Environment-friendly PP plastic floor and preparation method thereof

By using polypropylene and other environmentally friendly raw materials, combined with firing and PU treatment processes, environmentally friendly PP plastic floors with excellent performance are prepared, which solves the environmental protection and dimensional stability of PVC plastic floors and achieves high quality and safe environmental protection Plastic flooring products.

CN119041652APending Publication Date: 2024-11-29NANJING MGM NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411120790.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing PVC plastic floors have problems such as poor environmental protection, poor dimensional stability, inability to biodegrade and produce toxic gases, making it difficult to prepare environmentally friendly plastic floors with good performance.

Method used

Polypropylene is used as the substrate, combined with maleic anhydride grafted polypropylene, calcium carbonate, paratholite, ammonium polyphosphate-loaded sepiolite fiber and other raw materials, through firing, PU treatment and secondary heating and tempering, Eco-friendly PP plastic floors with excellent mechanical properties, sound insulation, flame retardant and thermal insulation properties were prepared.

Benefits of technology

It improves the environmental protection performance, mechanical performance and use safety of PP plastic flooring, ensuring the green and environmental protection of the products and high-quality production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004995020280000121
    Figure BDA0004995020280000121
  • Figure BDA0004995020280000131
    Figure BDA0004995020280000131
Patent Text Reader

Abstract

The invention relates to the field of plastic floors, and particularly discloses an environment-friendly PP plastic floor and a preparation method thereof. The environment-friendly PP plastic floor is prepared by the following steps: sequentially paving a film on a PP middle backing material, a PP printing surface material and a PP transparent material, firing into a semi-finished product, curing, carrying out surface PU (Poly Urethane) treatment, carrying out secondary heating and tempering, and molding, the PP middle base material is prepared from the following raw materials in parts by mass: 25 to 35 parts of polypropylene, 10 to 15 parts of maleic anhydride grafted polypropylene, 90 to 120 parts of calcium carbonate, 20 to 40 parts of palygorskite, 10 to 30 parts of ammonium polyphosphate loaded sepiolite fiber, 1 to 4 parts of antistatic agent, 2 to 4 parts of antioxidant, 2 to 4 parts of stabilizer, 1 to 3 parts of coupling agent and 0.1 to 1 part of toner. The environment-friendly PP plastic floor has the advantages of being environmentally friendly, excellent in flame retardant property and good in sound insulation effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of plastic flooring, and more specifically, to an environmentally friendly PP plastic flooring and a preparation method thereof. Background Art

[0002] The current trend of plastic flooring product development is to use polymer compound materials as the base material to replace natural wood and reduce damage to the natural environment. Since PVC has good flame retardancy and self-extinguishing properties, and its performance can be changed by changing the amount of plasticizers and fillers added, PVC plastic flooring is the most widely used.

[0003] However, PVC plastic flooring has the disadvantage of poor environmental performance. It produces toxic hydrogen chloride and carbon monoxide gas when it is cracked, and dioxin and other toxic gases after combustion. It usually contains phthalic acid plasticizers, which can cause reproductive toxicity when precipitated. In addition, PVC flooring has poor dimensional stability, and unclassified recycled flooring cannot be biodegraded after being abandoned and buried, causing white pollution. PP material is odorless and non-toxic, does not volatilize toxic gases, has high chemical stability, and has good environmental performance.

[0004] With respect to the above-mentioned related technologies, how to use PP material as a base material to produce an environmentally friendly plastic floor with good performance is a problem that needs to be solved urgently. Summary of the invention

[0005] In order to obtain a green and environmentally friendly PP plastic floor, the present application provides an environmentally friendly PP plastic floor and a preparation method thereof.

[0006] In the first aspect, the present application provides an environmentally friendly PP plastic floor, which adopts the following technical solution:

[0007] An environmentally friendly PP plastic floor, which is prepared by sequentially laying a film of a PP mid-base material, a PP printed surface, and a PP transparent material, firing the semi-finished product, and then undergoing curing, surface PU treatment, secondary heating and tempering, and molding;

[0008] The PP base material includes the following raw materials in parts by weight:

[0009] 25-35 parts of polypropylene, 10-15 parts of maleic anhydride grafted polypropylene, 90-120 parts of calcium carbonate, 20-40 parts of palygorskite, 10-30 parts of ammonium polyphosphate loaded sepiolite fiber, 1-4 parts of antistatic agent, 2-4 parts of antioxidant, 2-4 parts of stabilizer, 1-3 parts of coupling agent, and 0.1-1 parts of color powder.

