Preparation method of material for inhibiting cyclic expansion and pulverization of silicon-carbon negative electrode

Through the silicon carbon material process of high elastic polymer coating and high ionic conductivity material absorption, the problem of cyclic expansion and powderization of silicon negative electrodes is solved, and the high cycle stability and electrochemical performance of lithium-ion batteries are improved, making up for the current situation. There are disadvantages of complex process and insufficient electrochemical performance in the technology.

CN119050291APending Publication Date: 2024-11-29CIVIL AVIATION FLIGHT UNIV OF CHINA +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411042120.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The silicon negative electrode has severe volume expansion during the circulation process, resulting in structural collapse, powderization and repeated formation of solid electrolyte interface film, resulting in irreversible consumption of active lithium ions and rapid attenuation of capacity, reducing the Coulomb efficiency and cycle life of lithium ion batteries. .

Method used

The silicon carbon particles are coated with high elastic polymer materials and fully absorb high ionic conductivity materials on their surfaces. Through this process, the silicon carbon material is bound to circulating expansion, inhibit silicon expansion and powdering, and reduce lithium ions. consumption.

Benefits of technology

It achieves a good capacity retention rate during the long-term charge and discharge cycle, improves the cycle stability and electrochemical performance of lithium-ion batteries, solves the problem of expansion and powderization of silicon negative electrodes, and has a simple process and controllable structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050291A_ABST
    Figure CN119050291A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a material for inhibiting cyclic expansion and pulverization of a silicon-carbon negative electrode, and the silicon-carbon negative electrode which has high mechanical strength and good ionic conductivity and can inhibit self-cyclic expansion and pulverization is prepared by a method of coating a high-elasticity polymer on silicon-carbon particles and then compounding the silicon-carbon particles with a high-ionic-conductivity material. The silicon-carbon negative electrode prepared by the invention has the advantages of simple process at normal temperature, high mechanical property, high ionic conductivity, high electrochemical stability and the like. The defects that other methods need multi-stage pore forming, equipment is expensive, procedures are complex, and high mechanical performance and high electrochemical performance cannot be achieved at the same time are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of new energy and lithium batteries, and in particular to a method for preparing a material that inhibits cyclic expansion and pulverization of a silicon-carbon negative electrode. Background Art

[0002] The specific energy of silicon anode is 4200mAh / g, which is much higher than the currently commonly used graphite anode (372mAh / g), and is the best choice for the next generation of lithium-ion battery anode materials. However, the silicon anode will experience severe volume expansion during the cycle, causing its structure to gradually collapse and pulverize, and the solid electrolyte interphase (SEI) film to form repeatedly, resulting in irreversible consumption of active lithium ions and rapid capacity decay, thereby reducing the coulombic efficiency and cycle life of the battery. Researchers have developed a variety of methods to suppress the expansion and pulverization problem of silicon anodes. For example: the method of developing amorphous porous silicon. During the lithium insertion process, the amorphous porous silicon expands isotropically, which is conducive to alleviating the pulverization and shedding of particles caused by volume changes, avoiding the collapse of the porous structure, and effectively extending the lithium insertion cycle life of amorphous porous silicon (CN 102969488A); using the high-energy ball milling method to combine nano-silicon with MXene of two-dimensional layered structure, and designing the shell-core structure of the porous network, it can effectively buffer the volume expansion of nano-silicon particles during the charging and discharging process, prevent the direct contact between the electrolyte and the silicon interface, and then synergistically improve the specific capacity and cycle stability of lithium-ion batteries (CN109346681A); developing a method for preparing silicon-carbon composite materials, using a metal organic framework ZIF8 membrane to wrap the nano-silicon core-shell structure to form a precursor, adding a carbon source to carbonize to obtain a carbon layer to wrap the nano-silicon core-shell structure. This method can achieve a single continuous wrapping of nano-silicon by the carbon layer, avoid the re-agglomeration of nano-silicon, effectively alleviate the volume expansion of silicon materials during the charging and discharging process, and effectively control the pulverization and deactivation of silicon powder (CN109742355A), etc. However, these methods also have their own disadvantages, such as complicated preparation process, low electronic conductivity, and inability to completely solve the pulverization problem.

