Polishing solution as well as preparation method and polishing method thereof
By using the combination of concentrated sulfuric acid, ethylene glycol, citric acid, corrosion inhibitor and n-butanol in the electrochemical polishing liquid, the problems of low electrochemical polishing efficiency and complex process of the existing traditional Chinese medicine bracket are solved, and the normal temperature is achieved The high-efficiency polishing under the bottom ensures smoothness and integrity of the bracket surface.
Patent Information
- Application Number
- CN202411251825.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-29
AI Technical Summary
The existing electrochemical polishing technology has problems such as low efficiency, complicated process and easy to destroy special structures for the surface treatment of shape memory metal alloy medical brackets, and the process parameters are complex and difficult to apply to actual production.
Using a polishing liquid including concentrated sulfuric acid, ethylene glycol, citric acid, corrosion inhibitor and n-butanol, the medical scaffold is treated at room temperature by electrochemical polishing method, and the strong corrosion of concentrated sulfuric acid is avoided by using citric acid and corrosion inhibitor to prevent strong corrosion of concentrated sulfuric acid, forming A uniform passivation film ensures surface integrity and smoothness.
Electrochemical polishing at room temperature is achieved, the smoothness and integrity of the surface of medical stents is improved, the operation risk and process complexity are reduced, and the corrosion inhibition ability and surface brightness of the polishing liquid are enhanced.
Smart Images

Figure CN119041000A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemical polishing, and in particular relates to a polishing liquid and a configuration method thereof, and a polishing method. Background Art
[0002] Shape memory metal alloys have unique shape memory properties and superelasticity, as well as good mechanical properties, friction and corrosion resistance, and biocompatibility, making them ideal materials for medical stents. Medical stents made of shape memory alloys need to be polished because unpolished medical stents have a high surface roughness. If they are directly implanted in the body, they will produce greater resistance to the blood and have an adverse effect on blood flow, and may further cause thrombosis.
[0003] In industry, the surface treatment of medical stents is generally carried out by combining mechanical polishing with chemical polishing. However, both mechanical polishing and chemical polishing are inefficient, cumbersome, and easily damage the special structure of the medical stent. Electrochemical polishing can obtain a smooth and uniform surface and can be applied to workpieces of various shapes. Therefore, it can be considered for the polishing of medical stents.
[0004] However, the electrochemical properties of shape memory alloys are relatively special. It is a film-forming metal that is easily passivated or self-passivated. When it is used as an anode, it is difficult to dissolve. In their paper "Electrolytic Polishing to Improve the Surface Performance of Metal Alloy Cardiovascular Stents", Sun Xiaoyu et al. disclosed a polishing scheme for cardiovascular stents using an alcohol-salt five-toxic electrolyte electrolytic polishing process. This process is used to explore the changes in the morphology, heat-affected zone, recast layer, slag, surface roughness, surface chemical composition, electrochemical corrosion and other properties of the surface of the cardiovascular stent, so as to improve the surface integrity and biocompatibility of the metal alloy stent. However, this electrolytic polishing liquid has high requirements for electrolytic equipment, and the process parameters are complicated to explore, making it difficult to apply to actual production. In the paper "Biocompatibility of Electrochemical Polished Surfaces of Ultrafine-Grained TiNi Alloys", Xu Xiaojing et al. proposed using a mixed solution of concentrated sulfuric acid and concentrated phosphoric acid to polish TiNi alloys. This double acid solution is highly corrosive, and the operating temperature is as high as 80℃-90℃, which is highly dangerous to operate. Summary of the invention
[0005] The object of the present invention is to provide a polishing liquid and a preparation method thereof, and a polishing method, which are intended to polish medical implants.
[0006] To achieve the above-mentioned purpose, the present invention provides a polishing liquid, comprising concentrated sulfuric acid, ethylene glycol, citric acid, a corrosion inhibitor, and n-butanol; in terms of mass percentage, the content of concentrated sulfuric acid is 2%-9%, the content of ethylene glycol is 0.25%-2%, the content of citric acid is 21%-32%, the content of corrosion inhibitor is 6%-12%, and the content of n-butanol is 50%-67.5%.
[0007] Optionally, the corrosion inhibitor comprises glycerol.