[0010] By adopting the above technical scheme, polypropylene is used as the base material, and its environmental performance is better than PVC; calcium carbonate is a commonly used reinforcing filler for plastic floors, which helps to ensure that PP plastic floors have better mechanical properties; palygorskite has a rich microporous structure, good sound insulation effect, and has heat insulation and thermal insulation properties, has a good flame retardant effect, and is low in price and natural and non-toxic; sepiolite fiber is a natural mineral fiber with corrosion resistance, friction resistance, penetration resistance, sound insulation, and heat resistance; ammonium polyphosphate is a halogen-free environmentally friendly flame retardant with excellent flame retardant properties. When ammonium polyphosphate is loaded on sepiolite fiber, sepiolite fiber The high porosity and good adsorption properties of PP plastic flooring can help improve the flame retardant properties of PP plastic flooring; maleic anhydride grafted polypropylene can improve the affinity of polypropylene matrix with calcium carbonate, palygorskite, and ammonium polyphosphate loaded sepiolite fibers, and improve the dispersibility of calcium carbonate, palygorskite, and ammonium polyphosphate loaded sepiolite fibers; coupling agents can help further promote the uniform dispersion of calcium carbonate, palygorskite, and ammonium polyphosphate loaded sepiolite fibers; antistatic agents can help reduce static adhesion of PP plastic flooring and improve processing performance and use performance; antioxidants and stabilizers can help improve the service life and application stability of PP plastic flooring.

[0011] The present invention uses polypropylene as a base material, maleic anhydride grafted polypropylene as a compatibilizer, calcium carbonate as a reinforcing filler, and then adds palygorskite and ammonium polyphosphate loaded sepiolite fibers. The flaky palygorskite and fibrous ammonium polyphosphate loaded sepiolite fibers are filled in the gaps of calcium carbonate, further enhancing the mechanical properties of the PP plastic floor. The combination of the two makes the PP plastic floor have excellent sound insulation performance, which helps to reduce the noise between floors, and makes the PP plastic floor have excellent flame retardant and heat insulation performance, thereby improving the safety of the PP plastic floor.

[0012] Preferably, the ammonium polyphosphate loaded sepiolite fiber is obtained by acid-activating the sepiolite fiber and then adsorbing the ammonium polyphosphate.

[0013] Preferably, the preparation method of the ammonium polyphosphate-loaded sepiolite fiber specifically comprises:

[0014] The sepiolite fiber is acid-activated by using an acid solution, and then washed to neutrality to obtain the activated sepiolite fiber;

[0015] The activated sepiolite fiber is immersed in water, water-soluble ammonium polyphosphate is added thereto at 40-80° C., stirred for 6-12 hours, allowed to stand, filtered, and dried to obtain the ammonium polyphosphate-loaded sepiolite fiber.

[0016] By adopting the above technical scheme, the sepiolite fiber has a high specific surface area, high porosity and strong adsorption performance; acid washing helps to remove soluble impurities, and helps to increase the specific surface area, pore volume and porosity, thereby promoting the improvement of the adsorption performance of the sepiolite fiber; ammonium polyphosphate is loaded onto the sepiolite fiber through impregnation treatment, and when burned, the ammonium polyphosphate can react with the carbon element in the polypropylene matrix to form a stable carbon layer, which plays a role in heat insulation and oxygen isolation; the fiber network formed by the sepiolite fiber can provide an inorganic network skeleton when carbonizing, which helps to improve the flame retardant performance.

[0017] Preferably, the mass of the water-soluble ammonium polyphosphate is 5-30% of the mass of the sepiolite fiber.

[0018] Preferably, the water-soluble ammonium polyphosphate is ammonium tripolyphosphate.

[0019] Preferably, the palygorskite is a modified palygorskite that is activated by acid and then surface treated with a surfactant.

[0020] Preferably, the preparation method of the modified palygorskite comprises:

[0021] The palygorskite is subjected to acid activation treatment with an acid solution, and then washed to neutrality to obtain activated palygorskite; the activated palygorskite is immersed in a surfactant aqueous solution, stirred at 40-80° C. for 2-6 hours, filtered, and dried to obtain modified palygorskite.

