.30%; Ni: 0.20%-0.80%; Mo: 0.05%-0.20%; Ti: 0.008%-0.018%; the balance is Fe and unavoidable impurities.
[0012] Furthermore, the microstructure of the finished steel plate is ferrite + bainite structure, wherein the volume percentage of ferrite is 60% to 75%.
[0013] Furthermore, the yield strength of the finished steel plate is ≥335MPa, the tensile strength is ≥490MPa; the impact energy at -90°C is ≥200J; the uniform elongation is ≥10%; the low-temperature fracture CTOD characteristic value of the base material and the welding heat affected zone at -30°C to -70°C is >0.2mm.
[0014] Furthermore, after simulated welding and heat treatment at 580-600°C, the mechanical properties of the finished steel plate meet the following requirements: yield strength ≥335MPa, tensile strength ≥490MPa, uniform elongation ≥10%, and impact energy at -90°C ≥180J.
[0015] Furthermore, the thickness of the finished steel plate is 40 to 60 mm.
[0016] A method for manufacturing an NV4-4 steel plate with high uniform elongation and good low-temperature fracture toughness, the production process includes molten steel smelting and casting, billet heating, multi-stage controlled rolling, controlled cooling, and stacking slow cooling; wherein the following processes are controlled:
[0017] 1) Billet heating;
[0018] Heating temperature 1150~1250℃, soaking temperature 1130~1230℃, soaking time 60~90min;
[0019] 2) Two-stage controlled rolling;
[0020] Two-stage controlled rolling is adopted; the first stage rolling temperature is 1120-1180℃, the deformation rate of a single pass is ≥15%; the intermediate billet thickness is 1.8-2.5 times the thickness of the finished steel plate; the second stage rolling temperature is 800-900℃, the deformation rate of a single pass is ≥12%; the final rolling temperature is 780-880℃;
[0021] 3) Controlled cooling;
[0022] The average cooling rate is 10-20℃ / S, the start cooling temperature is 720-780℃, and the final cooling temperature is 430-500℃;
[0023] 4) Stacking and slow cooling: The steel plates after controlled cooling are subjected to stacking and slow cooling treatment, with the treatment time being ≥36h to obtain finished steel plates.
[0024] Furthermore, during the molten steel smelting and casting process, the treatment time of LF refining and RH refining is 20 to 40 minutes, the superheat of the molten steel in the tundish is ≤35°C; the continuous casting slab is stacked and slowly cooled for a treatment time of ≥24 hours;
[0025] Furthermore, during the molten steel smelting and casting process, the molten steel is cast in a protected manner throughout the entire process, and the continuous casting billet forming process adopts light pressure reduction and electromagnetic stirring.
[0026] Furthermore, during the molten steel smelting and casting process, the inclusions in the refined steel meet the following requirements: Class A inclusions ≤ Grade 0.5, Class B inclusions ≤ Grade 1.0, Class C inclusions ≤ Grade 1.0, and Class D inclusions ≤ Grade 0.5.
[0027] Furthermore, in the step 3), the cooling is controlled by using the ACC laminar flow fully automatic cooling control mode, and the head and tail of the steel plate are shielded throughout the whole process.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1) The chemical composition is reasonably designed. By adding appropriate amounts of alloys and using low P and S pure steel smelting, the purity of the steel is improved, ensuring that the NV4-4 high-strength steel plate has high uniform elongation and excellent low-temperature fracture performance.
[0030] 2) When heating the steel billet, the austenite temperature and the holding time in the austenite stage are reasonably designed to achieve the purpose of refining the grain size of the original austenite structure of the steel plate, ensure the smooth rolling and uniformity of the subsequent steel plate, and provide a tissue basis for improving the strength and toughness of the steel plate.
[0031] 3) Through the combination of two-stage controlled rolling + water cooling (TMCP) process, the organization of NV4-4 high-strength steel plate with high uniform elongation and excellent low-temperature fracture resistance is strengthened and toughened, the phase transformation organization is uniformly refined, the morphology and grain size are controlled, and higher dimensional accuracy and surface quality control are achieved.
