Graphite / silicon composite material and preparation method and application thereof
By using an expanded graphite skeleton in lithium-ion batteries to embed silicon nanoparticles and surface coating, the volume expansion problem of silicon materials during high-temperature sintering and the problem of insufficient graphite energy density is solved, and high energy density and excellent rate performance are achieved. Lithium-ion battery.
Patent Information
- Application Number
- CN202411184599.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-26
Smart Images

Figure CN119050308A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium ion batteries, and in particular, relates to a graphite / silicon composite material and a preparation method and application thereof. Background Art
[0002] In recent years, lithium-ion batteries (LIBs) have been widely used in portable devices, electric vehicles, and energy storage grids. The demand for high energy density applications has encouraged researchers to explore high-capacity, environmentally friendly, and low-cost electrode materials. Among the materials that form an intermetallic phase with lithium (Li), silicon (Si) is considered to be one of the most promising anode materials to replace the most advanced graphite materials. It has a capacity of 4200mAh g -1 The high theoretical specific capacity and low delithiation potential (~0.4 V vs Li / Li + ), relatively low voltage hysteresis, and its precursor materials (such as silicon dioxide) are very abundant and low-cost. However, the huge volume expansion of silicon (ranging from 300% to 400%) leads to the pulverization of silicon particles and the repeated formation of an unstable solid-electrolyte interphase (SEI), and silicon has low electrical conductivity.
[0003] The graphite negative electrode has the advantages of stable structure and excellent conductivity, but its theoretical specific capacity is 372mAh / g, and the energy density improvement is limited. + The diffusion inside the particles does not match the lithium insertion and extraction rate on the particle surface, and various polarizations will inevitably occur, including ohmic polarization, concentration overpotential, and charge transfer overpotential. Therefore, whether from the perspective of cost or performance, constructing a reasonable graphite and nano-silicon composite material is considered to be the most reasonable direction for exploring new negative electrode materials.
[0004] The prior art discloses a method for preparing a carbon-silicon sandwich material and its application in lithium-ion batteries. The method comprises the following steps: (1) mixing nano-silicon, graphite material and non-graphite conductive carbon layer material; (2) extruding or rolling the mixture so that the graphite material separates and surrounds the nano-silicon to form a tightly stacked multi-layer sandwich structure; (3) performing a first sintering at 200-1200°C in an inert atmosphere to obtain a carbon-silicon sandwich material precursor; (4) uniformly mixing the carbon-silicon sandwich material precursor and the non-graphite conductive carbon layer material, and performing a second sintering at 800-1200°C in an inert atmosphere to obtain carbon-silicon sandwich material particles. The composite material prepared by this method has been sintered twice, but silicon will melt again in a high temperature environment to form large particles. Although the interlayer limits a certain amount of expansion, the expansion inhibition is not obvious because silicon aggregates again at high temperature and becomes larger in volume.
[0005] The contents of the background technology section are merely the technologies known to the inventors and do not necessarily represent the prior art in the field. Summary of the invention
[0006] In view of at least one problem in the prior art, the present application provides a graphite / silicon composite material in a first aspect. The graphite / silicon composite material comprises:
[0007] Expanded graphite;
[0008] Silicon nanoparticles located between the layers of the expanded graphite; and
[0009] A coating layer, coating the surface of the expanded graphite;
[0010] Wherein, the coating layer includes a conductive agent and a binder.
[0011] This application combines the high capacity of silicon and the excellent conductivity of graphite, and has the advantages of high energy density, excellent rate performance, high cycle efficiency, etc. It is environmentally friendly and sustainable. This application uses expanded graphite as a skeleton. Expanded graphite with a layered structure can enhance the Li + The diffusion rate inside the graphite accelerates the graphite dynamics. Silicon nanoparticles are only located between the layers of expanded graphite, but not on the surface, which can effectively inhibit the volume expansion of silicon and improve the low conductivity of silicon. The surface coating can further reduce the volume expansion of silicon, facilitate the rapid transmission of ions and electrons, and weaken the contact between the material and the electrolyte, significantly improving the cycle performance.
[0012] In some embodiments of the present application, the graphite / silicon composite material satisfies at least one of the following conditions:
[0013] a) the content of silicon in the graphite / silicon composite material is 0.2-30wt%, and the content of carbon is 70-99.8wt%;
[0014] b) Median particle size D of the graphite / silicon composite material 50 5~15μm;
[0015] c) the interlayer spacing of the expanded graphite is 0.4 to 1.2 nm;
[0016] d) The median particle size D of the silicon nanoparticles 50 0.5~1.2nm;
[0017] e) the coating layer has a thickness of 0.01 to 100 nm;
[0018] f) the conductive agent is selected from one or more of carbon black, conductive carbon fiber, graphene and carbon nanotubes;
[0019] g) the binder is a polyacrylic acid series binder;
[0020] h) The mass ratio of the conductive agent to the binder in the coating layer is 1:(20-30).
[0021] Graphite / silicon composite materials that meet the above conditions have better performance.
[0022] The second aspect of the present application provides a method for preparing a graphite / silicon composite material, comprising the following steps:
[0023] S1: dispersing silicon nanoparticles in an organic solvent to obtain an impregnating agent;
[0024] S2: placing the expanded graphite into the impregnating agent for vacuum impregnation, so that the silicon nanoparticles are deposited between the layers and on the surface of the expanded graphite to obtain a first intermediate product;
[0025] S3: subjecting the first intermediate product to ultrasonic treatment to uniformly disperse the silicon nanoparticles deposited between the expanded graphite layers, and removing the silicon nanoparticles deposited on the surface of the expanded graphite to obtain a second intermediate product;
[0026] S4: filtering the second intermediate product, and then freeze-drying the filter residue to obtain a third intermediate product; and
[0027] S5: using a polymer precursor to coat the surface of the third intermediate product to obtain the graphite / silicon composite material; wherein the polymer precursor includes a conductive agent and a binder.
