High-stiffness temperature-resistant hollow paper tube, preparation method thereof and application of high-stiffness temperature-resistant hollow paper tube in cigarette heating
By mixing basalt fibers with wood pulp and applying boric acid solution, the problem of insufficient stiffness and temperature resistance of hollow paper tubes is solved, and a hollow paper tube with high stiffness and high temperature resistance is achieved, which is suitable for heating cigarettes. Preparation improves the appearance and sensory quality of the tobacco branches.
Patent Information
- Application Number
- CN202411348837.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-29
AI Technical Summary
The existing hollow paper tubes have problems such as insufficient stiffness, poor temperature resistance, easy deformation and baking breath in heated cigarettes, which affect the appearance and sensory quality of the cigarette sticks.
By mixing basalt fibers with wood pulp and applying boric acid solution to the surface of the paper, combining diatomaceous earth and additives, a hollow paper tube with high stiffness and high temperature resistance is formed, and a hollow paper tube is made of spiral molding.
It significantly improves the stiffness and temperature resistance of the hollow paper tube, reduces deformation and baking atmosphere, improves the appearance and sensory quality of the cigarette stick, and is suitable for the preparation of heated cigarettes.
Abstract
Description
Technical Field
[0001] The invention relates to a hollow paper tube, in particular to a high-stiffness and heat-resistant hollow paper tube, and also to a preparation method thereof and application thereof as a hollow cooling section of a heated cigarette filter, belonging to the technical field of novel tobacco. Background Art
[0002] As people pay more attention to safety and health, the sales of heated cigarettes in foreign markets are growing. Hollow paper tubes are gradually replacing hollow acetate thin-walled hollow tubes due to their low cost and easy aroma loading. However, compared with the latter, hollow paper tubes have certain defects in process maturity and sensory experience. For example, the hollow paper tube is not stiff enough, and when it is compounded with the acetate filter segment, it is easy to produce irreversible deformation problems due to certain extrusion, which leads to poor circumference of the filter rod and wrinkles during the cigarette rolling process; in addition, in the surrounding heated cigarettes, the heating temperature is about 250 degrees Celsius, and the cellulose in the paper is prone to carbonization. After heating and smoking, the hollow paper tube is not only prone to collapse, affecting the appearance quality, but also the paper baking smell of the paper tube will bring a bad smoking experience, affecting the sensory quality of heated cigarettes. Summary of the invention
[0003] In view of the technical problems existing in the existing hollow paper tubes, the first object of the present invention is to provide a hollow paper tube with high stiffness and high temperature resistance.
[0004] The second object of the present invention is to provide a method for preparing a high-stiffness and heat-resistant hollow paper tube, which hardly changes the existing processing technology of the hollow paper tube, is simple to operate, has low cost, and can be industrially produced.
[0005] The third object of the present invention is to provide an application of a high-stiffness and heat-resistant hollow paper tube, which can replace the existing hollow paper tube for the preparation of heated cigarettes. It can overcome the problems that the hollow paper tube is easy to deform and wrinkle during the composite process of the hollow paper tube and the acetate filter rod or the cigarette stick rolling process, and solve the technical defects of the existing hollow paper tube, such as poor heat resistance, easy to bring the smell of paper baking during the smoking process, poor sensory quality, and easy deformation of the paper tube after heating and smoking.
[0006] In order to achieve the above technical objectives, the present invention provides a method for preparing a high-stiffness and heat-resistant hollow paper tube, which comprises mixing and beating basalt fiber and wood pulp to obtain a mixed fiber slurry, adding diatomaceous earth, a wetting agent and a retention agent to the mixed fiber slurry, stirring the mixed fiber slurry evenly, and then performing a scooping forming process, coating the forming paper with a boric acid solution, drying and cutting the paper to obtain a base paper, and spirally forming the base paper into a hollow paper tube.