[0022] By adopting the above technical solution, the specific surface area and porosity of palygorskite are further improved, and the dispersion performance of palygorskite is promoted and the possibility of palygorskite agglomeration is reduced through surfactant treatment.

[0023] Preferably, the coupling agent is an aluminate coupling agent.

[0024] Preferably, the antistatic agent is an alkyl sulfonic acid.

[0025] In the second aspect, the present application provides a method for preparing an environmentally friendly PP plastic floor, using the following technical solution:

[0026] A method for preparing an environmentally friendly PP plastic floor comprises the following steps:

[0027] According to the proportion, polypropylene, maleic anhydride grafted polypropylene, calcium carbonate, palygorskite, ammonium polyphosphate loaded sepiolite fiber, antistatic agent, antioxidant, stabilizer, coupling agent and color powder are mixed and stirred evenly, and then the mixture is subjected to banburying, calendering, cooling, cutting and curing to obtain PP mid-base material;

[0028] The PP mid-base material, PP printed surface material and PP transparent material are sequentially molded, pushed and molded, fired by a hot press to obtain a semi-finished product, and cured until the temperature of the semi-finished product tends to be stable;

[0029] The surface of the coating film is treated with PU by a UV machine, and the physical properties are treated by secondary heating and tempering by a tempering machine. After curing and molding, an environmentally friendly PP plastic floor is obtained.

[0030] By adopting the above technical solution, the preparation method is simple and scientific, the production efficiency is high and the product quality is good.

[0031] In summary, this application has the following beneficial effects:

[0032] 1. Since the present application uses polypropylene as the base material, maleic anhydride grafted polypropylene as the compatibilizer, calcium carbonate as the reinforcing filler, and then adds palygorskite and ammonium polyphosphate loaded sepiolite fibers, the flaky palygorskite and fibrous ammonium polyphosphate loaded sepiolite fibers are filled in the gaps of calcium carbonate, which further enhances the mechanical properties of the PP plastic floor. The combination of the two makes the PP plastic floor have excellent sound insulation performance, which helps to reduce the noise between floors, and makes the PP plastic floor have excellent flame retardant and heat insulation properties, thereby improving the safety of the PP plastic floor.

[0033] 2. The raw materials used in this application are green, environmentally friendly, safe and pollution-free, and the preparation method is simple and scientific, with high production efficiency and good product quality. DETAILED DESCRIPTION

[0034] To further help understand the technical solution of the present invention, the technical solution of the present invention is described in more detail below by providing several specific implementation examples. All of these described embodiments are only partial embodiments of the present invention, not all of them.

[0035] The following specific embodiments may be combined with each other, and the same or similar concepts or processes may not be described in detail in some embodiments; and the reaction devices, monomer compounds, etc. involved in the following embodiments are all commercially available.

[0036] The following specific embodiments may be combined with each other, and the same or similar concepts or processes therein may not be described in detail in some embodiments.

[0037] The following examples are further explanations of the present invention, but the present invention is not limited thereto. Unless otherwise specified in the examples, the percentages are all by mass.

[0038] Preparation Example

[0039] Preparation Example 1

[0040] This preparation example provides an ammonium polyphosphate-loaded sepiolite fiber, and the preparation method is as follows:

[0041] The sepiolite fiber is immersed in a 10 wt % hydrochloric acid solution, stirred at 50° C. for 2 h, filtered, and washed until neutral to obtain activated sepiolite fiber;

[0042] The activated sepiolite fiber was immersed in water, and 5% of the mass of the sepiolite fiber was added thereto at 75°C, stirred for 6 hours, allowed to stand for 24 hours, filtered, and dried at 80°C to obtain the ammonium polyphosphate-loaded sepiolite fiber.

[0043] Preparation Example 2

[0044] The only difference between this preparation example and preparation example 1 is that the ammonium polyphosphate-loaded sepiolite fiber is prepared by the following method:

[0045] The sepiolite fiber is immersed in a 10 wt % hydrochloric acid solution, stirred at room temperature for 3 hours, filtered, and washed to neutrality to obtain activated sepiolite fiber;

[0046] The activated sepiolite fiber was immersed in water, and 20% of the mass of the sepiolite fiber was added thereto at 60°C, stirred for 8 hours, allowed to stand for 24 hours, filtered, and dried at 80°C to obtain the ammonium polyphosphate loaded sepiolite fiber.