[0028] The method provided in the present application embeds silicon nanoparticles between graphite layers by vacuum impregnation, and then performs ultrasonic treatment to cause collisions between graphite particles, so that silicon nanoparticles deposited on the outer surface of graphite are shaken off and rubbed off, and silicon nanoparticles deposited between graphite layers are dispersed more evenly. Next, the organic solvent is removed by filtration and freeze drying, which can effectively prevent the aggregation of silicon nanoparticles. Finally, the prepared material is surface coated, which can further reduce the volume expansion of silicon, weaken the contact between the negative electrode material and the electrolyte, and significantly improve the cycle performance.
[0029] In some embodiments of the present application, the preparation method further comprises the following steps:
[0030] S0: preparing the expanded graphite by using artificial graphite;
[0031] Optionally, the interlayer spacing of the expanded graphite is 0.4 to 1.2 nm;
[0032] Optionally, the median particle size D of the artificial graphite 50 5~15μm;
[0033] Optionally, the artificial graphite is rapidly heated to 800-1200° C. and then kept warm, thereby obtaining the expanded graphite; further optionally, the heating rate is 10-30° C. / min, and the keeping time is 5-60 min.
[0034] Expanded graphite is prepared by increasing the interlayer spacing of graphite through high temperature heat treatment, which can enhance the Li + The diffusion rate inside the graphite accelerates the graphite dynamics. The obtained expanded graphite has high conductivity and excellent dynamic properties.
[0035] In some embodiments of the present application, in step S1, the solid content of the impregnating agent is 5 to 25%;
[0036] Optionally, the median particle size D of the silicon nanoparticles is 50 0.5~1.2nm;
[0037] Optionally, the organic solvent is selected from one or more of water, ethanol, isopropanol, n-propanol and acetone;
[0038] Optionally, the silicon nanoparticles are dispersed in the organic solvent by stirring, and further optionally, the stirring time is 0.1 to 2 hours.
[0039] The impregnating agent that meets the above conditions has better performance.
[0040] In some embodiments of the present application, in step S2, the vacuum impregnation time is 0.5 to 8 hours;
[0041] Optionally, the mass ratio of the expanded graphite to the impregnating agent is 1:(1-5).
[0042] Vacuum impregnation can successfully embed silicon nanoparticles into the interlayers of expanded graphite while preserving the original morphology of graphite.
[0043] In some embodiments of the present application, in step S3, the ultrasonic temperature is room temperature, the ultrasonic time is 10 to 120 min, and the ultrasonic power is 60 to 300 kHz;
[0044] Optionally, in step S4, freeze-drying the filter residue includes: firstly quick-freezing the filter residue in liquid nitrogen, and then placing it in a freeze dryer for freeze-drying; further optionally, the freeze-drying is carried out in a vacuum environment, and the freeze-drying time is 5 to 24 hours.
[0045] Ultrasonic treatment is simple and effective. It can cause collisions between graphites, thereby shaking off and rubbing off silicon nanoparticles deposited on the outer surface of graphite, and making the silicon nanoparticles deposited between graphite layers more evenly dispersed.
[0046] The second intermediate product is filtered to remove most of the solution, and then the filter residue is freeze-dried. Freeze-drying can protect the original structure and shape of the material to the greatest extent, preventing the silicon nanoparticles from aggregating and increasing in volume, thereby causing uncontrollable expansion.
[0047] In some embodiments of the present application, in step S5, the third intermediate product is mixed with the polymer precursor and water to prepare a slurry, and then spray-dried, so that the polymer precursor is coated on the surface of the third intermediate product;
[0048] Optionally, the solid content of the slurry is 20-30%;
[0049] Optionally, the mass ratio of the conductive agent to the binder in the polymer precursor is 1:(20-30);
[0050] Optionally, the mass ratio of the polymer precursor to the third intermediate product is (0.5-1):100.
[0051] In the present application, the polymer precursor includes a conductive agent and a binder, which can not only isolate the contact between silicon and the electrolyte, but also effectively increase the migration rate of lithium ions, thereby improving the charge and discharge efficiency and cycle performance.
[0052] The third aspect of the present application provides a negative electrode sheet, which includes any of the graphite / silicon composite materials described above, or a graphite / silicon composite material prepared by any of the preparation methods described above.
[0053] A fourth aspect of the present application provides a lithium-ion battery, comprising the above-mentioned negative electrode sheet.
[0054] The lithium-ion battery provided in the present application has excellent properties such as high energy density, excellent rate performance, and high cycle efficiency.
[0055] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] The accompanying drawings constituting a part of the present disclosure are used to provide a further understanding of the present disclosure. The illustrative embodiments of the present disclosure and their descriptions are used to explain the present disclosure and do not constitute improper limitations on the present disclosure.
[0057] Figure 1 It is a schematic diagram of the structure of a graphite / silicon composite material provided in one embodiment of the present application.
[0058] Figure 2 This is a process flow chart for preparing a graphite / silicon composite material provided in one embodiment of the present application.
[0059] Figure 3 This is a process flow chart for preparing a graphite / silicon composite material provided in another embodiment of the present application. DETAILED DESCRIPTION
[0060] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present invention. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.
[0061] The disclosure below provides many different embodiments or examples for implementing the present invention. In order to simplify the disclosure of the present invention, the components and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplicity and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides various specific examples of processes and materials, but those of ordinary skill in the art can appreciate the application of other processes and / or the use of other materials.
[0062] In addition, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those generally understood by those of ordinary skill in the art to which the present invention belongs. It will also be understood that terms, such as those defined in commonly used dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology and the present invention, and will not be interpreted in an idealized or overly formal sense unless explicitly defined in this article.
[0063] As used herein, "about" or "approximately" includes the stated value and means within an acceptable range of deviation from the particular value as determined by one skilled in the art, taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean within one or more standard deviations, or within ±30%, ±20%, ±10%, or ±5% of the stated value.
[0064] The following is a more detailed description of the specific embodiments of the present invention in conjunction with the accompanying drawings and examples, so that the scheme of the present invention and its advantages in various aspects can be better understood. However, the specific embodiments and examples described below are only for the purpose of illustration, rather than for limiting the present invention.