[0008] Optionally, the polishing liquid is prepared by first preparing solution A and solution B, and then evenly mixing the solution A, the solution B and n-butanol in proportion; wherein the solution A includes concentrated sulfuric acid and ethylene glycol, and in the solution A, the mass percentage of concentrated sulfuric acid is 80%-90%, and the mass percentage of ethylene glycol is 10%-20%; the solution B includes citric acid and the corrosion inhibitor, and in the solution B, the mass percentage of citric acid is 70%-80%, and the mass percentage of the corrosion inhibitor is 20%-30%; in the polishing liquid, the mass percentage of the solution A is 2.5%-10%, and the mass percentage of the solution B is 30%-40%.
[0009] To achieve the above-mentioned purpose, the present invention also provides a method for preparing a polishing liquid, which is used to prepare the polishing liquid as described above, comprising the following steps: preparing solution A; preparing solution B; mixing the solution A, the solution B and n-butanol in proportion; wherein the solution A comprises concentrated sulfuric acid and ethylene glycol, and in the solution A, the mass percentage of concentrated sulfuric acid is 80%-90%, and the mass percentage of ethylene glycol is 10%-20%; the solution B comprises citric acid and the corrosion inhibitor, and in the solution B, the mass percentage of citric acid is 70%-80%, and the mass percentage of the corrosion inhibitor is 20%-30%; in the polishing liquid, the mass percentage of the solution A is 2.5%-10%, and the mass percentage of the solution B is 30%-40%.
[0010] Optionally, the corrosion inhibitor comprises glycerol.
[0011] To achieve the above-mentioned objectives, the present invention also provides a polishing method, comprising: configuring a polishing liquid as described above; placing a cathode made of an inert metal at least partially in the polishing liquid, and using an object to be polished as an anode and immersing it in the polishing liquid; keeping the polishing liquid at a preset temperature, and supplying power to the cathode, the anode, and the circuit formed by the polishing liquid to perform a polishing operation.
[0012] Optionally, the cathode is arranged in parallel with the anode.
[0013] Optionally, the distance between the cathode and the anode is 5 mm-30 mm.
[0014] Optionally, the preset temperature is 10° C.-30° C., the current in the circuit formed by the cathode, the anode and the polishing liquid is 0.5A-2A, and the polishing time is 10s-60s.
[0015] Optionally, the target object includes a medical stent, and the medical stent is made of metal material.
[0016] Compared with the prior art, the polishing liquid and its preparation method and polishing method of the present invention have the following advantages: the aforementioned polishing liquid includes concentrated sulfuric acid, ethylene glycol, citric acid, corrosion inhibitor and n-butanol; in terms of mass percentage, the content of concentrated sulfuric acid is 2%-9%, the content of ethylene glycol is 0.25%-2%, the content of citric acid is 21%-32%, the content of corrosion inhibitor is 6%-12%, and the content of n-butanol is 50%-67.5%. When the polishing liquid is used to electrochemically polish the medical stent, the polishing operation can be performed at room temperature, and the introduction of citric acid can effectively avoid the strong corrosion of the concentrated sulfuric acid to the medical stent, thereby ensuring the surface integrity of the medical stent during the polishing process.
[0017] Furthermore, the polishing liquid is prepared by: first preparing solution A and solution B, and then evenly mixing solution A, solution B and n-butanol; wherein solution A includes concentrated sulfuric acid and ethylene glycol, and in solution A, the mass percentage of concentrated sulfuric acid is 80%-90%, and the mass percentage of ethylene glycol is 10%-20%; solution B includes citric acid and the corrosion inhibitor, and in solution B, the mass percentage of citric acid is 70%-80%, and the mass percentage of the corrosion inhibitor is 20%-30%; in the polishing liquid, the mass percentage of solution A is 2.5%-10%, and the mass percentage of solution B is 30%-40%. The polishing liquid prepared in this way can make the surface of the medical stent brighter after polishing. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings are used to better understand the present invention and shall not constitute improper limitations of the present invention.
[0019] Figure 1 FIG. 1 is a schematic diagram of the surface morphology of an unpolished medical stent used in Example 1 of the present invention.
[0020] Figure 2 yes Figure 1 The figure is a schematic diagram of the morphology of the medical stent after being polished with the polishing liquid provided in Example 1.
[0021] Figure 3FIG. 4 is a schematic diagram of the morphology of the surface of the unpolished medical stent used in Example 2 of the present invention.
[0022] Figure 4 yes Figure 3 The figure is a schematic diagram of the morphology of the medical stent after being polished by the polishing liquid provided in Example 2. DETAILED DESCRIPTION
[0023] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the present embodiment only illustrate the basic concept of the present invention in a schematic manner, and only the components related to the present invention are shown in the figure instead of being drawn according to the number, shape and size of the components in the actual implementation. The type, quantity and proportion of each component in the actual implementation can be a random change, and the component layout type may also be more complicated.