[0003] Therefore, there is an urgent need to develop a preparation method with simple preparation process, excellent electrochemical performance and the ability to inhibit the expansion and powdering of silicon negative electrodes during long cycles. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a method for preparing a material that inhibits the cyclic expansion and pulverization of a silicon-carbon negative electrode. The prepared silicon-carbon material has high ionic conductivity and electronic conductivity, and can maintain a good capacity retention rate during long-term charge and discharge cycles. The silicon-carbon particles are coated with a highly elastic polymer material on the outer layer, which can restrain the silicon-carbon particles during the continuous expansion and pulverization of the silicon-carbon particles during the cycle, thereby inhibiting the expansion and pulverization of silicon during the charge and discharge process, reducing the consumption of lithium ions, and solving the problems mentioned in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing a material that inhibits the cyclic expansion and pulverization of a silicon-carbon negative electrode, comprising the following steps:

[0006] S1, dispersing a high elastic polymer emulsion and a conductive agent in a solvent according to a mass ratio to prepare a uniform solution;

[0007] S2, dispersing the silicon-carbon material in the above solution so that its surface is fully covered with a layer of polymer containing a conductive agent, and then removing the solvent in an oven at 80° C.;

[0008] S3. Swell the material of S2 in a high ion conductivity solution so that the polymer material coated on the outer layer of the silicon-carbon material can be fully absorbed.

[0009] Preferably, the silicon-carbon material has a particle size of 7-10 μm, a silicon content of 44%-48%, and a gram capacity of 1780-1900 mAh / g.

[0010] Preferably, the high elastic polymer emulsion is one or more of natural rubber emulsion, chloroprene rubber latex, styrene-butadiene rubber emulsion, cis-1,4-butadiene rubber emulsion and silicone rubber emulsion.

[0011] Preferably, the conductive agent is one or more of acetylene black, carbon nanotubes, and graphene.

[0012] Preferably, the mass ratio of the conductive agent in the high elastic polymer emulsion is 5%-20%.

[0013] Preferably, the high ionic conductivity solution is one or more of succinonitrile, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, N-butylpyridine bis(trifluoromethanesulfonyl)imide, 1-octyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide, and 1-dodecyl-3-methyl-1H-imidazole sulfate.

[0014] Preferably, the swelling time is 0.5h-2h.

[0015] Preferably, after 50 cycles at 0.3C rate, the prepared silicon-carbon negative electrode material has a gram capacity of 1784.5 mAh / g and a coulombic efficiency of 99.7%, and after 300 cycles, there are no cracks or powdering on the surface of the silicon-carbon negative electrode material.

[0016] The beneficial effects of the present invention are as follows: the silicon-carbon negative electrode material prepared by the present invention has the advantages of simple process at room temperature, controllable structure, high ionic conductivity and high electronic conductivity. It makes up for the shortcomings of other methods that require expensive equipment, complicated procedures, and cannot suppress the expansion of the negative electrode in long cycles. The existing technology often finds it difficult to balance the mechanical properties and electrochemical properties of the silicon-carbon negative electrode. The silicon-carbon material is first coated with a highly elastic polymer on the outer layer, and then absorbs a material with high ionic conductivity, and has excellent electrochemical properties. This silicon-carbon has excellent cycle stability in a long cycle condition at a current density of 0.3C, and there is no powdering on the particle surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A schematic diagram showing that the pulverization of the silicon-carbon negative electrode material of the present invention is suppressed after cycling;

[0018] Figure 2 is the stress-strain diagram of the high elastic coating layer of the silicon-carbon negative electrode material of the present invention;

[0019] Figure 3 The SEM images of the negative electrode surface of the silicon-carbon negative electrode material of the present invention after 300 cycles, (a) and (b) are commercial silicon-carbon negative electrodes, (c) and (d) are the silicon-carbon negative electrodes of the present invention;

[0020] Figure 4 This is a performance diagram of the silicon-carbon negative electrode material of the present invention after 50 cycles at a 0.3C rate. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] The natural rubber latex and carbon nanotubes were weighed in a mass ratio of 85:15, and stirred and ultrasonicated for 30 minutes to form a uniform solution. The silicon-carbon material was placed in it, and the stirring and ultrasonication were continued for 60 minutes, and then the solvent was removed in an oven at 80°C. The dried material was then placed in succinonitrile at 65°C and fully swollen for 40 minutes before being taken out.