[0007] The key to the technical solution of the present invention is that basalt fiber is introduced into the base paper of the hollow paper tube, which gives the paper a higher stiffness while ensuring the flexibility of the paper, effectively solving the problem of irreversible deformation of the hollow paper tube due to extrusion when compounded with the acetate filter segment and wrinkles easily generated during the cigarette rolling process, and greatly reducing the loss rate of the hollow paper tube during the compounding process; however, the compatibility between basalt fiber and wood pulp is poor, and the bonding strength is low. The present invention further coats boric acid on the surface of the paper, which can not only promote the bonding strength between basalt fiber and wood pulp fiber, but also improve the temperature resistance of the hollow paper tube under 200-300°C, which not only reduces the baking smell of the paper and improves the sensory quality, but also avoids the influence of the deformation of the paper tube after heating and smoking on the appearance quality.
[0008] As a preferred solution, the length of the basalt fiber is 1 to 8 mm, and the diameter is 7 to 15 μm. Choosing basalt fibers of appropriate sizes can be better incorporated into wood pulp and improve their dispersibility in wood pulp.
[0009] As a preferred solution, the basalt fiber is added in a ratio of 0.3 to 0.7 times the mass of the wood pulp. Within the preferred range, as the basalt fiber addition ratio increases, the stiffness of the base paper increases significantly, but if the basalt fiber ratio is too high, the flexibility of the base paper will be affected.
[0010] As a preferred solution, the wood pulp is composed of coniferous wood pulp and broadleaf wood pulp in a mass ratio of 4:6 to 5:5. Mixing the two in a preferred ratio can improve the flexibility of the base paper.
[0011] As a preferred solution, the beating degree of the mixed beating is 40°SR~60°SR.
[0012] As a preferred solution, the amount of diatomaceous earth added is 1 to 10% of the total mass of basalt fiber and wood pulp;
[0013] As a preferred solution, the amount of the wetting agent added is 2-6% of the total mass of the basalt fiber and wood pulp;
[0014] As a preferred solution, the amount of the retention agent added is 0.05-2% of the total mass of the basalt fiber and wood pulp.
[0015] As a preferred solution, the specific surface area of the diatomaceous earth is 40 to 65 m 2 / g, density is 1.9~2.3g / cm 3 , the particle size is 300-600 mesh. Diatomaceous earth, wetting agent and retention aid are commonly used additives in the papermaking process.
[0016] As a preferred solution, the wet strength agent includes polyamide epichlorohydrin resin.
[0017] As a preferred solution, the retention aid includes cationic polyacrylamide.
[0018] As a preferred solution, the concentration of boric acid in the boric acid solution is 1-10%, and the solvent is composed of ethanol and water in a volume ratio of 40-80%:20-60%. Boric acid coated on the molding paper can strengthen the bonding force between basalt fiber and wood pulp fiber through physical and chemical bonding. At the same time, boric acid has good high temperature stability, forms a protective layer on the wood pulp fiber, and reduces the impact of high temperature on the wood pulp fiber.
[0019] As a preferred solution, the coating amount of the boric acid solution on the molding paper is 1 to 10 g / m 2 Measurement.
[0020] As a preferred solution, the drying is carried out using two groups of drying cylinders, wherein the pressure of the rollers in the drying cylinders of the first group of drying cylinders is 80-100 kg / cm, the drying cylinder temperature is 110-130°C, and the drying time is 10-20 min; the pressure of the rollers in the drying cylinders of the second group of drying cylinders is 40-60 kg / cm, the drying cylinder temperature is 80-100°C, and the drying time is 20-30 min.
[0021] As a preferred solution, the hollow paper tube comprises an inner and outer layer; the gram weight of the inner layer of paper is 100-200 g / m 2 , thickness is 0.2~0.3mm, outer paper weight is 40~100g / m 2 , thickness is 0.1~0.2mm.
[0022] The present invention also provides a high stiffness and heat-resistant hollow paper tube, which is obtained by the preparation method. Compared with the conventional hollow paper tube, the hollow paper tube prepared by the present invention has high stiffness and high temperature resistance.