[0032] 4) The prepared steel plate has high strength (yield strength ≥335MPa, tensile strength ≥490MPa), low temperature resistance (-90℃ impact energy ≥200J), uniform elongation ≥10%, maximum thickness 60mm, low temperature fracture (-30℃, -50℃, -70℃) CTOD (crack tip opening displacement) characteristic value of parent material and welding heat affected zone>0.2mm, and the mechanical properties of the steel plate after 580-600℃ simulated welding and heat treatment still meet the yield strength ≥335MPa, tensile strength ≥490MPa, uniform elongation ≥10%, -90℃ impact energy ≥180J; its good uniformity of organizational properties, tear resistance and resistance to low temperature fracture can meet the technical requirements of marine steel plates in harsh and demanding marine environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a metallographic photograph of the finished steel plate prepared in Example 1 of the present invention.
[0034] Figure 2 This is a photograph of non-metallic inclusions in the finished steel plate prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0035] The invention discloses an NV4-4 steel plate with high uniform elongation and good low-temperature fracture toughness, wherein the chemical composition of the steel plate is, by mass percentage, C: 0.05%-0.15%; Si: 0.06%-0.25%; Mn: 1.10%-1.75%; S: ≤0.002%; P: ≤0.008%; Als: 0.015%-0.045%; N: 0.003%-0.015%; Nb: 0.02%-0.06%; Cu: 0.10%-0.30%; Cr: 0.10%-0.30%; Ni: 0.20%-0.80%; Mo: 0.05%-0.20%; Ti: 0.008%-0.018%; the remainder is Fe and unavoidable impurities.
[0036] The microstructure of the finished steel plate is ferrite + bainite structure, wherein the volume percentage of ferrite is 60% to 75%.
[0037] The yield strength of the finished steel plate is ≥335MPa, the tensile strength is ≥490MPa; the impact energy at -90℃ is ≥200J; the uniform elongation is ≥10%; the low-temperature fracture CTOD characteristic value of the base material and the welding heat affected zone at -30℃~-70℃ is >0.2mm.
[0038] After simulated welding and heat treatment at 580-600℃, the mechanical properties of the finished steel plate meet the following requirements: yield strength ≥335MPa, tensile strength ≥490MPa, uniform elongation ≥10%, and impact energy at -90℃ ≥180J.
[0039] The thickness of the finished steel plate is 40 to 60 mm.
[0040] The present invention discloses a method for manufacturing a NV4-4 steel plate with high uniform elongation and good low-temperature fracture toughness. The production process includes molten steel smelting and casting, billet heating, multi-stage controlled rolling, controlled cooling, and stacking slow cooling. The following processes are controlled:
[0041] 1) Molten steel smelting and casting;
[0042] The treatment time of LF refining and RH refining is 20-40min, and the superheat of molten steel in the tundish is ≤35℃; the continuous casting slab is stacked and slowly cooled, and the treatment time is ≥24h; the molten steel is cast with full protection, and the continuous casting slab forming process adopts light pressure and electromagnetic stirring. After refining, the inclusions in the steel meet the requirements of: Class A inclusions ≤0.5, Class B inclusions ≤1.0, Class C inclusions ≤1.0, and Class D inclusions ≤0.5.
[0043] 2) Billet heating;
[0044] Heating temperature 1150~1250℃, soaking temperature 1130~1230℃, soaking time 60~90min;
[0045] 3) Two-stage controlled rolling;
[0046] Two-stage controlled rolling is adopted; the first stage rolling temperature is 1120-1180℃, the deformation rate of a single pass is ≥15%; the intermediate billet thickness is 1.8-2.5 times the thickness of the finished steel plate; the second stage rolling temperature is 800-900℃, the deformation rate of a single pass is ≥12%; the final rolling temperature is 780-880℃;
[0047] 4) Control cooling;
[0048] The average cooling rate is 10-20℃ / S, the start cooling temperature is 720-780℃, and the final cooling temperature is 430-500℃; the controlled cooling adopts the ACC laminar flow fully automatic controlled cooling mode, and the steel plate is shielded at the head and tail throughout the process.