[0024] like Figure 1As shown in FIG. 1 , it can be seen that the pulverization of the silicon-carbon negative electrode material of the present invention is suppressed after cycling. The stress-strain of the high elastic coating layer of the silicon-carbon negative electrode material is shown in FIG. Figure 2 As shown by Figure 2 It can be seen that the maximum elastic strain of the material is 450% and the maximum stress is 22.5Mpa. The material was equipped in a button battery (rate 0.3C) to test its 300-cycle long cycle stability, and the performance is listed in Appendix 1. Figure 3 It can also be seen that Figure 3 Figures (a) and (b) are commercial silicon-carbon negative electrodes, and after cycling, the surface of the material has obvious cracks and powdering; Figures (c) and (d) are the silicon-carbon negative electrode of the present invention, and it can be seen that there are no cracks on the surface of the material after cycling. Figure 4 As shown in the figure, it is the performance diagram of the silicon-carbon negative electrode material of the present invention after 0.3C rate cycling. It can be seen that after 50 cycles, the gram capacities of the commercial silicon-carbon material and the silicon-carbon material of the present invention are 1582.8mAh / g and 1784.5mAh / g, respectively, and the coulombic efficiencies are 99.2% and 99.7%, respectively. It proves that the silicon-carbon negative electrode material of the present invention has excellent cycle stability in the long cycle condition of current density 0.3C rate, and there is no powdering on the particle surface.

[0025] Example 2

[0026] Weigh the chloroprene rubber latex and carbon nanotubes at a mass ratio of 90:10, stir and ultrasonicate for 30 minutes to form a uniform solution. Place the silicon-carbon material in it, continue stirring and ultrasonicate for 60 minutes, and then remove the solvent in an oven. Then place the dried material in 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt at 25°C, and take it out after fully swelling for 60 minutes.

[0027] The material was equipped in a button cell (rate 0.3C) to test its 300-cycle long cycle stability, and the performance is listed in Appendix 1.

[0028] Example 3

[0029] Weigh styrene-butadiene rubber latex and carbon nanotubes at a mass ratio of 80:20, stir and ultrasonicate for 30 minutes to form a uniform solution. Place silicon-carbon material in it, continue stirring and ultrasonicate for 60 minutes, and then remove the solvent in an oven. Then place the dried material in 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt at 25°C, and take it out after fully swelling for 50 minutes.

[0030] The material was equipped in a button cell (rate 0.3C) to test its 300-cycle long cycle stability, and the performance is listed in Appendix 1.

[0031] Example 4

[0032] Weigh butadiene rubber latex and acetylene black in a mass ratio of 88:12, stir and ultrasonicate for 30 minutes to form a uniform solution. Place the silicon-carbon material in it, continue to stir and ultrasonicate for 60 minutes, and then remove the solvent in an oven. Then place the dried material in N-butylpyridine bis(trifluoromethanesulfonyl)imide salt at 25°C, and take it out after fully swelling for 45 minutes.

[0033] The material was equipped in a button cell (rate 0.3C) to test its 300-cycle long cycle stability, and the performance is listed in Appendix 1.

[0034] Example 5

[0035] Weigh chloroprene rubber latex and graphene in a mass ratio of 85:15, stir and ultrasonicate for 30 minutes to form a uniform solution. Place silicon-carbon material in it, continue to stir and ultrasonicate for 60 minutes, and then remove the solvent in an oven. Then place the dried material in 1-octyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide salt at 30°C, and take it out after fully swelling for 65 minutes.

[0036] The material was equipped in a button cell (rate 0.3C) to test its 300-cycle long cycle stability, and the performance is listed in Appendix 1.