[0065] Figure 1 FIG. 2 shows a graphite / silicon composite material provided by an embodiment of the present application. Figure 1As shown, the graphite / silicon composite material provided by the present application comprises expanded graphite 2, silicon nanoparticles 3 and a coating layer 1. The silicon nanoparticles 3 are located between the layers of the expanded graphite 2, and the coating layer 1 is coated on the surface of the expanded graphite 2.
[0066] This application combines the high capacity of silicon and the excellent conductivity of graphite, and has the advantages of high energy density, excellent rate performance, high cycle efficiency, etc. It is environmentally friendly and sustainable. This application uses expanded graphite as a skeleton. Expanded graphite with a layered structure can enhance the Li + The diffusion rate inside the graphite accelerates the graphite dynamics. Silicon nanoparticles are only located between the layers of expanded graphite, but not on the surface, which can effectively inhibit the volume expansion of silicon and improve the low conductivity of silicon. The surface coating can further reduce the volume expansion of silicon, facilitate the rapid transmission of ions and electrons, and weaken the contact between the material and the electrolyte, significantly improving the cycle performance.
[0067] In the present application, the coating layer 1 includes a conductive agent and a binder. The coating layer provided in the present application can not only isolate the contact between silicon and the electrolyte, but also effectively increase the migration rate of lithium ions, thereby improving the charge and discharge efficiency.
[0068] Optionally, the coating layer has a thickness of 0.01 to 100 nm. In some specific embodiments, the coating layer may have a thickness of 0.01 nm, 1 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.
[0069] Optionally, the conductive agent is selected from one or more of carbon black, conductive carbon fiber, graphene and carbon nanotubes. Optionally, the binder is a polyacrylic acid series binder, such as polyacrylic acid, lithium polyacrylate, polyacrylic acid-butyl acrylate copolymer, etc.
[0070] Optionally, the mass ratio of the conductive agent to the binder in the coating layer is 1:(20-30). At this mass ratio, the contact between silicon and the electrolyte can be more effectively isolated, and the role of the conductive agent can be played. In some specific embodiments, the mass ratio of the conductive agent to the binder can be 1:20, 1:21, 1:22, 1:23, 1:24, 1:25, 1:26, 1:27, 1:28, 1:29 or 1:30.
[0071] Optionally, the content of silicon in the graphite / silicon composite material is 0.2-30wt%, and the content of carbon is 70-99.8wt%. At the above content, the high capacity of silicon and the excellent conductivity of graphite can be fully utilized. In some specific embodiments, the content of silicon may be 0.2wt%, 3wt%, 6wt%, 9wt%, 12wt%, 15wt%, 18wt%, 21wt%, 24wt%, 27wt% or 30wt%. In some specific embodiments, the carbon content may be 70wt%, 73wt%, 76wt%, 79wt%, 82wt%, 85wt%, 88wt%, 91wt%, 94wt%, 97wt% or 99.8wt%.
[0072] Optionally, the interlayer spacing of the expanded graphite is 0.4 to 1.2 nm. The interlayer spacing in this range can effectively buffer the volume change of silicon nanoparticles during lithium insertion and extraction. In some specific embodiments, the interlayer spacing of the expanded graphite can be 0.4 nm, 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, 1 nm, 1.1 nm or 1.2 nm.
[0073] Optionally, the median particle size D of the silicon nanoparticles 50 The median particle size D of the silicon nanoparticles is 0.5 to 1.2 nm. The smaller the particle size, the smaller the absolute expansion, which is more conducive to the cycle performance. 50 It may be 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, 1.0 nm, 1.1 nm or 1.2 nm.
[0074] Figure 2 A method for preparing a graphite / silicon composite material provided in an embodiment of the present application is shown, comprising the following steps S1 to S5.
[0075] S1: dispersing silicon nanoparticles in an organic solvent to obtain an impregnating agent.
[0076] Optionally, the solid content of the impregnating agent is 5-25%, that is, it includes 5-25% silicon nanoparticles. In some specific embodiments, the solid content of the impregnating agent can be 5%, 7%, 9%, 11%, 13%, 15%, 17%, 19%, 21%, 23% or 25%.
[0077] Optionally, the median particle size D of the silicon nanoparticles 50 The median particle size D of the silicon nanoparticles is 0.5 to 1.2 nm. The smaller the particle size, the smaller the absolute expansion, which is more conducive to the cycle performance. 50 It may be 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, 1.0 nm, 1.1 nm or 1.2 nm.
[0078] Optionally, the organic solvent is selected from one or more of water, ethanol, isopropanol, n-propanol and acetone. Optionally, the silicon nanoparticles are dispersed in the organic solvent by stirring. Optionally, the stirring time is 0.1 to 2 hours. In some specific embodiments, the stirring time can be 0.1 hours, 0.5 hours, 1 hour, 1.5 hours or 2 hours.
[0079] S2: placing the expanded graphite into an impregnating agent for vacuum impregnation, so that the silicon nanoparticles are deposited between the layers and on the surface of the expanded graphite to obtain a first intermediate product.
[0080] Vacuum impregnation can successfully embed silicon nanoparticles into the interlayers of expanded graphite while preserving the original morphology of graphite.
[0081] Optionally, the vacuum impregnation time is 0.5 to 8 hours. In some specific embodiments, the vacuum impregnation time can be 0.5 hours, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours or 8 hours.
[0082] Optionally, the mass ratio of expanded graphite to impregnating agent is 1:(1-5). Within this range, the desired content of silicon nanoparticles can be obtained. In some specific embodiments, the mass ratio of expanded graphite to impregnating agent can be 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5 or 1:5.
[0083] S3: subjecting the first intermediate product to ultrasonic treatment to uniformly disperse the silicon nanoparticles deposited between the expanded graphite layers and to remove the silicon nanoparticles deposited on the surface of the expanded graphite, thereby obtaining a second intermediate product.
[0084] Ultrasonic treatment is simple and effective. It can cause collisions between graphites, thereby shaking off and rubbing off silicon nanoparticles deposited on the outer surface of graphite, and making the silicon nanoparticles deposited between graphite layers more evenly dispersed.