[0024] In addition, each embodiment of the following description has one or more technical features, but this does not mean that the user of the present invention must implement all the technical features in any embodiment at the same time, or can only implement part or all of the technical features in different embodiments separately. In other words, under the premise that implementation is possible, those skilled in the art can selectively implement part or all of the technical features in any embodiment according to the disclosure of the present invention and according to the design specifications or implementation requirements, or selectively implement a combination of part or all of the technical features in multiple embodiments, thereby increasing the flexibility of the implementation of the present invention.
[0025] The purpose of the present invention is to provide a polishing liquid and a preparation method thereof, wherein the polishing liquid can be used for electrochemical polishing of a medical stent, so as to improve the surface smoothness of the medical stent and enable the polishing operation to be performed at room temperature, thereby improving the safety of the polishing operation.
[0026] The polishing liquid provided in the embodiment of the present invention includes concentrated sulfuric acid, ethylene glycol, citric acid, a corrosion inhibitor, and n-butanol. In terms of mass percentage, the content of concentrated sulfuric acid is 2%-9%, the content of ethylene glycol is 0.25%-2%, the content of citric acid is 21%-32%, the content of corrosion inhibitor is 6%-12%, and the content of n-butanol is 50%-67.5%. It should be understood that the concentrated sulfuric acid here refers to a sulfuric acid solution with a mass percentage of 98%.
[0027] The polishing liquid can be used in electrochemical polishing of a target object made of metal. The target object is, for example, a medical stent. The following description will always take the medical stent as the target object.
[0028] During the polishing process, the medical stent acts as an anode, and the ions generated by the electrolysis of concentrated sulfuric acid and citric acid play a conductive role, so that an oxidation-reduction reaction occurs, thereby removing the oxide layer on the surface of the medical stent. Ethylene glycol and n-butanol together provide sufficient viscosity for the polishing liquid. The cations formed by the metal constituting the medical stent combine with the citrate to form a salt and cover the surface of the medical stent to form a passivation film, thereby preventing the concentrated sulfuric acid from causing strong corrosion to the medical stent and causing the fine structure of the medical stent to be destroyed. The corrosion inhibitor is adsorbed on the surface of the medical stent, which is conducive to the diffusion of the citrate on the surface of the medical stent, and improves the uniformity of the dispersion of the salt formed by the metal cation and the citrate on the surface of the medical stent, thereby improving the uniformity of the distribution of the passivation film and enhancing the corrosion inhibition ability of the polishing liquid on the medical stent. The combined effect of these reactions enables the polishing liquid to effectively improve the leveling ability of the surface of the medical stent. In addition, the polishing liquid also has the advantages of easy availability of raw materials and low cost.
[0029] Optionally, the method for preparing the polishing liquid includes: first preparing solution A and solution B, and then mixing the solution A, the solution B and n-butanol in proportion. Wherein, the solution A includes concentrated sulfuric acid and ethylene glycol, and in terms of mass percentage, the content of concentrated sulfuric acid in the solution A is 80%-90%, and the content of ethylene glycol in the solution A is 10%-20%; the solution B includes citric acid and the corrosion inhibitor, and in terms of mass percentage, the content of citric acid in the solution B is 70%-80%, and the content of the corrosion inhibitor is 20%-30%. In terms of mass percentage, the content of the solution A in the polishing liquid is 2.5%-10%, the content of the solution B is 30%-40%, and the content of n-butanol is 50%-67.5%. The polishing liquid prepared in this way can enhance the surface brightness of the medical stent during the polishing process.
[0030] Those skilled in the art can understand that the specific operation of preparing the solution A includes: first weighing concentrated sulfuric acid and ethylene glycol in proportion, then slowly adding the concentrated sulfuric acid to the ethylene glycol, and during the adding process, stirring the mixed solution of concentrated sulfuric acid and ethylene glycol in the same direction.
[0031] In addition, in some specific embodiments, the corrosion inhibitor includes glycerol (ie, propylene glycol).
[0032] The embodiment of the present invention also provides a polishing method based on the aforementioned polishing liquid, the polishing method comprising the following steps: first, preparing the polishing liquid. Then, placing a cathode made of an inert metal at least partially in the polishing liquid, and using the medical stent as an anode and immersed in the polishing liquid. Thereafter, the polishing liquid is kept at a preset temperature, and power is supplied to a circuit formed by the cathode, the anode, and the polishing liquid to perform a polishing operation.