[0023] The present invention also provides an application of a high stiffness and heat-resistant hollow paper tube, which is used as a hollow cooling section of a filter tip for preparing heated cigarettes. The hollow paper tube of the present invention replaces the existing hollow paper tube to prepare heated cigarettes. During the compounding process with the acetate filter tip section or the cigarette rolling process, it exhibits high stiffness and will not undergo irreversible deformation, thereby ensuring the appearance quality of the cigarette. At the same time, the hollow paper tube can withstand a high temperature environment of 200 to 300°C, which not only reduces the baking smell of the paper and improves the sensory quality, but also avoids the influence of the deformation of the paper tube after heating and smoking on the appearance quality.
[0024] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:
[0025] Compared with the existing hollow paper tubes, the hollow paper tubes of the present invention have higher stiffness. During the process of compounding with the acetate filter segment or rolling the cigarette, no irreversible deformation or wrinkles will occur, which greatly reduces the loss rate of the hollow paper tubes during the compounding process and ensures the appearance quality of the cigarette.
[0026] Compared with the existing hollow paper tubes, the hollow paper tubes of the present invention have a temperature resistance under the condition of 200-300°C, which not only reduces the baking smell of paper and improves the sensory quality, but also avoids the influence of the appearance quality caused by the deformation of the paper tube after heating and suction.
[0027] The hollow paper tube preparation method of the present invention is simple to operate, low in cost, and can be industrially produced. DETAILED DESCRIPTION
[0028] The following specific examples are intended to further illustrate the present invention in detail, rather than to limit the scope of protection of the claims.
[0029] Unless otherwise specified in the following examples, the chemical reagents used are all commercial reagents.
[0030] In the following examples, basalt fibers are commercial products with a length of 1 to 8 mm and a diameter of 7 to 15 μm.
[0031] Example 1
[0032] The composite pulp is prepared by mixing and beating basalt fiber and wood pulp in a mass ratio of 1:2, wherein the mass ratio of coniferous wood pulp and broadleaf wood pulp is 5:5, and diatomaceous earth (5% of the mass of wood pulp), wet strength agent polyamide epichlorohydrin resin (3% of the mass of wood pulp), and retention agent cationic polyacrylamide (1% of the mass of wood pulp) are added in sequence after being mixed and beaten (beating degree 50°SR) to obtain a composite pulp; after forming by fourdrinier papermaking, a layer of boric acid solution is coated on the surface of the paper, the mass concentration of the boric acid solution is 5%, and the solvent is a 70% ethanol aqueous solution (coating amount is 2g / m 2 After drying (using two groups of drying cylinders for drying, wherein the pressure of the rollers in the first group of drying cylinders is 100kg / cm, the drying cylinder temperature is 130°C, and the drying time is 20min; the pressure of the rollers in the second group of drying cylinders is 60kg / cm, the drying cylinder temperature is 100°C, and the drying time is 30min) and slitting, a hollow paper tube base paper is obtained, and the paper tube paper is spirally formed into a hollow paper tube (the paper tube paper includes an inner paper tube paper and an outer paper tube paper, and the gram weight of the inner paper tube paper is 180g / m 2 , thickness is 0.3mm, outer paper tube paper weight is 40g / m 2 , thickness is 0.1mm).
[0033] The prepared hollow paper tubes were tested in the following aspects:
[0034] 1. Test the hardness of the hollow paper tube according to the method of GB / T22838 "Determination of physical properties of cigarettes and filter rods".
[0035] 2. Take the hollow paper tube base paper sample and put it into an oven set at 250 degrees Celsius, heat and bake for 5 minutes, and measure the yellowing value of the paper.
[0036] Yellowing value (%) = (R0-R) / R0×100%, where R0 represents the initial whiteness of the paper tube base paper, and R represents the whiteness of the paper tube after baking. The lower the yellowing value, the better the temperature resistance of the paper.
