High-power silicon-carbon composite material and preparation method thereof

By doping lithium and deposition of amorphous carbon in silicon-carbon composite materials, and coating fast ion conductors by atomic vapor deposition, the problems of poor rate performance and low tap density of traditional silicon-carbon composite materials are solved, which significantly improves its Application performance in lithium-ion batteries.

CN119050319APending Publication Date: 2024-11-29SICHUAN KUNTIAN NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411243448.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The poor rate performance and low tap density of traditional silicon-carbon composite materials have resulted in poor application performance in high-energy density lithium-ion batteries.

Method used

Li-doped porous silicon is prepared by mixing silicon powder, silica and lithium carboxymethylcellulose, and metallic lithium and amorphous carbon are deposited on its surface, followed by rapid coating by atomic vapor deposition method Ion conductors, improving the electronic conductivity and density of materials.

Benefits of technology

It significantly improves the rate performance and tap density of silicon-carbon composite materials, reduces the powder resistivity and core defects of the material, and improves its fast charging performance and cycle stability in lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050319A_ABST
    Figure CN119050319A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion battery material preparation, and provides a high-power silicon-carbon composite material and a preparation method thereof.The preparation method of the high-power silicon-carbon composite material comprises the following steps that S1, silicon powder, silicon dioxide and carboxymethylcellulose lithium are mixed, carbonized and etched, and lithium-doped porous silicon is obtained; s2, introducing mixed gas into the lithium-doped porous silicon, and performing first deposition to obtain an intermediate material; s3, depositing a fast ion conductor on the surface of the intermediate material for the second time to obtain a silicon-carbon composite material; the mixed gas comprises lithium source gas and carbon source gas. According to the technical scheme, the problems of poor rate capability and low tap density of the silicon-carbon composite material in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery material preparation, and in particular to a high-power silicon-carbon composite material and a preparation method thereof. Background Art

[0002] The new silicon-carbon material is a new silicon-based material. It can be used as a negative electrode material in high energy density lithium-ion batteries because of its advantages such as high specific capacity, low expansion and good cycle performance. Traditional silicon-carbon materials are usually composed of porous carbon and nano-silicon, and nano-silicon is easily deposited in the pores of porous carbon, causing the overall electronic conductivity of the silicon-carbon material to deviate, thereby reducing its fast charging performance. Although the rate performance of silicon-carbon materials can be improved by doping and coating them, the poor electronic conductivity of porous carbon itself and its high contact with nano-silicon result in a large interface impedance of the silicon-carbon material, poor rate performance and low tap density. Therefore, it is of great significance to develop a high-power silicon-carbon composite material with good rate performance and high tap density. Summary of the invention

[0003] The present invention provides a high-power silicon-carbon composite material and a preparation method thereof, which solves the problems of poor rate performance and low tap density of the silicon-carbon composite material in the related art.

[0004] The technical solution of the present invention is as follows: The present invention provides a method for preparing a high-power silicon-carbon composite material, comprising the following steps: S1, mixing silicon powder, silicon dioxide and lithium carboxymethyl cellulose, carbonizing and etching to obtain lithium-doped porous silicon; S2, introducing a mixed gas into the lithium-doped porous silicon, performing a first deposition, and obtaining an intermediate material; S3, after a second deposition of a fast ion conductor on the surface of the intermediate material, obtaining a silicon-carbon composite material; The mixed gas includes a lithium source gas and a carbon source gas.

[0005] As a further technical solution, in step S1, the mass ratio of the silicon powder, silicon dioxide and lithium carboxymethyl cellulose is 10-12:20:1-5.

[0006] When the mass ratio of silicon powder, silicon dioxide and lithium carboxymethyl cellulose is 10~12:20:1~5, the rate performance and tap density of the silicon-carbon composite material can be improved.

[0007] As a further technical solution, in step S1, during the carbonization, the temperature is 500-800°C and the time is 1-6 hours; during the etching, hydrogen fluoride gas is used with a flow rate of 100-500 SCCM and the etching time is 1-3 hours.