[0085] Optionally, the ultrasonic temperature is room temperature, the ultrasonic time is 10 to 120 min, and the ultrasonic power is 60 to 300 kHz. Under the above conditions, the ultrasonic effect is better. In some specific embodiments, the ultrasonic time can be 10 min, 30 min, 50 min, 70 min, 90 min, 100 min, 110 min or 120 min. In some specific embodiments, the ultrasonic power can be 60 kHz, 100 kHz, 150 kHz, 200 kHz, 250 kHz or 300 kHz.
[0086] S4: filtering the second intermediate product, and then freeze-drying the filter residue to obtain a third intermediate product.
[0087] The second intermediate product is filtered to remove most of the solution, and then the filter residue is freeze-dried. Freeze-drying can protect the original structure and shape of the material to the greatest extent, preventing the silicon nanoparticles from aggregating and increasing in volume, thereby causing uncontrollable expansion.
[0088] Optionally, freeze drying the filter residue includes: firstly quick freezing the filter residue in liquid nitrogen, and then placing it in a freeze dryer for freeze drying. Optionally, freeze drying is carried out in a vacuum environment, which can protect the original structure and shape of the material to the greatest extent. Optionally, the freeze drying time is 5 to 24 hours. In some specific embodiments, the freeze drying time can be 5 hours, 7 hours, 9 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours.
[0089] S5: The third intermediate product is surface coated with a polymer precursor to obtain a graphite / silicon composite material.
[0090] In the present application, the polymer precursor includes a conductive agent and a binder, which can not only isolate the contact between silicon and the electrolyte, but also effectively increase the migration rate of lithium ions, thereby improving the charge and discharge efficiency and cycle performance.
[0091] Optionally, this step may specifically include: mixing the third intermediate product with a polymer precursor and water to prepare a slurry, and then spray-drying the slurry so that the polymer precursor is coated on the surface of the third intermediate product.
[0092] Optionally, the solid content of the slurry is 20-30%. In some specific embodiments, the solid content of the slurry may be 20%, 22%, 24%, 26%, 28% or 30%.
[0093] Optionally, the mass ratio of the conductive agent to the binder in the polymer precursor is 1:(20-30). In some specific embodiments, the mass ratio of the conductive agent to the binder may be 1:20, 1:21, 1:22, 1:23, 1:24, 1:25, 1:26, 1:27, 1:28, 1:29 or 1:30.
[0094] Optionally, the mass ratio of the polymer precursor to the third intermediate product is (0.5-1):100. Within this range, the formed coating layer will not be too thick or too thin, which is more conducive to improving the performance of the material. In some specific embodiments, the mass ratio of the polymer precursor to the third intermediate product may be 0.5:100, 0.6:100, 0.7:100, 0.8:100, 0.9:100 or 1:100.
[0095] Alternatively, if Figure 3 As shown, the above method may further include step S0: preparing expanded graphite by using artificial graphite.
[0096] Optionally, artificial graphite is rapidly heated to 800-1200° C. and then kept warm to obtain expanded graphite. At the above temperature, the van der Waals force between graphite layers can be destroyed, so that the volume of graphite expands and the interlayer distance increases.
[0097] Expanded graphite is prepared by increasing the interlayer spacing of graphite through high temperature heat treatment, which can enhance the Li + The diffusion rate inside the graphite accelerates the graphite dynamics. The obtained expanded graphite has high conductivity and excellent dynamic properties.
[0098] Optionally, the heating rate is 10 to 30°C / min, and the holding time is 5 to 60min. In some specific embodiments, the heating rate may be 10°C / min, 12°C / min, 14°C / min, 16°C / min, 18°C / min, 20°C / min, 22°C / min, 24°C / min, 26°C / min, 28°C / min or 30°C / min. In some specific embodiments, the holding time may be 5min, 10min, 20min, 30min, 40min, 50min or 60min.
[0099] Optionally, the interlayer spacing of the expanded graphite is 0.4-1.2 nm. In some specific embodiments, the interlayer spacing of the expanded graphite may be 0.4 nm, 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, 1 nm, 1.1 nm or 1.2 nm.
[0100] Optionally, the median particle size D of the artificial graphite 50 In some specific embodiments, the median particle size D of the artificial graphite is 5 to 15 μm. 50 It can be 5μm, 7μm, 9μm, 11μm, 13μm or 15μm.
[0101] The method provided in the present application embeds silicon nanoparticles between graphite layers by vacuum impregnation, and then performs ultrasonic treatment to cause collisions between graphite particles, so that silicon nanoparticles deposited on the outer surface of graphite are shaken off and rubbed off, and silicon nanoparticles deposited between graphite layers are dispersed more evenly. Next, the organic solvent is removed by filtration and freeze drying, which can effectively prevent the aggregation of silicon nanoparticles. Finally, the prepared material is surface coated, which can further reduce the volume expansion of silicon, weaken the contact between the negative electrode material and the electrolyte, and significantly improve the cycle performance.
[0102] This application combines the high capacity of silicon and the excellent conductivity of graphite, and has the advantages of high energy density, excellent rate performance, high cycle efficiency, etc. It is environmentally friendly and sustainable. This application uses expanded graphite as a skeleton. Expanded graphite with a layered structure can enhance the Li+ The diffusion rate inside the graphite accelerates the graphite dynamics. Silicon nanoparticles are only located between the layers of expanded graphite, but not on the surface, which can effectively inhibit the volume expansion of silicon and improve the low conductivity of silicon. The surface coating can further reduce the volume expansion of silicon, facilitate the rapid transmission of ions and electrons, and weaken the contact between the material and the electrolyte, significantly improving the cycle performance.
[0103] The present application further provides a negative electrode sheet, comprising the above-mentioned graphite / silicon composite material or the graphite / silicon composite material prepared by the above-mentioned preparation method.
[0104] The negative electrode sheet generally includes a negative electrode current collector and a negative electrode film layer disposed on the negative electrode current collector, wherein the negative electrode film layer may include the above-mentioned graphite / silicon composite material.
