Solid electrolyte, preparation method thereof and sodium metal battery

By using 3D printing technology in sodium metal batteries, the combined structure of thin film layer and columnar array layer is used to solve the problems of poor interface contact and low ion conductivity, and the efficient ion transport of sodium metal batteries is achieved and Stability improves the overall performance of the battery.

CN119050456APending Publication Date: 2024-11-29ZHEJIANG LIWINON ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411385539.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing sodium ion solid electrolytes have problems such as poor interface contact, low ion conductivity and poor low temperature performance in sodium metal batteries, resulting in uneven current distribution within the battery and sodium dendrites growth, which may cause short circuits.

Method used

Using solid electrolytes including a film layer and a columnar array layer, the film layer is located between the positive and negative electrodes for conducting ions, the columnar array layer is used to contact the positive and negative electrode materials, printed and UV-cured through 3D printing technology to ensure sodium The uniform distribution and dense arrangement of superion conductors shorten the ion transmission distance and improve the ion conductivity.

Benefits of technology

It significantly improves the ionic conductivity and electrochemical kinetics of sodium metal batteries, inhibits the growth of sodium dendrites, ensures uniform deposition and efficient transmission of ions inside the battery, and improves the energy density and cycling stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005070910300000081
    Figure BDA0005070910300000081
  • Figure BDA0005070910300000091
    Figure BDA0005070910300000091
  • Figure BDA0005070910300000092
    Figure BDA0005070910300000092
Patent Text Reader

Abstract

The invention belongs to the technical field of sodium metal batteries, and particularly relates to a solid electrolyte, a preparation method thereof and a sodium metal battery, the solid electrolyte comprises a thin film layer and two cylindrical object array layers, and the two cylindrical object array layers are respectively arranged on two side surfaces of the thin film layer; the columnar body array layer comprises a plurality of columnar bodies arranged on the surface of the thin film layer in an array mode, and the columnar bodies extend outwards from the thin film layer; the solid electrolyte also comprises a sodium super-ion conductor; when the solid electrolyte is applied to a thick electrode, good ionic conductivity and high ion migration speed can still be kept, and efficient transmission of ions in the battery is ensured; the problems that the energy efficiency of the battery is reduced due to the increase of the electrode thickness and potential safety hazards are caused by uneven ion deposition in the battery can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sodium metal batteries, and relates to a solid electrolyte and a preparation method thereof, and a sodium metal battery. Background Art

[0002] The abundance of sodium on Earth is more than four hundred times that of lithium. Due to the similar physical and chemical properties of sodium and lithium and its abundant reserves, sodium-ion batteries are expected to replace lithium-ion batteries. Sodium-ion batteries have great application potential in electric motorcycles, low-speed electric vehicles and large-scale energy storage.

[0003] In order to solve the problem of flammable and leaky sodium battery electrolyte, the industry uses solid electrolyte materials to replace liquid organic electrolytes and assemble solid sodium metal batteries. Solid sodium metal batteries not only significantly improve the safety of the battery, but also greatly broaden the electrochemical window. The use of high-potential positive electrode materials and metallic sodium negative electrodes further improves the energy density of the battery. Among the sodium ion solid electrolytes currently studied, due to the sodium superion conductor (NASICON) type solid electrolyte sodium zirconium silicon phosphorus oxide (Na3Zr2Si2PO 12 ) has been widely developed due to its high ionic conductivity and chemical stability; however, its interface contact with the electrode, especially the thick electrode, is poor, which will lead to a high interface impedance between the electrolyte and the metallic sodium negative electrode and uneven current distribution inside the battery; and the sodium deposition rate is fast where the current density is high, inducing the growth of dendrites on the surface of the sodium negative electrode. When the sodium dendrites grow to a certain extent, they may penetrate the diaphragm and cause a short circuit in the battery; although organic polymer solid electrolytes such as polyethylene oxidized (PEO), polyvinylidene difluoride (PVDF) and polymethyl methacrylate (PMMA) have sufficient flexibility and mechanical strength and can present good interface contact with the positive and negative electrodes, they generally have low ionic conductivity and poor low-temperature performance, and their application in solid-state sodium batteries with thick electrodes is also greatly limited. Summary of the invention