[0049] 5) Stacking and slow cooling: The steel plates after controlled cooling are subjected to stacking and slow cooling treatment, with the treatment time being ≥36h to obtain finished steel plates.
[0050] The present invention starts from the selection and proportion of alloy elements, steel cleanliness control, heating process improvement, rolling process optimization, cooling process control, microstructure strength and toughness matching, and finally determines the component system and its manufacturing process that can meet the purpose of the present invention. The appropriate carbon + manganese content and low alloy component system are used to realize the new low-temperature steel plate design. The production process is a new TMCP controlled rolling process. The TMCP state NV2-4L shipbuilding steel plate with a maximum thickness of 60mm is prepared using 230-360mm cross-section continuous casting billets. It has good strength and toughness matching in the full thickness section, and has high uniform elongation and good low-temperature CTOD and NDT fracture performance, so that the steel plate has good low-temperature resistance, fracture resistance and tearing characteristics, ensuring the use of low-temperature steel plates in different service environments. Technical requirements.
[0051] In the NV4-4 steel plate with high uniform elongation and good low-temperature fracture toughness described in the present invention, the action mechanism of each alloy component is as follows:
[0052] C: is a cheap element that effectively improves the strength of steel plates. However, as the carbon content increases, the plasticity, low-temperature toughness and welding crack sensitivity of the steel plates will be significantly reduced. An appropriate amount of carbon can cooperate with cooling control to ensure the strength and toughness indicators of the steel plates. From the perspective of improving the product's resistance to low-temperature fracture performance, the present invention controls the C content to 0.05% to 0.15%.
[0053] Si: It is the main deoxidizing component in the steelmaking process. It can be used as a deoxidizer and a reducing agent in the steelmaking process, which is beneficial to the improvement of the strength of the steel plate. However, when its content exceeds 0.5%, it will promote the formation of Maho Island and damage the weldability and low-temperature toughness. The appropriate addition of Si can improve the elastic limit and yield strength of steel, and can also improve the oxidation resistance of steel at high temperatures. For shipbuilding steel plates, a lower Si content can also improve the surface quality of the steel plate. The present invention aims to achieve the characteristics of the product having excellent low-temperature fracture resistance, so the Si content should not be too high. Therefore, the present invention controls the Si content to be 0.06% to 0.25%.
[0054] Mn: It is an essential element to ensure the strength and toughness of steel. Mn combines with S to form MnS, which can avoid hot cracks caused by the formation of FeS at the grain boundaries. Mn is also a good deoxidizer. An appropriate amount of manganese can improve the strength and toughness of steel, but if its content is too high, segregation will occur in the ingot, which will cause a banded structure that is difficult to eliminate after rolling, reducing the transverse performance and lamellar tear resistance of the steel plate. In order to improve the strength and toughness matching of the product, the present invention adds Mn together with nickel elements, which can improve the product's resistance to low-temperature fracture and low-temperature elongation performance. Therefore, the present invention controls the Mn content to 1.10% to 1.75%.
[0055] P: is an element that has an adverse effect on the impact value and will damage the low-temperature toughness due to segregation in the center of the slab and aggregation at the grain boundaries. In the present invention, the P content is controlled to be no higher than 0.008%.
[0056] S: is an element that has an adverse effect on the impact value and forms sulfide inclusions to become crack sources. In the present invention, the S content is controlled to be no higher than 0.002%.
[0057] Als: As a deoxidation and grain refinement element that must be added in the present invention, the added content is above 0.01%, but when the content exceeds 0.08%, hot cracks of the ingot are easily generated, and the toughness of the steel will be reduced. Therefore, the present invention controls its content to 0.015% to 0.045%.