[0105] The current collector may be a metal foil, such as an aluminum foil, a copper foil, etc., preferably a copper foil. The negative electrode film layer may further include a binder, a conductive agent, etc. The binder may be, for example, styrene-butadiene rubber (SBR), polyvinylidene chloride (PVDF), polyacrylic acid (PAA), sodium carboxymethyl cellulose (CMC-Na), sodium alginate, etc. The conductive agent may be, for example, graphene, carbon nanotubes, Ketjen black, conductive carbon black (SP), etc. Optionally, the negative electrode film layer may further include other additives, such as a dispersant (e.g., carboxymethyl cellulose (CMC)), etc.
[0106] The present application also provides a lithium-ion battery, which includes the above-mentioned negative electrode sheet. The lithium-ion battery also includes a positive electrode sheet, a separator and an electrolyte.
[0107] The lithium-ion battery of the present application is a secondary battery, which refers to a battery that can be used continuously by activating the active material by charging after the battery is discharged. Generally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet to play an isolating role. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet.
[0108] The positive electrode sheet may include a current collector and a positive electrode sheet film layer. The current collector may be a metal foil, such as an aluminum foil, a copper foil, etc. The specific type of active material in the positive electrode sheet film layer is not limited and can be selected according to actual needs. The present application also does not limit the types of diaphragms and electrolytes, which can be selected according to actual needs.
[0109] The lithium-ion battery provided in the present application has excellent properties such as high energy density, excellent rate performance, and high cycle efficiency.
[0110] The present invention will be described below with reference to specific embodiments. The process condition values taken in the following embodiments and comparative examples are exemplary, and their possible numerical ranges are as shown in the aforementioned summary of the invention. For process parameters not particularly noted, conventional techniques can be used. Unless otherwise specified, reagents and instruments used in the technical scheme provided by the present invention can be purchased from conventional channels or the market. It should be noted that, in the absence of conflict, the features in the embodiments in this application and the embodiments can be combined with each other.
[0111] Example 1
[0112] This embodiment prepares a graphite / silicon composite material, and the specific steps are as follows:
[0113] (1) The median particle size D 50 The artificial graphite with a particle size of 10.0-11.0 μm is rapidly heated at 1000° C., with a heating rate of 15° C. / min and a constant temperature time of 30 min to obtain expanded graphite with an interlayer spacing of 0.8-1.2 nm.
[0114] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0115] (3) The impregnating agent and expanded graphite are vacuum impregnated at a mass ratio of 3:1 for 4 hours to obtain a first intermediate product.
[0116] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0117] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 12 hours to obtain a third intermediate product. The freeze dryer operates in a vacuum environment.
[0118] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0119] Example 2
[0120] This embodiment prepares a graphite / silicon composite material, and the specific steps are as follows:
[0121] (1) The median particle size D 50The artificial graphite with a particle size of 7.0 to 8.0 μm is rapidly heated at 900° C., with a heating rate of 10° C. / min and a constant temperature time of 20 min to obtain expanded graphite with an interlayer spacing of 0.8 to 1.2 nm.
[0122] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an isopropanol solution and stirred for 0.3 h to obtain an impregnating agent with a uniform dispersion and a solid content of 6%.
[0123] (3) The impregnating agent and expanded graphite are vacuum impregnated at a mass ratio of 3:1 for 2 hours to obtain a first intermediate product.
[0124] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 30 min and the ultrasound power is 50 kHz, to obtain a second intermediate product.
[0125] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 8 hours to obtain a third intermediate product. The freeze dryer is operated in a vacuum environment.
[0126] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 20%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:20, and the mass ratio of the polymer precursor to the third intermediate product is 0.5:100.
[0127] Example 3
[0128] This embodiment prepares a graphite / silicon composite material, and the specific steps are as follows:
[0129] (1) The median particle size D 50 The artificial graphite with a particle size of 13.0-14.0 μm is rapidly heated at 1100° C., with a heating rate of 20° C. / min and a constant temperature time of 40 min to obtain expanded graphite with an interlayer spacing of 0.8-1.2 nm.
[0130] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an isopropanol solution and stirred for 0.8 h to obtain an impregnating agent with a uniform dispersion and a solid content of 10%.
[0131] (3) The impregnating agent and expanded graphite are vacuum impregnated at a mass ratio of 3:1 for 6 hours to obtain a first intermediate product.
[0132] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 90 min and the ultrasound power is 160 kHz, to obtain a second intermediate product.
[0133] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 16 hours to obtain a third intermediate product. The freeze dryer is operated in a vacuum environment.
[0134] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 30%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:30, and the mass ratio of the polymer precursor to the third intermediate product is 1:100.
[0135] Example 4
[0136] This embodiment prepares a graphite / silicon composite material, and the specific steps are as follows:
[0137] (1) The median particle size D 50 The artificial graphite with a particle size of 5.0 to 6.0 μm is rapidly heated at 1000° C., with a heating rate of 15° C. / min and a constant temperature time of 30 min to obtain expanded graphite with an interlayer spacing of 0.8 to 1.2 nm.
[0138] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0139] (3) The impregnating agent and expanded graphite are vacuum impregnated at a mass ratio of 3:1 for 4 hours to obtain a first intermediate product.
[0140] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0141] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 12 hours to obtain a third intermediate product. The freeze dryer operates in a vacuum environment.
[0142] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0143] Example 5
[0144] This embodiment prepares a graphite / silicon composite material, and the specific steps are as follows:
[0145] (1) The median particle size D 50 The artificial graphite with a particle size of 10.0-11.0 μm is rapidly heated at 1000° C., with a heating rate of 15° C. / min and a constant temperature time of 30 min to obtain expanded graphite with an interlayer spacing of 0.8-1.2 nm.
[0146] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 25%.
[0147] (3) The impregnating agent and expanded graphite are vacuum impregnated at a mass ratio of 3:1 for 4 hours to obtain a first intermediate product.
[0148] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0149] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 12 hours to obtain a third intermediate product. The freeze dryer operates in a vacuum environment.