[0008] As a further technical solution, the volume ratio of the lithium source gas to the carbon source gas is 1~3:10.

[0009] When the volume ratio of lithium source gas to carbon source gas is 1-3:10, the rate performance and tap density of the silicon-carbon composite material can be further improved.

[0010] As a further technical solution, the lithium source gas is one of methyl lithium, ethyl lithium, and propyl lithium; the carbon source gas is one of methane, ethane, ethylene, and acetylene.

[0011] As a further technical solution, in step S2, the flow rate of the mixed gas is 50~200 SCCM; during the first deposition, the vacuum is evacuated to 0.1~1 MPa, the temperature is 500~1000°C, and the deposition time is 30~300 min.

[0012] As a further technical solution, in step S3, the fast ion conductor is a lithium oxide fast ion conductor.

[0013] As a further technical solution, the lithium oxide fast ion conductor is one of LiLaO2, LiSeO2, LiNbO2, and LiCeO2.

[0014] As a further technical solution, in step S3, during the second deposition, an atomic vapor deposition method is used, and the deposition time is 10 to 60 minutes.

[0015] By using atomic vapor deposition to coat the surface of the intermediate material with a fast ion conductor, the rate performance and tap density of the silicon-carbon composite material can be further improved.

[0016] The present invention also provides a high-power silicon-carbon composite material, which is prepared by the preparation method of the high-power silicon-carbon composite material.

[0017] The working principle and beneficial effects of the present invention are: 1. In the present invention, lithium-doped porous silicon is prepared by carbonizing and etching silicon powder, silicon dioxide and lithium carboxymethyl cellulose at high temperature. By doping lithium into the porous silicon, the impedance is reduced while reducing the defects in the core of the silicon-carbon composite material, thereby improving the rate performance and tap density of the silicon-carbon composite material.

[0018] 2. In the present invention, by depositing metallic lithium and amorphous carbon in lithium-doped porous silicon, the pores of the lithium-doped porous silicon material are reduced, and the resistivity of the powder is reduced, thereby improving the rate performance and tap density of the silicon-carbon composite material.

[0019] 3. In the present invention, the atomic vapor deposition method is used to coat the fast ion conductor on the surface of the intermediate material, which has the advantages of high density and uniform deposition, can reduce the defects of the core of the silicon-carbon composite material, and improve the ionic conductivity of the silicon-carbon composite material, thereby improving the rate performance and tap density of the silicon-carbon composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0021] Figure 1 This is a SEM image of the silicon-carbon composite material prepared in Example 1; The silicon-carbon composite material in the figure presents a granular structure with a particle size ranging from 5 to 10 μm. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1 A method for preparing a high-power silicon-carbon composite material comprises the following steps: S1, 11g silicon powder, 20g silicon dioxide and 3g lithium carboxymethyl cellulose were mixed, carbonized at 600°C for 3h, hydrogen fluoride gas was introduced at a flow rate of 300SCCM, etched for 2h, and washed with deionized water to obtain lithium-doped porous silicon; S2, introducing a mixed gas of methyl lithium and methane with a volume ratio of 2:10 into the lithium-doped porous silicon at a flow rate of 100 SCCM, evacuating to 0.5 MPa, and depositing at 800° C. for 150 min to obtain an intermediate material; S3, by atomic vapor deposition, the intermediate material is transferred into the plasma vacuum chamber and pressed onto the surface of the rotating shaft, and the chamber is evacuated to 5×10 -4 Pa, and a mixed gas of argon and oxygen is introduced, with bulk LiLaO2 as the target, the distance between the target and the rotating axis is 15 cm, the power applied to the cathode is 12 kW, the rotation speed of the rotating axis is 3 m / s, and the LiLaO2 fast ion conductor is deposited on the surface of the intermediate material for 30 minutes through low-pressure plasma discharge to obtain a silicon-carbon composite material; The SEM image of the silicon-carbon composite material prepared in this embodiment is as follows: Figure 1 shown.