[0004] In view of the above problems existing in the prior art, the object of the present invention is to provide a solid electrolyte and a preparation method thereof and a sodium metal battery.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention provides a solid electrolyte, comprising a thin film layer;

[0007] Two columnar array layers are respectively arranged on the two side surfaces of the film layer;

[0008] The columnar array layer includes a plurality of columns arranged in an array on the surface of the film layer, and the plurality of columns are all extended outward from the film layer;

[0009] The solid-state electrolyte also includes a sodium superion conductor.

[0010] In some embodiments, in the thin film layer, based on the total mass of the thin film layer being 100%, the content of the sodium superion conductor is C1; in the columnar array layer, the surface density of the columnar body is N; based on the total mass of the columnar array layer being 100%, the content of the sodium superion conductor is C2;

[0011] Wherein, the value of C1 is 10% to 50%, and / or the value of C2 is 35% to 85%, and / or the value of N is 15 / 2.545 cm 2 ~35 pieces / 2.545cm 2 .

[0012] In some embodiments, C1, C2 and N all satisfy 2<(C1+C2) / N<7.

[0013] In some embodiments, the layer height of the thin film layer is 20 um to 50 um, and / or the layer height of the columnar array layer is 20 um to 30 um.

[0014] In some embodiments, the thin film layer and the columnar array layer are both printed by a 3D printer.

[0015] In some embodiments, the sodium superion conductor includes at least one of sodium zirconium silicon phosphorus oxide, β-aluminum oxide, and sodium antimonite sulfate.

[0016] The present invention also provides a method for preparing a solid electrolyte, comprising the following steps:

[0017] preparing a first slurry and a second slurry both containing a sodium superion conductor;

[0018] Printing the second slurry into a solid electrolyte having a plurality of columnar structures arranged in an array by a 3D printer to obtain a first columnar array layer;

[0019] On the surface of the first columnar array layer, the first slurry is printed into a solid electrolyte with a thin film structure by a 3D printer to obtain a thin film layer;

[0020] On the outer surface of the thin film layer, the second slurry is printed into a solid electrolyte having a plurality of columnar structures arranged in an array by a 3D printer to obtain a second columnar array layer.

[0021] In some embodiments, in the thin film layer, based on the total mass of the thin film layer being 100%, the content of the sodium superion conductor is C1; in the first columnar array layer and the second columnar array layer, the surface density of the columns is N; based on the total mass of the first columnar array layer or the second columnar array layer being 100%, in the first columnar array layer or the second columnar array layer, the content of the sodium superion conductor is C2;

[0022] Wherein, the value of C1 is 10% to 50%, the value of C2 is 35% to 85%, and the value of N is 15 / 2.545 cm 2 ~35 pieces / 2.545cm 2 .

[0023] In some embodiments, C1, C2 and N all satisfy 2<(C1+C2) / N<7.

[0024] In some embodiments, the obtained thin film layer has a layer height of 20 um to 50 um, and / or the obtained first columnar array layer and the obtained second columnar array layer have a layer height of 20 um to 30 um.

[0025] In some embodiments, the following steps are also included:

[0026] While the first slurry or the second slurry is printed by the 3D printer, ultraviolet light with a wavelength of 360nm to 420nm is used for irradiation throughout the whole process, so that the thin film layer, the first columnar array layer and the second columnar array layer are UV cured and formed.

[0027] In some embodiments, the following steps are also included:

[0028] During the printing of the first slurry and the second slurry by the 3D printer, the first slurry or the second slurry in the 3D printer tank is continuously stirred at a speed of 200 r / min to 300 r / min, and the temperature of the first slurry or the second slurry is maintained in the range of 25° C. to 35° C.