[0150] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0151] Example 6
[0152] This embodiment prepares a graphite / silicon composite material, and the specific steps are as follows:
[0153] (1) The median particle size D 50The artificial graphite with a particle size of 10.0-11.0 μm is rapidly heated at 1000° C., with a heating rate of 15° C. / min and a constant temperature time of 30 min to obtain expanded graphite with an interlayer spacing of 0.8-1.2 nm.
[0154] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0155] (3) The impregnating agent and expanded graphite are vacuum impregnated at a mass ratio of 1:1 for 4 hours to obtain a first intermediate product.
[0156] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0157] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 12 hours to obtain a third intermediate product. The freeze dryer operates in a vacuum environment.
[0158] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0159] Example 7
[0160] This embodiment prepares a graphite / silicon composite material, and the specific steps are as follows:
[0161] (1) The median particle size D 50 The artificial graphite with a particle size of 10.0-11.0 μm is rapidly heated at 1000° C., with a heating rate of 15° C. / min and a constant temperature time of 30 min to obtain expanded graphite with an interlayer spacing of 0.8-1.2 nm.
[0162] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0163] (3) Vacuum impregnating the impregnating agent and expanded graphite at a mass ratio of 3:1 for 0.5 h to obtain a first intermediate product.
[0164] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0165] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 12 hours to obtain a third intermediate product. The freeze dryer operates in a vacuum environment.
[0166] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0167] Example 8
[0168] This embodiment prepares a graphite / silicon composite material, and the specific steps are as follows:
[0169] (1) The median particle size D 50 The artificial graphite with a particle size of 10.0-11.0 μm is rapidly heated at 1000° C., with a heating rate of 15° C. / min and a constant temperature time of 30 min to obtain expanded graphite with an interlayer spacing of 0.8-1.2 nm.
[0170] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0171] (3) The impregnating agent and expanded graphite are vacuum impregnated at a mass ratio of 3:1 for 4 hours to obtain a first intermediate product.
[0172] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0173] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 5 hours to obtain a third intermediate product. The freeze dryer is operated in a vacuum environment.
[0174] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0175] Comparative Example 1
[0176] This comparative example prepares a graphite / silicon composite material, and the specific steps are as follows:
[0177] (1) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0178] (2) Vacuum impregnating the impregnating agent and artificial graphite at a mass ratio of 3:1 for 4 hours to obtain a first intermediate product. 50 It is 10.0~11.0μm.
[0179] (3) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0180] (4) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 12 hours to obtain a third intermediate product. The freeze dryer is operated in a vacuum environment.
[0181] (5) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0182] Comparative Example 2
[0183] This comparative example prepares a graphite / silicon composite material, and the specific steps are as follows:
[0184] (1) The median particle size D 50 The artificial graphite with a size of 10.0 to 11.0 μm was rapidly heated at 1000° C., with a heating rate of 5° C. / min and a constant temperature time of 30 min.
[0185] (2) The median particle size D 50Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0186] (3) Vacuum impregnating the impregnating agent and the graphite treated in step (1) at a mass ratio of 3:1 for 4 hours to obtain a first intermediate product.
[0187] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0188] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 12 hours to obtain a third intermediate product. The freeze dryer operates in a vacuum environment.
[0189] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0190] Comparative Example 3
[0191] This comparative example prepares a graphite / silicon composite material, and the specific steps are as follows:
[0192] (1) The median particle size D 50 The artificial graphite with a particle size of 10.0-11.0 μm is rapidly heated at 1000° C., with a heating rate of 15° C. / min and a constant temperature time of 30 min to obtain expanded graphite with an interlayer spacing of 0.8-1.2 nm.
[0193] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0194] (3) The impregnating agent and expanded graphite were naturally impregnated at a mass ratio of 3:1 under stirring for 4 hours to obtain a first intermediate product.
[0195] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0196] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 12 hours to obtain a third intermediate product. The freeze dryer operates in a vacuum environment.
[0197] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0198] Comparative Example 4
[0199] This comparative example prepares a graphite / silicon composite material, and the specific steps are as follows:
[0200] (1) The median particle size D 50 The artificial graphite with a particle size of 10.0-11.0 μm is rapidly heated at 1000° C., with a heating rate of 15° C. / min and a constant temperature time of 30 min to obtain expanded graphite with an interlayer spacing of 0.8-1.2 nm.
[0201] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0202] (3) The impregnating agent and expanded graphite are vacuum impregnated at a mass ratio of 3:1 for 4 hours to obtain a first intermediate product.
[0203] (4) The first intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 12 hours to obtain a second intermediate product. The freeze dryer is operated in a vacuum environment.
[0204] (6) The second intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0205] Comparative Example 5
[0206] This comparative example prepares a graphite / silicon composite material, and the specific steps are as follows:
[0207] (1) The median particle size D 50The artificial graphite with a particle size of 10.0-11.0 μm is rapidly heated at 1000° C., with a heating rate of 15° C. / min and a constant temperature time of 30 min to obtain expanded graphite with an interlayer spacing of 0.8-1.2 nm.
[0208] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0209] (3) The impregnating agent and expanded graphite are vacuum impregnated at a mass ratio of 3:1 for 4 hours to obtain a first intermediate product.
[0210] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0211] (5) The second intermediate product was filtered to remove most of the solution, and then dried in a vacuum drying oven for 12 hours to obtain a third intermediate product.
[0212] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0213] Comparative Example 6
[0214] This comparative example prepares a graphite / silicon composite material, and the specific steps are as follows:
[0215] (1) The median particle size D 50 The artificial graphite with a particle size of 10.0-11.0 μm is rapidly heated at 1000° C., with a heating rate of 15° C. / min and a constant temperature time of 30 min to obtain expanded graphite with an interlayer spacing of 0.8-1.2 nm.
[0216] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0217] (3) The impregnating agent and expanded graphite are vacuum impregnated at a mass ratio of 3:1 for 4 hours to obtain a first intermediate product.
[0218] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0219] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 12 hours to obtain the final product. The freeze dryer operates in a vacuum environment.