[0024] Example 2 A method for preparing a high-power silicon-carbon composite material comprises the following steps: S1, 10g silicon powder, 20g silicon dioxide and 1g lithium carboxymethyl cellulose were mixed, carbonized at 500°C for 6h, hydrogen fluoride gas was introduced at a flow rate of 500SCCM, etched for 1h, and washed with deionized water to obtain lithium-doped porous silicon; S2, introducing a mixed gas of ethyl lithium and ethylene in a volume ratio of 1:10 into the lithium-doped porous silicon at a flow rate of 100 SCCM, evacuating to 0.1 MPa, and depositing at 500° C. for 300 min to obtain an intermediate material; S3, by atomic vapor deposition, the intermediate material is transferred into the plasma vacuum chamber and pressed onto the surface of the rotating shaft, and the chamber is evacuated to 1×10 -4 Pa, and a mixed gas of argon and oxygen is introduced, block LiSeO2 is used as the target, the distance between the target and the rotation axis is 10 cm, the power applied to the cathode is 10 kW, the rotation rate of the rotation axis is 1 m / s, and the LiSeO2 fast ion conductor is deposited on the surface of the intermediate material for 60 minutes through low-pressure plasma discharge to obtain a silicon-carbon composite material.

[0025] Example 3 A method for preparing a high-power silicon-carbon composite material comprises the following steps: S1, 12g silicon powder, 20g silicon dioxide and 5g lithium carboxymethyl cellulose were mixed, carbonized at 800°C for 1h, hydrogen fluoride gas was introduced at a flow rate of 100SCCM, etching was performed for 3h, and deionized water was washed to obtain lithium-doped porous silicon; S2, introducing a mixed gas of ethyl lithium and ethylene in a volume ratio of 3:10 into lithium-doped porous silicon at a flow rate of 100 SCCM, evacuating to 1 MPa, and depositing at 1000° C. for 30 min to obtain an intermediate material; S3, by atomic vapor deposition, the intermediate material is transferred into the plasma vacuum chamber and pressed onto the surface of the rotating shaft, and the chamber is evacuated to 10×10 -4 Pa, and a mixed gas of argon and oxygen is introduced, block LiCeO2 is used as the target, the distance between the target and the rotation axis is 20 cm, the power applied to the cathode is 15 kW, the rotation rate of the rotation axis is 5 m / s, and the LiCeO2 fast ion conductor is deposited on the surface of the intermediate material for 10 minutes through low-pressure plasma discharge to obtain a silicon-carbon composite material.

[0026] Comparative Example 1 A method for preparing a high-power silicon-carbon composite material comprises the following steps: S1, 11g silicon powder, 20g silicon dioxide and 3g lithium carboxymethyl cellulose were mixed, carbonized at 600°C for 3h, hydrogen fluoride gas was introduced at a flow rate of 300SCCM, etched for 2h, and washed with deionized water to obtain lithium-doped porous silicon; S2. A mixed gas of methyl lithium and methane with a volume ratio of 2:10 was introduced into the lithium-doped porous silicon at a flow rate of 100 SCCM, the vacuum was evacuated to 0.5 MPa, and the mixture was deposited at 800° C. for 150 min to obtain a silicon-carbon composite material.

[0027] Comparative Example 2 The difference between this comparative example and Example 1 is that in step S2, the gas introduced does not include methyl lithium but only includes methane.

[0028] Comparative Example 3 The difference between this comparative example and Example 1 is that in step S2, the gas introduced does not include methane but only includes methyl lithium.

[0029] Comparative Example 4 A method for preparing a high-power silicon-carbon composite material comprises the following steps: S1, 11g silicon powder, 20g silicon dioxide and 3g lithium carboxymethyl cellulose were mixed, carbonized at 600°C for 3h, hydrogen fluoride gas was introduced at a flow rate of 300SCCM, etched for 2h, and washed with deionized water to obtain lithium-doped porous silicon; S2. Li-doped porous silicon was transferred into a plasma vacuum chamber by atomic vapor deposition and pressed onto the surface of the rotating shaft. The chamber was evacuated to 5×10 -4 Pa, and a mixed gas of argon and oxygen is introduced, block LiLaO2 is used as the target, the distance between the target and the rotation axis is 15 cm, the power applied to the cathode is 12 kW, the rotation rate of the rotation axis is 3 m / s, and the LiLaO2 fast ion conductor is deposited on the surface of the intermediate material for 30 minutes through low-pressure plasma discharge to obtain a silicon-carbon composite material.