[0058] Nb: Adding Nb to steel can effectively refine the grain size of the steel and improve the strength and toughness. However, when the addition amount is less than 0.01%, the effect is not obvious, so the present invention controls the Nb content to 0.02-0.06%.
[0059] Mo: It is the main element that expands the γ phase area, delays the formation of ferrite first during the γ→α phase transformation, and promotes the formation of acicular ferrite. It plays an important role in controlling the phase transformation structure, can effectively improve the material strength, reduce the phase transformation temperature, and reduce the critical cooling rate of bainite transformation, which is conducive to promoting bainite transformation in a wider cooling rate range, so that the thick steel plate has better process adaptability, and can effectively improve the stability of the strength and toughness properties in the thickness direction of the steel plate. Therefore, the present invention controls the Mo content to 0.05% to 0.20%.
[0060] Cu: Adding Cu to steel can improve the corrosion resistance and strength of the steel, and improve weldability, formability and machinability. Using Cu and Ni together can also avoid hot brittleness. The present invention controls the Cu content to 0.10% to 0.30%.
[0061] Cr: An important element for improving the hardenability of steel. For thick-gauge steel for shipbuilding and offshore platforms, adding a higher Cr content can effectively improve the hardenability to compensate for the strength loss caused by the thickness and improve the uniformity of performance in the thickness direction; therefore, the present invention controls the Cr content to 0.10% to 0.30%.
[0062] Ni: has a solid solution strengthening effect, can promote the alloy steel to form a stable austenite structure, has the characteristics of minimizing the Ar3 point and minimizing the increase in carbon equivalent or cold crack sensitivity coefficient Pcm, can improve the strength and toughness of the steel, and improve the hot brittleness caused by Cu in the steel. Therefore, the present invention controls the Ni content to 0.20% to 0.80%.
[0063] N: N combines with elements such as Al, Ti, and Nb to form nitrides, which are elements that refine the parent material structure. In order to achieve this effect, the N content needs to be above 0.002%; however, too much solid solution N is the cause of the deterioration of the toughness of the HAZ (heat affected zone). Reasonable control of the N content can play a role in refining the grains, so the present invention controls the N content to 0.003% to 0.015%.
[0064] Ti: A component added to improve the toughness of steel and welded parts, it works in the form of TiN. However, when its content exceeds 0.04%, it tends to form large particles of TiN and lose its desired effect. Therefore, the present invention controls the Ti content to 0.008% to 0.018%.
[0065] The manufacturing method of the NV4-4 steel plate with high uniform elongation and good low-temperature fracture toughness described in the present invention includes the following processes: molten steel smelting and casting → steel billet heating → two-stage controlled rolling → controlled cooling → stacking slow cooling. The key steps of the preparation process are as follows:
[0066] 1) Molten steel smelting and casting process: Select smelting raw materials, which should be mainly molten iron or high-quality return steel, with the content of elements such as P and S as low as possible, control the smelting composition according to the target value, strictly control the residual element content, and avoid the carbon equivalent exceeding the upper limit; LF refining and RH refining need to be processed for 20 to 40 minutes each; the superheat of the molten steel in the middle package is ≤35℃, and the casting is protected throughout the process; Class A, Class B, Class C, and Class D inclusions in the steel must meet the following requirements: Class A inclusions ≤0.5 level, Class B inclusions ≤1.0 level, Class C inclusions ≤1.0 level, and Class D inclusions ≤0.5 level; The continuous casting billet forming process adopts light pressure reduction technology, and electromagnetic stirring equipment is used, which can effectively solve the center segregation and grain size uniformity of the continuous casting billet. The continuous casting slab needs to be stacked and slowly cooled, and the stacking time is ≥24h.
[0067] 2) Billet heating process: adopt a new heating system, heating temperature 1150 ~ 1250 ℃, soaking temperature 1130 ~ 1230 ℃, soaking time 60 ~ 90min.