[0220] Comparative Example 7
[0221] This comparative example prepares a graphite / silicon composite material, and the specific steps are as follows:
[0222] (1) The median particle size D 50 The artificial graphite with a particle size of 10.0-11.0 μm is rapidly heated at 1000° C., with a heating rate of 15° C. / min and a constant temperature time of 30 min to obtain expanded graphite with an interlayer spacing of 0.8-1.2 nm.
[0223] (2) The median particle size D 50 Nano-silicon with a size of 1.3 to 2.0 nm is dispersed in an ethanol solution and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0224] (3) The impregnating agent and expanded graphite are vacuum impregnated at a mass ratio of 3:1 for 4 hours to obtain a first intermediate product.
[0225] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0226] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 12 hours to obtain a third intermediate product. The freeze dryer operates in a vacuum environment.
[0227] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0228] Comparative Example 8
[0229] This comparative example prepares a graphite / silicon composite material, and the specific steps are as follows:
[0230] (1) The median particle size D 50 The artificial graphite with a particle size of 10.0-11.0 μm is rapidly heated at 1000° C., with a heating rate of 15° C. / min and a constant temperature time of 30 min to obtain expanded graphite with an interlayer spacing of 0.8-1.2 nm.
[0231] (2) The median particle size D 50 Nano-silicon with a size of 0.5 to 0.8 nm is dispersed in water and stirred for 0.5 h to obtain an impregnating agent with a uniform dispersion and a solid content of 8%.
[0232] (3) The impregnating agent and expanded graphite are vacuum impregnated at a mass ratio of 3:1 for 4 hours to obtain a first intermediate product.
[0233] (4) The first intermediate product is subjected to ultrasound at room temperature, wherein the ultrasound time is 60 min and the ultrasound power is 120 kHz, to obtain a second intermediate product.
[0234] (5) The second intermediate product is filtered to remove most of the solution, then quickly frozen in liquid nitrogen, and placed in a freeze dryer for freeze drying for 12 hours to obtain a third intermediate product. The freeze dryer operates in a vacuum environment.
[0235] (6) The third intermediate product, the polymer precursor and pure water are uniformly mixed to obtain a slurry. The slurry is spray-dried to obtain a final product. The solid content of the slurry is 25%, the polymer precursor is composed of single-walled carbon nanotubes and lithium polyacrylate, the mass ratio of single-walled carbon nanotubes to lithium polyacrylate is 1:25, and the mass ratio of the polymer precursor to the third intermediate product is 0.8:100.
[0236] Test Example 1
[0237] Test samples: graphite / silicon composite materials provided in Examples 1 to 8, and composite materials provided in Comparative Examples 1 to 8.
[0238] Carbon content testing instrument: resistance muffle furnace SX-8-10.
[0239] Silicon content test method: magnetic material digestion method.
[0240] Particle size (D 50 )Testing instrument: Malvern, Master Size 3000.
[0241] The specific test results are shown in Table 1 below:
[0242] Table 1
[0243]
[0244] Test Example 2
[0245] Test samples: graphite / silicon composite materials provided in Examples 1 to 8, and composite materials provided in Comparative Examples 1 to 8.
[0246] Test method: The prepared graphite negative electrode material is prepared into a pole piece, specifically:
[0247] The above samples were mixed with conductive agent carbon black (Surper P) and CMC (carboxymethyl cellulose) binder at a mass ratio of 97:2:1 to obtain slurry, which was then coated on copper foil to form a negative electrode sheet. The prepared negative electrode sheet and lithium metal sheet were assembled into a lithium-ion button battery, and LiPF6 was dissolved in an electrolyte of ethylene carbonate / diethyl carbonate / ethyl methyl carbonate = 2:3:1 at a concentration of 1 mol / L. After the button battery assembly was completed, the capacity, rate performance and cycle performance tests were performed, as shown below:
[0248] (a) 0.1C discharge specific capacity test steps: ① stand for 5h; ② 0.05C discharge to 0.005V; ③ 0.05mA constant current discharge to 0.005V; ④ stand for 5min; ⑤ 0.01mA constant current discharge to 0.005V; ⑥ stand for 5min; ⑦ 0.1C charge to 2V; ⑧ stand for 5min;
[0249] (b) 2C discharge specific capacity test steps: ① stand for 5h; ② 0.05C discharge to 0.005V; ③ 0.05mA constant current discharge to 0.005V; ④ stand for 5min; ⑤ 0.01mA constant current discharge to 0.005V; ⑥ stand for 5min; ⑦ 0.1C charge to 2V; ⑧ stand for 5min; ⑨ 2C discharge to 0.005V, ⑩ stand for 30min; 0.1C discharge to 0.005V, Let stand for 30 minutes; 0.05C discharge to 0.005V Let stand for 30 minutes; 2C charging to 2V
[0250] (c) 5C discharge specific capacity test steps: ① stand for 5h; ② 0.05C discharge to 0.005V; ③ 0.05mA constant current discharge to 0.005V; ④ stand for 5min; ⑤ 0.01mA constant current discharge to 0.005V; ⑥ stand for 5min; ⑦ 0.1C charge to 2V; ⑧ stand for 5min; ⑨ 5C discharge to 0.005V, ⑩ stand for 30min; 0.1C discharge to 0.005V, Let stand for 30 minutes; 0.05C discharge to 0.005V Let stand for 30 minutes; 5C charging to 2V
[0251] (d) 0.1C 200-cycle capacity retention rate test procedure: Same as the 0.1C discharge specific capacity test procedure, set the program to cycle 200 times before stopping, and compare its capacity retention rate.
[0252] Data processing: Select 4 data with a range within 3mAh, remove the maximum and minimum data and calculate the average.