[0037] Example 2
[0038] The composite pulp is prepared by mixing and beating basalt fiber and wood pulp in a mass ratio of 3:5, wherein the mass ratio of coniferous wood pulp and broadleaf wood pulp is 4:6, and diatomaceous earth (2% of the mass of wood pulp), wet strength agent polyamide epichlorohydrin resin (4% of the mass of wood pulp), and retention agent cationic polyacrylamide (1.5% of the mass of wood pulp) are added in sequence after being mixed and beaten (beating degree 60°SR) to obtain a composite pulp; after forming by fourdrinier papermaking, a layer of boric acid solution is coated on the surface of the paper, the mass concentration of the boric acid solution is 10%, and the solvent is a 70% ethanol aqueous solution (coating amount is 5g / m 2 After drying (using two groups of drying cylinders for drying, wherein the pressure of the rollers in the first group of drying cylinders is 100kg / cm, the drying cylinder temperature is 130°C, and the drying time is 20min; the pressure of the rollers in the second group of drying cylinders is 60kg / cm, the drying cylinder temperature is 100°C, and the drying time is 30min) and slitting, a hollow paper tube base paper is obtained, and the paper tube paper is spirally formed into a hollow paper tube (the paper tube paper includes an inner paper tube paper and an outer paper tube paper, and the gram weight of the inner paper tube paper is 180g / m 2 , thickness is 0.3mm, outer paper tube paper weight is 40g / m 2 , thickness is 0.1mm).
[0039] Example 3
[0040] The composite pulp is prepared by mixing and beating basalt fiber and wood pulp in a mass ratio of 2:5, wherein the mass ratio of coniferous wood pulp and broadleaf wood pulp is 5:5, and diatomaceous earth (10% of the mass of wood pulp), wet strength agent polyamide epichlorohydrin resin (4% of the mass of wood pulp), and retention agent cationic polyacrylamide (0.5% of the mass of wood pulp) are added in sequence after the pulp is mixed and beaten (beating degree 55°SR) to obtain a composite pulp; after forming by fourdrinier papermaking, a layer of boric acid solution is coated on the surface of the paper, the mass concentration of the boric acid solution is 8%, and the solvent is a 70% ethanol aqueous solution (coating amount is 7g / m 2After drying (using two groups of drying cylinders for drying, wherein the pressure of the rollers in the first group of drying cylinders is 100kg / cm, the drying cylinder temperature is 130°C, and the drying time is 20min; the pressure of the rollers in the second group of drying cylinders is 60kg / cm, the drying cylinder temperature is 100°C, and the drying time is 30min) and slitting, a hollow paper tube base paper is obtained, and the paper tube paper is spirally formed into a hollow paper tube (the paper tube paper includes an inner paper tube paper and an outer paper tube paper, and the gram weight of the inner paper tube paper is 180g / m 2 , thickness is 0.3mm, outer paper tube paper weight is 40g / m 2 , thickness is 0.1mm).
[0041] Comparative Example 1
[0042] The difference from Example 1 is that the hollow paper tube is prepared by a conventional method without adding basalt fiber and boric acid coating.
[0043] Comparative Example 2
[0044] The difference from Example 1 is that the prepared paper tube only has basalt fiber added, and is not coated with boric acid.
[0045] Comparative Example 3
[0046] The difference from Example 1 is that the coating amount of the boric acid solution is 40 g / m 2 .
[0047] Table 1 Comparison of stiffness of paper tubes prepared in Example and Comparative Example
[0048] Hardness test value / % Example 1 93 Example 2 95 Example 3 90 Comparative Example 1 84 Comparative Example 2 92 Comparative Example 3 62
[0049] Table 2 Comparison of yellowing values of paper tubes prepared in Examples and Comparative Examples
[0050] Yellowing value determination / % Example 1 30 Example 2 20 Example 3 25 Comparative Example 1 55
Claims
1. A method for preparing a high stiffness heat-resistant hollow paper tube, characterized in that: The basalt fiber and wood pulp are mixed and beaten to obtain a mixed fiber slurry, diatomaceous earth, a wetting agent and a retention aid are added to the mixed fiber slurry, stirred evenly, and then scooped to form a net, a boric acid solution is coated on the forming paper, and the paper is dried and cut to obtain base paper, and the base paper is spirally formed and rolled into a hollow paper tube.