[0047] Preparation Example 3

[0048] The only difference between this preparation example and preparation example 1 is that the ammonium polyphosphate-loaded sepiolite fiber is prepared by the following method:

[0049] The sepiolite fiber is immersed in a 10 wt % hydrochloric acid solution, stirred at 40° C. for 2 h, filtered, and washed until neutral to obtain activated sepiolite fiber;

[0050] The activated sepiolite fiber was immersed in water, and 30% of the mass of the sepiolite fiber was added thereto at 75°C, stirred for 8 hours, allowed to stand for 24 hours, filtered, and dried at 80°C to obtain the ammonium polyphosphate-loaded sepiolite fiber.

[0051] Example

[0052] Example 1

[0053] This embodiment discloses an environmentally friendly PP plastic floor, and the preparation method is as follows:

[0054] 30 parts of polypropylene, 10 parts of maleic anhydride grafted polypropylene, 100 parts of calcium carbonate, 25 parts of palygorskite, 20 parts of ammonium polyphosphate loaded sepiolite fiber, 2 parts of antistatic agent, 3 parts of antioxidant, 3 parts of stabilizer, 2 parts of coupling agent, and 0.2 parts of color powder are mixed and stirred uniformly; in this embodiment, the polypropylene is a random copolymer polypropylene, the model is SECCO B4902T; the model of maleic anhydride grafted polypropylene is ZJ-900P; the ammonium polyphosphate loaded sepiolite fiber is prepared by Preparation Example 1; the antistatic agent is an alkyl sulfonic acid antistatic agent, specifically sodium dodecyl sulfonate; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1; the stabilizer is zinc stearate; the coupling agent is aluminate coupling agent SG-Al821, and the color powder is carbon black;

[0055] The mixed materials are subjected to mixing, calendering, cooling, cutting, storage and curing to obtain PP mid-base material;

[0056] The PP mid-base material, PP printed surface material, and PP transparent material are sequentially molded, pushed, and molded; in this embodiment, the PP printed surface material and the PP transparent material are both from Nanjing Meigaomei New Materials Co., Ltd.; and then fired in a hot press to obtain a semi-finished product, which is cured for 48 hours until the temperature of the semi-finished product tends to be stable;

[0057] The surface of the coating film is treated with PU by a UV machine, and the physical properties are treated by secondary heating and tempering by a tempering machine. After cutting, curing and molding, the environmentally friendly PP plastic floor is obtained.

[0058] Example 2

[0059] The difference between this embodiment and embodiment 1 is that the environmentally friendly PP plastic floor is prepared by the following method:

[0060] 25 parts of polypropylene, 15 parts of maleic anhydride grafted polypropylene, 100 parts of calcium carbonate, 40 parts of palygorskite, 10 parts of ammonium polyphosphate loaded sepiolite fiber prepared in Preparation Example 1, 2 parts of alkyl sulfonic acid antistatic agent, 3 parts of antioxidant, 3 parts of zinc stearate, 2 parts of aluminate coupling agent, and 0.2 parts of carbon black were mixed and stirred uniformly;

[0061] The mixed materials are subjected to mixing, calendering, cooling, cutting, storage and curing to obtain PP mid-base material;

[0062] The PP mid-base material, PP printed surface material and PP transparent material are sequentially molded, pushed and molded; then fired in a hot press to obtain a semi-finished product, which is cured for 48 hours until the temperature of the semi-finished product tends to be stable;

[0063] The surface of the coating film is treated with PU by a UV machine, and the physical properties are treated by secondary heating and tempering by a tempering machine. After cutting, curing and molding, the environmentally friendly PP plastic floor is obtained.