[0068] 3) Two-stage controlled rolling process: adopt a new two-stage controlled rolling technology, the first stage rolling temperature is 1120~1180℃, the single pass deformation rate is ≥15%; the intermediate billet thickness is 1.8~2.5 times the finished steel plate thickness; the second stage rolling temperature is 800~900℃, the single pass deformation rate is ≥12%, and the final rolling temperature is 780~880℃.
[0069] The present invention combines a large deformation rolling process to refine the original structure, control and adjust the composition of the phase change structure, the uniform refinement degree and the precipitation behavior of multi-phase particles, ensure the uniformity of the grain size on the full thickness section of the thick steel plate, and improve the uniform elongation and low temperature fracture resistance (CTOD) of the steel grade.
[0070] 4) Controlled cooling process: The average cooling rate of the steel plate is 10℃~20℃ / S, the start cooling temperature is 720~780℃, and the final cooling temperature is 430~500℃. The cooling process adopts the ACC laminar flow fully automatic cooling control mode, and the head and tail of the steel plate are shielded throughout the process to ensure the uniformity and stability of the performance of different positions of the steel plate.
[0071] 5) Stacking and slow cooling process: The steel plates after controlled cooling are stacked and slow cooled, and the slow cooling time is ≥36h to obtain finished steel plates.
[0072] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.
[0073] [Example]
[0074] The chemical composition of the NV4-4 high-strength and low-temperature marine steel plate (referred to as the steel plate) prepared in each embodiment is shown in Table 1, the molten steel smelting process parameters are shown in Table 2, the rolling and cooling process parameters of the steel plate are shown in Table 3, the conventional mechanical properties of the steel plate are shown in Table 4-1, and the mechanical properties of the steel plate after simulated welding and heat treatment of each embodiment are shown in Table 4-2; the low-temperature fracture performance of the steel plate is shown in Table 5.
[0075] Table 1 Chemical composition of steel in each example (mass percentage %)
[0076]
[0077] Table 2 Steelmaking process parameters of various examples
[0078]
[0079] Table 3 Steel plate rolling and cooling process parameters of each embodiment
[0080]
[0081] Note: t is the thickness of finished steel plate, mm.
[0082] Table 4-1 Conventional mechanical properties of finished steel plates in various embodiments
[0083]
[0084]
[0085] Table 4-2 Mechanical properties of finished steel plates in various embodiments after simulated welding and heat treatment
[0086]
[0087] Table 5 Low temperature fracture properties of finished steel plates of various embodiments
[0088]
[0089] Microstructure and inclusions of the steel plate obtained from Example 1 ( Figure 1 , Figure 2 ) It can be seen that after being processed by the new TMCP two-stage controlled rolling process described in the present invention, the steel plate structure is basically ferrite + bainite structure, the finished steel plate structure has clear grain boundaries, fine grains, and few inclusions, thereby achieving the high uniform elongation and good low-temperature fracture toughness characteristics of the NV4-4 steel plate.
[0090] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An NV4-4 steel plate with high uniform elongation and good low temperature fracture toughness, characterized in that: The chemical composition of the steel plate is calculated by mass percentage as follows: C: 0.05% to 0.15%; Si: 0.06% to 0.25%; Mn: 1.10% to 1.75%; S: ≤ 0.002%; P: ≤ 0.008%; Als: 0.015% to 0.045%; N:0.003%~0.015%; Nb : 0.02%~0.06%; Cu: 0.10%~0.30%; Cr: 0.10%~0.30%; Ni: 0.20%~0.80%; Mo: 0.05%~0.20%; Ti: 0.008%~0.018%; the balance is Fe and unavoidable impurities.
2. The NV4-4 steel plate with high uniform elongation and good low temperature fracture toughness according to claim 1, characterized in that: The microstructure of the finished steel plate is ferrite + bainite structure, wherein the volume percentage of ferrite is 60% to 75%.
3. The NV4-4 steel plate with high uniform elongation and good low temperature fracture toughness according to claim 1, characterized in that: The yield strength of the finished steel plate is ≥335MPa, the tensile strength is ≥490MPa; the impact energy at -90℃ is ≥200J; the uniform elongation is ≥10%; the low-temperature fracture CTOD characteristic value of the base material and the welding heat affected zone at -30℃~-70℃ is >0.2mm.