[0037] Example 6

[0038] Weigh the silicone rubber emulsion and carbon nanotubes at a mass ratio of 88:12, stir and ultrasonicate for 30 minutes to form a uniform solution. Place the silicon-carbon material in it, continue to stir and ultrasonicate for 60 minutes, and then remove the solvent in an oven. Then place the dried material in 1-dodecyl-3-methyl-1H-imidazole sulfate at 25°C, and take it out after fully swelling for 60 minutes.

[0039] The material was equipped in a button cell (rate 0.3C) to test its 300-cycle long cycle stability, and the performance is listed in Appendix 1.

[0040] Table 1

[0041]

[0042] The above table shows the test results of post-cycle pulverization and post-cycle capacity retention of the silicon-carbon negative electrode prepared in Examples 1 to 6. As can be seen from the above table, a layer of high electron conductivity polymer elastomer is coated on the surface of the silicon-carbon particles, and then the plastic crystal material or ionic liquid material is swollen inside the linear polymer to prepare a new silicon-carbon negative electrode material with high mechanical properties, good ionic conductivity and suppressed expansion.

[0043] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a material that inhibits cyclic expansion and pulverization of a silicon-carbon negative electrode, characterized in that: The steps include: S1, dispersing a high elastic polymer emulsion and a conductive agent in a solvent according to a mass ratio to prepare a uniform solution; S2, dispersing the silicon-carbon material in the above solution so that its surface is fully covered with a layer of polymer containing a conductive agent, and then removing the solvent in an oven at 80° C.; S3. Swell the material of S2 in a high ion conductivity solution so that the polymer material coated on the outer layer of the silicon-carbon material can be fully absorbed.

2. The method for preparing a material for inhibiting cyclic expansion and pulverization of a silicon-carbon negative electrode according to claim 1, characterized in that: The silicon-carbon material has a particle size of 7-10 μm, a silicon content of 44%-48%, and a gram capacity of 1780-1900 mAh / g.

3. The method for preparing a material for inhibiting cyclic expansion and pulverization of a silicon-carbon negative electrode according to claim 1, characterized in that: The dispersion method in step S1 is stirring and / or ultrasound.

4. The method for preparing a material for inhibiting cyclic expansion and pulverization of a silicon-carbon negative electrode according to claim 1, characterized in that: The high elastic polymer emulsion is one or more of natural rubber emulsion, chloroprene rubber latex, styrene-butadiene rubber emulsion, cis-1,4-butadiene rubber emulsion and silicone rubber emulsion.

5. The method for preparing a material for inhibiting cyclic expansion and pulverization of a silicon-carbon negative electrode according to claim 1, characterized in that: The conductive agent is one or more of acetylene black, carbon nanotubes and graphene.

6. The method for preparing a material for inhibiting cyclic expansion and pulverization of a silicon-carbon negative electrode according to claim 1, characterized in that: The mass ratio of the conductive agent in the high-elastic polymer emulsion is 5%-20%.

7. The method for preparing a material for inhibiting cyclic expansion and pulverization of a silicon-carbon negative electrode according to claim 5, characterized in that: The high ion conductivity solution is one or more of succinonitrile, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, N-butylpyridine bis(trifluoromethanesulfonyl)imide, 1-octyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide, and 1-dodecyl-3-methyl-1H-imidazole sulfate.

8. The method for preparing a material for inhibiting cyclic expansion and pulverization of a silicon-carbon negative electrode according to claim 1, characterized in that: The swelling time is 0.5h-2h.

9. The method for preparing a material for inhibiting cyclic expansion and pulverization of a silicon-carbon negative electrode according to claim 1, characterized in that: After 50 cycles at a rate of 0.3C, the prepared silicon-carbon negative electrode material has a gram capacity of 1784.5 mAh / g and a coulombic efficiency of 99.7%. After 300 cycles, there are no cracks or powdering on the surface of the silicon-carbon negative electrode material.

Citation Information

Cited By

  • Double-coating-layer modified silicon-based negative electrode material and preparation method thereof, negative electrode and lithium ion battery

    CN121964601A

  • A negative electrode material, a preparation method therefor, and an application thereof