[0064] Example 3

[0065] The difference between this embodiment and embodiment 1 is that the environmentally friendly PP plastic floor is prepared by the following method:

[0066] 35 parts of polypropylene, 12 parts of maleic anhydride grafted polypropylene, 100 parts of calcium carbonate, 20 parts of palygorskite, 30 parts of ammonium polyphosphate loaded sepiolite fiber prepared in Preparation Example 1, 2 parts of alkyl sulfonic acid antistatic agent, 3 parts of antioxidant, 3 parts of zinc stearate, 2 parts of aluminate coupling agent, and 0.2 parts of carbon black were mixed and stirred uniformly;

[0067] The mixed materials are subjected to mixing, calendering, cooling, cutting, storage and curing to obtain PP mid-base material;

[0068] The PP mid-base material, PP printed surface material and PP transparent material are sequentially molded, pushed and molded; then fired in a hot press to obtain a semi-finished product, which is cured for 48 hours until the temperature of the semi-finished product tends to be stable;

[0069] The surface of the coating film is treated with PU by a UV machine, and the physical properties are treated by secondary heating and tempering by a tempering machine. After cutting, curing and molding, the environmentally friendly PP plastic floor is obtained.

[0070] Example 4

[0071] The difference between this embodiment and embodiment 1 is that the environmentally friendly PP plastic floor is prepared by the following method:

[0072] 30 parts of polypropylene, 10 parts of maleic anhydride grafted polypropylene, 100 parts of calcium carbonate, 25 parts of palygorskite, 20 parts of ammonium polyphosphate loaded sepiolite fiber prepared in Preparation Example 2, 2 parts of alkyl sulfonic acid antistatic agent, 3 parts of antioxidant, 3 parts of zinc stearate, 2 parts of aluminate coupling agent, and 0.2 parts of carbon black were mixed and stirred uniformly;

[0073] The mixed materials are subjected to mixing, calendering, cooling, cutting, storage and curing to obtain PP mid-base material;

[0074] The PP mid-base material, PP printed surface material and PP transparent material are sequentially molded, pushed and molded; then fired in a hot press to obtain a semi-finished product, which is cured for 48 hours until the temperature of the semi-finished product tends to be stable;

[0075] The surface of the coating film is treated with PU by a UV machine, and the physical properties are treated by secondary heating and tempering by a tempering machine. After cutting, curing and molding, the environmentally friendly PP plastic floor is obtained.

[0076] Example 5

[0077] The difference between this embodiment and embodiment 1 is that the environmentally friendly PP plastic floor is prepared by the following method:

[0078] 30 parts of polypropylene, 10 parts of maleic anhydride grafted polypropylene, 100 parts of calcium carbonate, 25 parts of palygorskite, 20 parts of ammonium polyphosphate loaded sepiolite fiber prepared in Preparation Example 3, 2 parts of alkyl sulfonic acid antistatic agent, 3 parts of antioxidant, 3 parts of zinc stearate, 2 parts of aluminate coupling agent, and 0.2 parts of carbon black were mixed and stirred uniformly;

[0079] The mixed materials are subjected to mixing, calendering, cooling, cutting, storage and curing to obtain PP mid-base material;

[0080] The PP mid-base material, PP printed surface material and PP transparent material are sequentially molded, pushed and molded; then fired in a hot press to obtain a semi-finished product, which is cured for 48 hours until the temperature of the semi-finished product tends to be stable;

[0081] The surface of the coating film is treated with PU by a UV machine, and the physical properties are treated by secondary heating and tempering by a tempering machine. After cutting, curing and molding, the environmentally friendly PP plastic floor is obtained.

[0082] Example 6

[0083] The difference between this embodiment and embodiment 1 is that the surface of palygorskite is modified by the following method:

[0084] The palygorskite was immersed in a 10wt% hydrochloric acid solution and immersed at 40°C for 2h to obtain activated palygorskite; the activated palygorskite was immersed in a 5wt% Tween T-80 solution, stirred at 60°C for 4h, filtered and dried to obtain modified palygorskite.

[0085] Environmentally friendly PP plastic floor is made by the following method:

[0086] 30 parts of polypropylene, 10 parts of maleic anhydride grafted polypropylene, 100 parts of calcium carbonate, 25 parts of modified palygorskite, 20 parts of ammonium polyphosphate loaded sepiolite fiber prepared in Preparation Example 1, 2 parts of alkyl sulfonic acid antistatic agent, 3 parts of antioxidant, 3 parts of zinc stearate, 2 parts of aluminate coupling agent, and 0.2 parts of carbon black were mixed and stirred uniformly;

[0087] The mixed materials are subjected to mixing, calendering, cooling, cutting, storage and curing to obtain PP mid-base material;

[0088] The PP mid-base material, PP printed surface material and PP transparent material are sequentially molded, pushed and molded; then fired in a hot press to obtain a semi-finished product, which is cured for 48 hours until the temperature of the semi-finished product tends to be stable;

[0089] The surface of the coating film is treated with PU by a UV machine, and the physical properties are treated by secondary heating and tempering by a tempering machine. After cutting, curing and molding, the environmentally friendly PP plastic floor is obtained.