[0030] The silicon-carbon composite materials prepared by the preparation methods of Examples 1 to 3 and Comparative Examples 1 to 4 were subjected to the following performance tests: The silicon-carbon composite materials prepared by the preparation methods of Examples 1 to 3 and Comparative Examples 1 to 4 were tested for specific surface area and tap density in accordance with the national standard GB / T38823-2020 "Silicon Carbon", and the powder resistivity was tested using a four-probe tester (model PY68200A); the test results are shown in Table 1 below.

[0031] Table 1 Test results

[0032] In Table 1, compared with Comparative Example 1, the silicon-carbon composite material of Example 1 has a high specific surface area and a high tap density, and a low powder resistivity, indicating that the rate performance and tap density of the silicon-carbon composite material can be improved by coating the surface of the silicon-carbon composite material with a lithium oxide fast ion conductor using an atomic vapor deposition method. Compared with Comparative Examples 2 to 4, the silicon-carbon composite material of Example 1 has a high specific surface area and a high tap density, and a low powder resistivity, indicating that depositing metallic lithium and amorphous carbon in lithium-doped porous silicon can improve the rate performance and tap density of the silicon-carbon composite material.

[0033] Experimental Example 1 Button battery performance test: Preparation of button cells: The silicon-carbon composite material prepared by the preparation methods of Examples 1 to 3 and Comparative Examples 1 to 4 is used as a negative electrode material for a lithium-ion battery, and the lithium-ion battery is a button cell. The preparation method of the button cell comprises the following steps: adding 4 g of a binder, 1 g of a conductive agent and 220 mL of a solvent to 95 g of the silicon-carbon composite material, stirring and slurrying, coating the mixture on a copper foil, drying and rolling to obtain a negative electrode sheet, and then assembling the button cell in an argon-filled glove box; wherein the binder is LA132, the conductive agent is conductive carbon black, and the solvent is NMP; The electrochemical performance of button cells was tested on a Wuhan Blue Electric CT2001A battery tester, where the charge and discharge voltage range was 0.005~2.0V and the charge and discharge rate was 0.1C. After the negative electrode sheet of the button cell is fully charged and expanded, the thickness D1 of the negative electrode sheet of the button cell after rolling is tested, and then the full-charge thickness D2 of the negative electrode sheet is dissected when the button cell is fully charged to 100% SOC, and the full-charge expansion rate is calculated according to the following formula; Full-charge expansion rate = (D2-D1) / D1×100%; The button cell performance test results are shown in Table 2 below.

[0034] Table 2 Button battery performance test results

[0035] In Table 2, compared with Comparative Example 1, the first discharge specific capacity and first efficiency of the button cell of Example 1 are high, and the full charge expansion rate is low, indicating that the use of atomic vapor deposition to coat the surface of the silicon-carbon composite material with a lithium oxide fast ion conductor can reduce the irreversible capacity of the silicon-carbon composite material and improve the first efficiency. Compared with Comparative Examples 3-4, the first discharge specific capacity and first efficiency of the button cell of Example 1 are high, and the full charge expansion rate is low, indicating that depositing metallic lithium and amorphous carbon in lithium-doped porous silicon reduces the powder resistivity, thereby reducing the irreversible capacity of the silicon-carbon composite material and improving the first efficiency.