[0253] The specific test results are shown in Table 2 below:
[0254] Table 2
[0255]
[0256] As can be seen from the above, the lithium ion battery provided by the present application has excellent performances such as high energy density, excellent rate performance, and high cycle efficiency. In Comparative Example 1, when artificial graphite that has not been expanded is directly used, the silicon nanoparticles cannot enter between the graphite layers, so the performance of the obtained material is not good. . In Comparative Example 2, the heating rate is too slow, the expansion effect of graphite is poor, and therefore the silicon nanoparticles are less precipitated. In Comparative Example 3, vacuum impregnation is not used, and the deposition effect of silicon nanoparticles is also poor. In Comparative Example 4, ultrasound is not performed, the silicon nanoparticles on the surface of the expanded graphite are not removed, and the silicon nanoparticles between the expanded graphite layers are also unevenly distributed. In Comparative Example 5, the silicon nanoparticles are easily agglomerated together, which causes the aggregate volume to increase and brings about an uncontrollable expansion effect. In Comparative Example 6, the polymer precursor is not coated, the negative electrode material is directly in contact with the electrolyte, and the material performance deteriorates. In Comparative Example 7, the silicon nanoparticles used have a large particle size and cannot be effectively deposited between the layers of the expanded graphite, so the performance of the resulting negative electrode material is poor. In Comparative Example 8, water-dispersed silicon nanoparticles were used. The silicon nanoparticles were easily agglomerated in water, so the performance of the obtained negative electrode material was not very good.
[0257] Obviously, the above embodiments are merely examples for clearly explaining the present invention, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the protection scope of the present invention.
Claims
1. A graphite / silicon composite material, It is characterized in that include: Expanded graphite; Silicon nanoparticles, located between the layers of the expanded graphite; as well as A coating layer, coating the surface of the expanded graphite; Wherein, the coating layer includes a conductive agent and a binder.
2. The graphite / silicon composite material according to claim 1, It is characterized in that The graphite / silicon composite material meets at least one of the following conditions: a) the content of silicon in the graphite / silicon composite material is 0.2-30wt%, and the content of carbon is 70-99.8wt%; b) median particle size D of the graphite / silicon composite material 50 5~15μm; c) the interlayer spacing of the expanded graphite is 0.4 to 1.2 nm; d) The median particle size D of the silicon nanoparticles 50 0.5~1.2nm; e) the coating layer has a thickness of 0.01 to 100 nm; f) the conductive agent is selected from one or more of carbon black, conductive carbon fiber, graphene and carbon nanotubes; g) the binder is a polyacrylic acid series binder; h) The mass ratio of the conductive agent to the binder in the coating layer is 1:(20-30).
3. A method for preparing a graphite / silicon composite material, It is characterized in that The following steps are involved: S1: dispersing silicon nanoparticles in an organic solvent to obtain an impregnating agent; S2: placing the expanded graphite into the impregnating agent for vacuum impregnation, so that the silicon nanoparticles are deposited between the layers and on the surface of the expanded graphite to obtain a first intermediate product; S3: subjecting the first intermediate product to ultrasonic treatment to uniformly disperse the silicon nanoparticles deposited between the expanded graphite layers, and removing the silicon nanoparticles deposited on the surface of the expanded graphite to obtain a second intermediate product; S4: filtering the second intermediate product, and then freeze-drying the filter residue to obtain a third intermediate product; as well as S5: using a polymer precursor to coat the surface of the third intermediate product to obtain the graphite / silicon composite material; wherein the polymer precursor includes a conductive agent and a binder.
4. The preparation method according to claim 3, It is characterized in that The following steps are also included: S0: preparing the expanded graphite by using artificial graphite; Optionally, the interlayer spacing of the expanded graphite is 0.4 to 1.2 nm; Optionally, the median particle size D of the artificial graphite 50 5~15μm; Optionally, the artificial graphite is rapidly heated to 800-1200° C. and then kept warm, thereby obtaining the expanded graphite; further optionally, the heating rate is 10-30° C. / min, and the keeping time is 5-60 min.
5. The preparation method according to claim 3, It is characterized in that In step S1, the solid content of the impregnating agent is 5 to 25%; Optionally, the median particle size D of the silicon nanoparticles is 50 0.5~1.2nm; Optionally, the organic solvent is selected from one or more of ethanol, isopropanol, n-propanol and acetone; Optionally, the silicon nanoparticles are dispersed in the organic solvent by stirring, and further optionally, the stirring time is 0.1 to 2 hours.
6. The preparation method according to claim 3, It is characterized in that In step S2, the vacuum impregnation time is 0.5 to 8 hours; Optionally, the mass ratio of the expanded graphite to the impregnating agent is 1:(1-5).
7. The preparation method according to claim 3, It is characterized in that In step S3, the ultrasonic temperature is room temperature, the ultrasonic time is 10 to 120 minutes, and the ultrasonic power is 60 to 300 kHz; Optionally, in step S4, freeze-drying the filter residue includes: firstly quick-freezing the filter residue in liquid nitrogen, and then placing it in a freeze dryer for freeze-drying; further optionally, the freeze-drying is carried out in a vacuum environment, and the freeze-drying time is 5 to 24 hours.
8. The preparation method according to claim 3, It is characterized in that In step S5, the third intermediate product is mixed with the polymer precursor and water to prepare a slurry, and then spray-dried, so that the polymer precursor is coated on the surface of the third intermediate product; Optionally, the solid content of the slurry is 20-30%; Optionally, the mass ratio of the conductive agent to the binder in the polymer precursor is 1:(20-30); Optionally, the mass ratio of the polymer precursor to the third intermediate product is (0.5-1):
100.
9. A negative electrode sheet, It is characterized in that The invention comprises the graphite / silicon composite material as claimed in claim 1 or 2, or the graphite / silicon composite material prepared by the preparation method as claimed in any one of claims 3 to 8.
10. A lithium ion battery, It is characterized in that Including the negative electrode sheet as claimed in claim 9.
Citation Information
Patent Citations
Preparation method of high power capacity lithium ion battery cathode material
CN102769139A
Silicon-based negative electrode material, preparation method thereof and application of silicon-based negative electrode material in lithium-ion battery
CN108054368A
Silicon carbon composite material and preparation method and application thereof
CN110289412A
Silicon-carbon negative electrode material, preparation method and lithium ion battery
CN110739455A
Expanded graphite nano-silicon composite negative electrode material for lithium ion battery and preparation method of expanded graphite nano-silicon composite negative electrode material
CN114497476A