[0033] The inert metal is titanium, for example. The preset temperature is greater than or equal to 10° C. and less than or equal to 30° C., the current in the circuit formed by the cathode, the anode, and the polishing liquid is greater than or equal to 0.5A and less than or equal to 2A, and the polishing time is not less than 10s and not more than 60s.
[0034] Preferably, the cathode is arranged in parallel with the anode so that the distance between the cathode and the anode at any position is maintained at a preset value. According to actual needs, the preset value is greater than or equal to 5 mm and less than or equal to 30 mm. It should be noted that the distance between the cathode and the anode refers to the width of the gap between the cathode and the anode.
[0035] In order to make the objects, advantages and features of the present invention more clear, the present invention is further described in detail below in conjunction with specific embodiments.
[0036] The medical stent used in the first embodiment is a nickel-titanium stent, and the medical stent is a hollow cylindrical structure when expanded. The width of the stent rod in the medical stent is 0.05mm-0.25mm, and the thickness of the stent rod is 0.04mm-0.15mm. The width of the stent rod refers to the size of the stent rod in the circumferential direction of the medical stent, and the thickness of the stent rod refers to the size of the stent rod in the radial direction of the medical stent. The medical stent before polishing is observed using an optical microscope. The morphology of the outer surface of the medical stent is as follows: Figure 1 As shown, it has obvious scratches and defects, and the surface is uneven and matte.
[0037] In the polishing liquid of Example 1, the content of solution A is 10%, the content of solution B is 40%, and the content of n-butanol is 50%, calculated by mass percentage. In solution A, the content of concentrated sulfuric acid is 85%, and the content of ethylene glycol is 15%, calculated by mass percentage. In solution B, the content of citric acid is 75%, and the content of glycerol is 25%, calculated by mass percentage. During polishing, a titanium rod is used as a cathode, and the minimum distance between the cathode and the outer peripheral surface of the medical stent as an anode is 5 mm; the temperature of the polishing liquid is set to 10°C, and the current flowing through the cathode, the anode, and the polishing liquid is set to 2A; the polishing time is 55s.
[0038] After polishing, the medical stent was placed in a 75% by mass ethanol solution for cleaning for 3 minutes and dried. The medical stent after polishing was observed using an optical microscope. The morphology is as follows: Figure 2 As shown. Figure 2 and Figure 1 It can be seen that the outer surface of the medical stent after polishing is smooth and has a mirror-like gloss, and the scratches and defects on the surface are basically gone.
[0039] The medical stent used in Example 2 is a nickel-titanium stent, and the medical stent is a hollow cylindrical structure when expanded. The width of the stent rod in the medical stent is 0.05mm-0.25mm, and the thickness of the stent rod is 0.04mm-0.15mm. The width of the stent rod refers to the size of the stent rod in the circumferential direction of the medical stent, and the thickness of the stent rod refers to the size of the stent rod in the radial direction of the medical stent. The medical stent before polishing is observed using an optical microscope. The morphology of the outer surface of the medical stent is as follows: Figure 3 As shown, it has obvious scratches and defects, and the surface is uneven and matte.
[0040] In the polishing liquid of Example 2, the content of solution A is 8%, the content of solution B is 35%, and the content of n-butanol is 57%, calculated by mass percentage. In solution A, the content of concentrated sulfuric acid is 90%, and the content of ethylene glycol is 10%, calculated by mass percentage. In solution B, the content of citric acid is 70%, and the content of glycerol is 30%, calculated by mass percentage. During polishing, a titanium rod is used as a cathode, and the minimum distance between the cathode and the outer peripheral surface of the medical stent as an anode is 30 mm; the temperature of the polishing liquid is set to 30°C; the current flowing through the cathode, the anode, and the polishing liquid is set to 1A; and the polishing time is 15s.
[0041] After polishing, the medical stent was placed in a 75% by mass ethanol solution for cleaning for 3 minutes and dried. The medical stent after polishing was observed using an optical microscope. The morphology is as follows: Figure 4 As shown. Figure 2 and Figure 1 It can be seen that the outer surface of the medical stent after polishing is smooth and has a mirror-like gloss, and the scratches and defects on the surface are basically gone.