[0036] Experimental Example 2 Soft pack performance test: Preparation of soft-pack battery: The silicon-carbon composite material prepared by the preparation method of Examples 1 to 3 and Comparative Examples 1 to 4 was doped with 90% artificial graphite as the negative electrode material, and assembled with the positive electrode ternary material, electrolyte and separator into a 5Ah soft-pack battery; wherein the positive electrode ternary material is LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2; the diaphragm is celegard 2400; the electrolyte is a LiPF6 solution with a concentration of 1.3 mol / L, and the LiPF6 solution is a mixed solution of EC and DEC with a volume ratio of 1:1; The following performance tests are performed on soft pack batteries: 1. Liquid absorption capacity test: Use a 1mL burette and absorb 1mL of electrolyte, add one drop on the surface of each negative electrode sheet, and count until the electrolyte is completely absorbed. Record the time t, which is the liquid absorption speed; 2. Rate test: Use 0.5C / 1C / 2C to test the constant current ratio of its soft pack battery; 3. Cycle performance test: The soft pack battery is subjected to cycle performance test. During the cycle performance test, the charge and discharge voltage range is 2.5-4.2V, the temperature is 25±3.0℃, the charge and discharge rate is 1.0C / 1.0C, and the cycle number is 500 times; The soft pack performance test results are shown in Table 3 below.

[0037] Table 3 Soft pack performance test results

[0038] In Table 3, compared with Comparative Examples 1 to 4, the soft-pack lithium-ion batteries prepared from the silicon-carbon composite materials of Examples 1 to 3 have high rate performance, good cycle performance, and fast liquid absorption speed. The reason is that the silicon-carbon composite materials of Examples 1 to 3 have a high specific surface area, which can improve their liquid absorption capacity; the silicon-carbon composite materials of Examples 1 to 3 have a low powder resistivity, which can improve their cross-flow ratio; the silicon-carbon composite materials of Examples 1 to 3 have a low full-charge expansion rate, which can improve their cycle performance.

[0039] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-power silicon-carbon composite material, characterized in that: The following steps are involved: S1, mixing silicon powder, silicon dioxide and lithium carboxymethyl cellulose, carbonizing and etching to obtain lithium-doped porous silicon; S2, introducing a mixed gas into the lithium-doped porous silicon, performing a first deposition, and obtaining an intermediate material; S3, after a second deposition of a fast ion conductor on the surface of the intermediate material, obtaining a silicon-carbon composite material; The mixed gas includes a lithium source gas and a carbon source gas.

2. The method for preparing a high-power silicon-carbon composite material according to claim 1, characterized in that: In step S1, the mass ratio of the silicon powder, silicon dioxide and lithium carboxymethyl cellulose is 10-12:20:1-5.

3. The method for preparing a high-power silicon-carbon composite material according to claim 1, characterized in that: In step S1, during the carbonization, the temperature is 500-800° C. and the time is 1-6 hours; during the etching, hydrogen fluoride gas is used with a flow rate of 100-500 SCCM and the etching time is 1-3 hours.

4. The method for preparing a high-power silicon-carbon composite material according to claim 1, characterized in that: The volume ratio of the lithium source gas to the carbon source gas is 1-3:

10.

5. The method for preparing a high-power silicon-carbon composite material according to claim 1, characterized in that: The lithium source gas is one of methyl lithium, ethyl lithium and propyl lithium; the carbon source gas is one of methane, ethane, ethylene and acetylene.

6. The method for preparing a high-power silicon-carbon composite material according to claim 1, characterized in that: In step S2, the flow rate of the mixed gas is 50-200 SCCM; during the first deposition, the vacuum is evacuated to 0.1-1 MPa, the temperature is 500-1000° C., and the deposition time is 30-300 min.

7. The method for preparing a high-power silicon-carbon composite material according to claim 1, characterized in that: In step S3, the fast ion conductor is a lithium oxide fast ion conductor.

8. The method for preparing a high-power silicon-carbon composite material according to claim 7, characterized in that: The lithium oxide fast ion conductor is one of LiLaO2, LiSeO2, LiNbO2 and LiCeO2.

9. The method for preparing a high-power silicon-carbon composite material according to claim 1, characterized in that: In step S3, during the second deposition, an atomic vapor deposition method is used, and the deposition time is 10 to 60 minutes.

10. A high-power silicon-carbon composite material, characterized in that: The high-power silicon-carbon composite material is prepared by the preparation method of any one of claims 1 to 9.