4. The NV4-4 steel plate with high uniform elongation and good low temperature fracture toughness according to claim 1, characterized in that: After simulated welding and heat treatment at 580-600℃, the mechanical properties of the finished steel plate meet the following requirements: yield strength ≥335MPa, tensile strength ≥490MPa, uniform elongation ≥10%, and impact energy at -90℃ ≥180J.
5. The NV4-4 steel plate with high uniform elongation and good low temperature fracture toughness according to claim 1, characterized in that: The thickness of the finished steel plate is 40 to 60 mm.
6. The method for manufacturing the NV4-4 steel plate having high uniform elongation and good low temperature fracture toughness according to any one of claims 1 to 5, characterized in that: The production process includes molten steel smelting and casting, billet heating, multi-stage controlled rolling, controlled cooling, and stacking slow cooling; the following processes are controlled: 1) Billet heating; Heating temperature 1150~1250℃, soaking temperature 1130~1230℃, soaking time 60~90min; 2) Two-stage controlled rolling; Two-stage controlled rolling is adopted; the first stage rolling temperature is 1120-1180℃, the deformation rate of a single pass is ≥15%; the intermediate billet thickness is 1.8-2.5 times the thickness of the finished steel plate; the second stage rolling temperature is 800-900℃, the deformation rate of a single pass is ≥12%; the final rolling temperature is 780-880℃; 3) Controlled cooling; The average cooling rate is 10-20℃ / S, the start cooling temperature is 720-780℃, and the final cooling temperature is 430-500℃; 4) Stacking and slow cooling: The steel plates after controlled cooling are subjected to stacking and slow cooling treatment, with the treatment time being ≥36h to obtain finished steel plates.
7. The method for manufacturing the NV4-4 steel plate with high uniform elongation and good low temperature fracture toughness according to claim 6, characterized in that: During the molten steel smelting and casting process, the treatment time of LF refining and RH refining is 20-40 minutes, and the superheat of the molten steel in the tundish is ≤35°C; the continuous casting slab is stacked and slowly cooled, and the treatment time is ≥24 hours.
8. The method for manufacturing the NV4-4 steel plate with high uniform elongation and good low temperature fracture toughness according to claim 6, characterized in that: During the molten steel smelting and casting process, the molten steel is cast in a protected manner throughout the entire process, and the continuous casting billet forming process adopts light pressure reduction and electromagnetic stirring.
9. The method for manufacturing the NV4-4 steel plate with high uniform elongation and good low temperature fracture toughness according to claim 6, characterized in that: During the molten steel smelting and casting process, the inclusions in the refined steel meet the following requirements: Class A inclusions ≤ Grade 0.5, Class B inclusions ≤ Grade 1.0, Class C inclusions ≤ Grade 1.0, and Class D inclusions ≤ Grade 0.
5.
10. The method for manufacturing the NV4-4 steel plate with high uniform elongation and good low temperature fracture toughness according to claim 6, characterized in that: In the step 3), the cooling is controlled by using the ACC laminar flow fully automatic controlled cooling mode, and the head and tail of the steel plate are shielded throughout the whole process.
Citation Information
Patent Citations
Anti-deformation X80-X100 pipeline steel plate and manufacturing method thereof
CN102851587A
500MPa-grade crack arrest steel plate and production method thereof
CN114480809A
Wear-resistant steel with high uniform elongation and manufacturing method thereof
CN114763590A
Hot-dip galvanized steel and manufacturing method thereof
CN114807737A
Acid-corrosion-resistant X70 pipeline steel plate and manufacturing method thereof
CN104388837A
Cited By
Extremely cold anti-fatigue ultrahigh-strength maritime work steel and manufacturing method thereof
CN120464944A
Extremely cold fatigue-resistant ultra-high strength marine engineering steel and its manufacturing method
CN120464944B