[0029] The present invention further provides a sodium metal battery, comprising the above-mentioned solid electrolyte, and also comprising a positive electrode material and a negative electrode material respectively arranged on the two side surfaces of the solid electrolyte; the positive electrode material and the negative electrode material are both obtained by in-situ casting on the surface of the solid electrolyte.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The thin film layer of the solid electrolyte in the present invention is located between the positive and negative electrodes for conducting ions, and the two columnar array layers are used to contact the positive and negative electrode materials respectively; a large number of densely arranged electrolyte slurry rods are distributed on the columnar array layer, which can make the electrolyte and the positive and negative electrodes adhere more closely, and the electrolyte slurry rods of this columnar structure extend vertically outward from the thin film layer, and can penetrate into the interior of the positive and negative electrode materials, shorten the ion transmission distance, and improve the ion conductivity; the electrolyte slurry rods on the columnar array layer are arranged evenly and densely, so that the deposition of ions during charging and discharging is uniform, and the growth of sodium dendrites can be effectively inhibited; the solid electrolyte in the present invention can still maintain good ion conductivity and faster ion migration speed when applied to thick electrodes, ensuring efficient transmission of ions inside the battery; it can solve the problem of reduced battery energy efficiency due to increased electrode thickness and potential safety hazards caused by uneven ion deposition inside the battery. DETAILED DESCRIPTION

[0032] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be described in further detail below in conjunction with specific implementation methods, but the implementation methods of the present invention are not limited thereto.

[0033] The present invention provides a solid electrolyte, comprising a thin film layer;

[0034] Two columnar array layers are respectively arranged on the two side surfaces of the thin film layer;

[0035] The columnar array layer includes a plurality of columns arranged in an array on the surface of the film layer, and the plurality of columns are all extended outward from the film layer;

[0036] When the solid electrolyte is in use, the thin film layer is located between the positive and negative electrodes for conducting ions, and the two columnar array layers are used to contact the positive and negative electrode materials respectively. The structure of the columnar array layer can make the electrolyte adhere more closely to the positive and negative electrodes; in addition, a large number of densely arranged electrolyte slurry rods are distributed on the columnar array layer. The electrolyte slurry rods with this columnar structure extend vertically outward from the thin film layer and can penetrate into the interior of the positive and negative electrode materials, so that sodium ions and electrons can be quickly transferred between the thick electrode active materials along these electrolyte slurry rods, shortening the transmission distance and improving the ion conductivity; the electrolyte slurry rods with the columnar structure on the columnar array layer are evenly and densely arranged, and the deposition of ions becomes uniform during the charge and discharge process, which can effectively inhibit the growth of sodium dendrites and reduce the risk of sodium dendrites piercing the diaphragm.

[0037] Further, in the thin film layer, based on the total mass of the thin film layer being 100%, the content of sodium zirconium silicon phosphorus oxygen is C1; in the columnar array layer, the surface density of the columnar body is N, based on the total mass of the thin film layer being 100%, the content of sodium zirconium silicon phosphorus oxygen is C2;

[0038] Furthermore, the value of C1 is 10% to 50%, and / or the value of C2 is 35% to 85%, and / or the value of N is 15 / 2.545 cm 2 ~35 pieces / 2.545cm 2 ;

[0039] Furthermore, C1, C2 and N all satisfy 2<(C1+C2) / N<7; the values ​​of C1, C2 and N are directly related to the mechanical properties and ion transport properties of the thin film layer and the columnar array layer. Too high or too low C1, C2 and N will have an adverse effect on the battery performance, so in this solution, C1, C2 and N are kept within the above preferred range; in this solution, the positive and negative electrode slurries can be in-situ coated on the surface of the solid electrolyte, and the array rods with an appropriate density can achieve close fit between the positive and negative electrode slurries and the solid electrolyte, solving the problem of poor solid-solid contact in solid-state batteries; the distribution of the sodium zirconium silicon phosphorus oxygen content in the thin film layer can make While improving the ionic conductivity of the middle thin film layer, the solid electrolyte still has good tensile strength and mechanical strength, which is sufficient to inhibit the growth of dendrites, thereby maintaining the high and stable discharge capacity and capacity retention rate of the solid-state battery during long-term cycling; in addition, the columnar array layer contains a high concentration of sodium zirconium silicon phosphorus oxygen, which can penetrate deep into the positive and negative electrodes, thereby forming a large number of continuously arranged high-speed ion transmission channels, allowing sodium ions to be transmitted over long distances to the inside of the thick electrode, improving the electrochemical kinetics of the battery, especially the discharge rate performance of the battery is significantly improved, and even at a high rate of 3C, there is still a capacity retention rate of nearly 90%.