[0090] Comparative Example

[0091] Comparative Example 1

[0092] The difference between this comparative example and comparative example 1 is that the environmentally friendly PP plastic floor is prepared by the following method:

[0093] Mix 30 parts of polypropylene, 100 parts of calcium carbonate, 2 parts of alkyl sulfonic acid antistatic agent, 3 parts of antioxidant, 3 parts of zinc stearate, 2 parts of aluminate coupling agent and 0.2 parts of carbon black and stir evenly;

[0094] The mixed materials are subjected to mixing, calendering, cooling, cutting, storage and curing to obtain PP mid-base material;

[0095] The PP mid-base material, PP printed surface material and PP transparent material are sequentially molded, pushed and molded; then fired in a hot press to obtain a semi-finished product, which is cured for 48 hours until the temperature of the semi-finished product tends to be stable;

[0096] The surface of the coating film is treated with PU by a UV machine, and the physical properties are treated by secondary heating and tempering by a tempering machine. After cutting, curing and molding, the environmentally friendly PP plastic floor is obtained.

[0097] Comparative Example 2

[0098] The difference between this comparative example and comparative example 1 is that the environmentally friendly PP plastic floor is prepared by the following method:

[0099] 30 parts of polypropylene, 10 parts of maleic anhydride grafted polypropylene, 100 parts of calcium carbonate, 45 parts of palygorskite, 2 parts of alkyl sulfonic acid antistatic agent, 3 parts of antioxidant, 3 parts of zinc stearate, 2 parts of aluminate coupling agent, and 0.2 parts of carbon black were mixed and stirred uniformly;

[0100] The mixed materials are subjected to mixing, calendering, cooling, cutting, storage and curing to obtain PP mid-base material;

[0101] The PP mid-base material, PP printed surface material and PP transparent material are sequentially molded, pushed and molded; then fired in a hot press to obtain a semi-finished product, which is cured for 48 hours until the temperature of the semi-finished product tends to be stable;

[0102] The surface of the coating film is treated with PU by a UV machine, and the physical properties are treated by secondary heating and tempering by a tempering machine. After cutting, curing and molding, the environmentally friendly PP plastic floor is obtained.

[0103] Comparative Example 3

[0104] The difference between this comparative example and comparative example 1 is that the environmentally friendly PP plastic floor is prepared by the following method:

[0105] 30 parts of polypropylene, 10 parts of maleic anhydride grafted polypropylene, 100 parts of calcium carbonate, 45 parts of ammonium polyphosphate loaded sepiolite fiber prepared in Preparation Example 1, 2 parts of alkyl sulfonic acid antistatic agent, 3 parts of antioxidant, 3 parts of zinc stearate, 2 parts of aluminate coupling agent, and 0.2 parts of carbon black were mixed and stirred uniformly;

[0106] The mixed materials are subjected to mixing, calendering, cooling, cutting, storage and curing to obtain PP mid-base material;

[0107] The PP mid-base material, PP printed surface material and PP transparent material are sequentially molded, pushed and molded; then fired in a hot press to obtain a semi-finished product, which is cured for 48 hours until the temperature of the semi-finished product tends to be stable;

[0108] The surface of the coating film is treated with PU by a UV machine, and the physical properties are treated by secondary heating and tempering by a tempering machine. After cutting, curing and molding, the environmentally friendly PP plastic floor is obtained.

[0109] Performance testing

[0110] The environmentally friendly PP plastic floor samples prepared in Examples 1-6 and Comparative Examples 1-3 were taken to test the impact resistance, heating dimensional change rate, flame retardant performance and sound insulation effect of the plastic floor. The impact resistance was tested with reference to the standard GB / T 9639.1-2008; the heating dimensional change rate was tested with reference to the standard DIN ENISO 23999; the flame retardant performance was tested with reference to the standard GB / T 2408-2021, and the sound insulation performance was tested with reference to the standard GB / T 19885-2005.

[0111] The test results are summarized in Table 1.