[0042] The medical stent used in Example 3 is a nickel-titanium stent, and the medical stent is a hollow cylindrical structure when expanded. The width of the stent rod in the medical stent is 0.05mm-0.25mm, and the thickness of the stent rod is 0.04mm-0.15mm. The width of the stent rod refers to the size of the stent rod in the circumferential direction of the medical stent, and the thickness of the stent rod refers to the size of the stent rod in the radial direction of the medical stent. The medical stent before polishing was observed under an optical microscope, and obvious scratches and defects can be seen on the outer surface of the medical stent, and the surface is uneven and matte.
[0043] In the polishing liquid of Example 3, the content of solution A is 3%, the content of solution B is 30%, and the content of n-butanol is 67%, calculated by mass percentage. In solution A, the content of concentrated sulfuric acid is 80%, and the content of ethylene glycol is 20%, calculated by mass percentage. In solution B, the content of citric acid is 80%, and the content of glycerol is 20%, calculated by mass percentage. During polishing, a titanium rod is used as a cathode, and the minimum distance between the cathode and the outer peripheral surface of the medical stent as an anode is 15 mm; the temperature of the polishing liquid is set to 25°C, and the current flowing through the cathode, the anode, and the polishing liquid is 0.5 A; the polishing time is 60 s.
[0044] After polishing, the medical stent was placed in a 75% by mass ethanol solution for cleaning for 3 minutes and dried. The medical stent after polishing was observed under an optical microscope and found that the outer surface of the medical stent was smooth and had a mirror-like gloss, and the scratches and defects on the surface were basically gone.
[0045] Although the present invention is disclosed as above, it is not limited thereto. Those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A polishing liquid, characterized in that: It includes the following components in mass percentage: Concentrated sulfuric acid 2%-9% Ethylene glycol 0.25%-2% Citric acid 21%-32% Corrosion inhibitor 6%-12% n-Butanol 50%-67.5%.
2. The polishing liquid according to claim 1, characterized in that The corrosion inhibitor includes glycerol.
3. The polishing liquid according to claim 1, characterized in that The polishing liquid is prepared by first preparing solution A and solution B, and then uniformly mixing solution A, solution B and n-butanol according to a proportion. Wherein, the solution A includes concentrated sulfuric acid and ethylene glycol, and in the solution A, the mass percentage of concentrated sulfuric acid is 80%-90%, and the mass percentage of ethylene glycol is 10%-20%; the solution B includes citric acid and the corrosion inhibitor, and in the solution B, the mass percentage of citric acid is 70%-80%, and the mass percentage of the corrosion inhibitor is 20%-30%; in the polishing liquid, the mass percentage of the solution A is 2.5%-10%, and the mass percentage of the solution B is 30%-40%.
4. A method for preparing a polishing liquid, for preparing the polishing liquid as claimed in claim 1, characterized in that: The steps include: Prepare solution A; Prepare solution B; Mix the solution A, the solution B and n-butanol uniformly according to proportion; Wherein, the solution A includes concentrated sulfuric acid and ethylene glycol, and in the solution A, the mass percentage of concentrated sulfuric acid is 80%-90%, and the mass percentage of ethylene glycol is 10%-20%; the solution B includes citric acid and the corrosion inhibitor, and in the solution B, the mass percentage of citric acid is 70%-80%, and the mass percentage of the corrosion inhibitor is 20%-30%; in the polishing liquid, the mass percentage of the solution A is 2.5%-10%, and the mass percentage of the solution B is 30%-40%.
5. The method for preparing the polishing liquid according to claim 4, characterized in that: The corrosion inhibitor includes glycerol.
6. A polishing method, characterized in that: include: A polishing liquid as described in any one of claims 1 to 3; Placing a cathode made of an inert metal at least partially in the polishing liquid, and using the object to be polished as an anode and immersed in the polishing liquid; The polishing liquid is kept at a preset temperature, and power is supplied to a circuit formed by the cathode, the anode, and the polishing liquid to perform a polishing operation.
7. The polishing method according to claim 6, characterized in that: The cathode is arranged in parallel with the anode.
8. The polishing method according to claim 7, characterized in that: The distance between the cathode and the anode is 5 mm to 30 mm.
9. The polishing method according to claim 6, characterized in that: The preset temperature is 10° C.-30° C., the current in the circuit formed by the cathode, the anode and the polishing liquid is 0.5A-2A, and the polishing time is 10s-60s.
10. The polishing method according to claim 6, characterized in that: The target object includes a medical stent, and the medical stent is made of metal material.