2. The method for preparing a high stiffness heat-resistant hollow paper tube according to claim 1, characterized in that: The basalt fiber has a length of 1 to 8 mm and a diameter of 7 to 15 μm.
3. The method for preparing a high stiffness heat-resistant hollow paper tube according to claim 1 or 2, characterized in that: The mixing ratio of the basalt fiber is 0.3 to 0.7 times the mass of the wood pulp.
4. The method for preparing a high stiffness and heat-resistant hollow paper tube according to claim 3, characterized in that: The wood pulp is composed of coniferous wood pulp and broadleaf wood pulp in a mass ratio of 4:6 to 5:
5.
5. The method for preparing a high stiffness and heat-resistant hollow paper tube according to claim 1, characterized in that: The beating degree of the mixed beating is 40°SR~60°SR.
6. The method for preparing a high stiffness and heat-resistant hollow paper tube according to claim 1, characterized in that: The amount of diatomaceous earth added is 1 to 10% of the total mass of basalt fiber and wood pulp; The amount of the wetting agent added is 2-6% of the total mass of the basalt fiber and wood pulp; The addition amount of the retention agent is 0.05-2% of the total mass of the basalt fiber and the wood pulp.
7. The method for preparing a high stiffness and heat-resistant hollow paper tube according to claim 6, characterized in that: The specific surface area of the diatomaceous earth is 40 to 65 m 2 / g, density is 1.9~2.3g / cm 3 , particle size is 300-600 mesh; The wet strength agent includes polyamide epichlorohydrin resin; The retention aid includes cationic polyacrylamide.
8. The method for preparing a high stiffness and heat-resistant hollow paper tube according to claim 1, characterized in that: The concentration of boric acid in the boric acid solution is 1-10%, and the solvent is composed of ethanol and water in a volume ratio of 40-80%:20-60%.
9. The method for preparing a high stiffness heat-resistant hollow paper tube according to claim 1 or 8, characterized in that: The coating amount of the boric acid solution on the forming paper is 1 to 10 g / m 2 Measurement.
10. The method for preparing a high stiffness and heat-resistant hollow paper tube according to claim 1, characterized in that: The drying is carried out using two groups of drying cylinders, wherein the pressure of the rollers in the drying cylinders of the first group of drying cylinders is 80-100 kg / cm, the drying cylinder temperature is 110-130°C, and the drying time is 10-20 min; the pressure of the rollers in the drying cylinders of the second group of drying cylinders is 40-60 kg / cm, the drying cylinder temperature is 80-100°C, and the drying time is 20-30 min.
11. The method for preparing a high stiffness and heat-resistant hollow paper tube according to claim 1, characterized in that: The hollow paper tube includes two layers, inner and outer; the gram weight of the inner layer of paper is 100-200g / m 2 , thickness is 0.2~0.3mm, outer paper weight is 40~100g / m 2 , thickness is 0.1~0.2mm.
12. A high stiffness and heat-resistant hollow paper tube, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 11.
13. The use of a high stiffness and heat-resistant hollow paper tube according to claim 12, characterized in that: The hollow cooling section as a filter tip is used in the preparation of heated cigarettes.
Citation Information
Patent Citations
Papermaking method and sized paper and coated paper obtained by papermaking method
CN104389238A
Heat-not-burn cigarette cooling unit containing phase change cooling material and heat-not-burn cigarette
CN117179372A
High-whiteness titanium-free tipping base paper product and preparation process thereof
CN118407282A
Preparation method of hollow cooling tobacco aroma paper tube for heating cigarettes
CN118668529A
Manufacturing method of plastic-substituted packaging paper with foaming buffer layer
CN118686015A
Cited By
Low-interception high-aroma-loading hollow tube for heating cigarettes and application
CN119423361A
Low-interception hollow tube for heating cigarettes and application of low-interception hollow tube
CN119423363A