[0112] Table 1

[0113]

[0114]

[0115] In combination with Examples 1-6, Comparative Example 1 and Table 1, it can be seen that the PP plastic floor prepared according to the formula and method disclosed in the present application not only has environmentally friendly raw materials, is green and safe, but also has good mechanical properties, high dimensional stability, excellent flame retardant properties, and better sound insulation effect. It can be used in multiple application environments such as homes and workplaces, and has better application effects and performance.

[0116] Combining Examples 1-6, Comparative Example 2, Comparative Example 3 and Table 1, it can be seen that the combination of palygorskite and ammonium polyphosphate-loaded sepiolite fiber can give the PP plastic floor better flame retardant properties and higher sound insulation effects, so that the PP plastic floor has better performance.

[0117] It can be seen from Example 1, Example 6 and Table 1 that surface modification of palygorskite can further improve the mechanical properties and sound insulation effect of the PP plastic floor.

[0118] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An environmentally friendly PP plastic floor, characterized in that: The PP mid-base material, PP printed surface and PP transparent material are laid in sequence, fired into semi-finished products, and then cured, surface PU treated, heated and tempered for the second time, and formed; The PP base material includes the following raw materials in parts by weight: 25-35 parts of polypropylene, 10-15 parts of maleic anhydride grafted polypropylene, 90-120 parts of calcium carbonate, 20-40 parts of palygorskite, 10-30 parts of ammonium polyphosphate loaded sepiolite fiber, 1-4 parts of antistatic agent, 2-4 parts of antioxidant, 2-4 parts of stabilizer, 1-3 parts of coupling agent, and 0.1-1 parts of color powder.

2. The environmentally friendly PP plastic floor according to claim 1, characterized in that: The ammonium polyphosphate loaded sepiolite fiber is obtained by absorbing the ammonium polyphosphate after the sepiolite fiber is activated by acid.

3. The environmentally friendly PP plastic floor according to claim 2, characterized in that: The preparation method of the ammonium polyphosphate-loaded sepiolite fiber specifically comprises: The sepiolite fiber is acid-activated by using an acid solution, and then washed to neutrality to obtain the activated sepiolite fiber; The activated sepiolite fiber is immersed in water, water-soluble ammonium polyphosphate is added thereto at 40-80° C., stirred for 6-12 hours, allowed to stand, filtered, and dried to obtain the ammonium polyphosphate-loaded sepiolite fiber.

4. The environmentally friendly PP plastic floor according to claim 3, characterized in that: The mass of the water-soluble ammonium polyphosphate is 5-30% of the mass of the sepiolite fiber.

5. The environmentally friendly PP plastic floor according to claim 3, characterized in that: The water-soluble ammonium polyphosphate is ammonium tripolyphosphate.

6. The environmentally friendly PP plastic floor according to claim 1, characterized in that: The palygorskite is a modified palygorskite that is activated by acid and then surface treated by a surfactant.

7. The environmentally friendly PP plastic floor according to claim 6, characterized in that: The preparation method of the modified palygorskite comprises: The palygorskite is subjected to acid activation treatment with an acid solution, and then washed to neutrality to obtain activated palygorskite; the activated palygorskite is immersed in a surfactant aqueous solution, stirred at 40-80° C. for 2-6 hours, filtered, and dried to obtain modified palygorskite.

8. The environmentally friendly PP plastic floor according to claim 1, characterized in that: The coupling agent is an aluminate coupling agent.

9. The environmentally friendly PP plastic floor according to claim 1, characterized in that: The antistatic agent is an alkyl sulfonic acid.

10. A method for preparing the environmentally friendly PP plastic floor as claimed in claim 1, characterized in that: The following steps are involved: According to the proportion, polypropylene, maleic anhydride grafted polypropylene, calcium carbonate, palygorskite, ammonium polyphosphate loaded sepiolite fiber, antistatic agent, antioxidant, stabilizer, coupling agent and color powder are mixed and stirred evenly, and then the mixture is subjected to banburying, calendering, cooling, cutting and curing to obtain PP mid-base material; The PP mid-base material, PP printed surface material and PP transparent material are sequentially molded, pushed and molded, fired by a hot press to obtain a semi-finished product, and cured until the temperature of the semi-finished product tends to be stable; The surface of the coating film is treated with PU by a UV machine, and the physical properties are treated by secondary heating and tempering by a tempering machine. After curing and molding, an environmentally friendly PP plastic floor is obtained.