[0040] Furthermore, the layer height of the thin film layer is 20um-50um, and / or the layer height of the columnar array layer is 20um-30um.

[0041] Furthermore, the thin film layer and the columnar array layer are both printed by a 3D printer; the solid electrolyte in the present invention is obtained by 3D printing, with high production efficiency and good precision.

[0042] Furthermore, the sodium superion conductor includes at least one of sodium zirconium silicon phosphorus oxide, β-aluminum oxide, and sodium antimonite sulfide; in the present invention, the sodium superion conductor is preferably sodium zirconium silicon phosphorus oxide (Na3Zr2Si2PO 12 ), because sodium zirconium silicon phosphorus oxide is less sensitive to water, oxygen, etc., shows better antioxidant ability, higher stability, and is more suitable for 3D printing process; while β-alumina (β-Al2O3) may react with water and oxygen to generate alkaline impurities such as NaOH or Na2CO3, which can easily reduce the conductivity of the electrolyte; and sodium thioantimonate (Na3SbS4) may react with water, and react with water in the air to generate toxic gases such as hydrogen sulfide.

[0043] The preparation method of the solid electrolyte is as follows:

[0044] Prepare a first slurry and a second slurry respectively;

[0045] Printing the second slurry into a solid electrolyte having a plurality of columnar structures arranged in an array by a 3D printer to obtain a first columnar array layer;

[0046] On the surface of the first columnar array layer, a solid electrolyte having a thin film structure is printed by a 3D printer to obtain a thin film layer;

[0047] On the outer surface of the thin film layer, a plurality of solid electrolytes with columnar structures are arranged in an array by a 3D printer to obtain a second columnar array layer.

[0048] Furthermore, while the first slurry or the second slurry is printed by a 3D printer, ultraviolet light with a wavelength of 360nm to 420nm is used for irradiation throughout the process, so that the thin film layer, the first columnar array layer and the second columnar array layer are UV cured and formed; while the 3D printer is printing, ultraviolet light is used for irradiation throughout the process, and the slurry can be quickly formed after being extruded through the nozzle, which can improve the accuracy of the finished product and save a molding process after printing.

[0049] Furthermore, during the printing of the first slurry and the second slurry by the 3D printer, the first slurry or the second slurry in the 3D printer material tank is continuously stirred at a speed of 200r / min to 300r / min, and the temperature of the first slurry or the second slurry is maintained in the range of 25 to 35°C; the first slurry and the second slurry are maintained in a suitable temperature range and are continuously stirred during the printing process to avoid coagulation or agglomeration inside the slurry, so that the printed solid electrolyte has good surface state and mechanical properties.

[0050] The present invention further provides a sodium metal battery, comprising the above-mentioned solid electrolyte, and also comprising a positive electrode material and a negative electrode material respectively arranged on the surfaces of both sides of the solid electrolyte; the positive electrode material and the negative electrode material are obtained by in-situ casting and molding on the surface of the solid electrolyte; different from the solid-liquid interface in the liquid battery, the contact between the solid electrolyte and the electrode is mainly solid-solid interface contact, under this contact mode, it is usually difficult to achieve sufficient fit between the solid electrolyte and the electrode, and the contact area is relatively small, resulting in a high interface contact impedance, limiting the transmission efficiency of ions at the interface, thereby affecting the energy density and power density of the battery; in addition, there may be defects such as cracks and pores at the solid-solid interface These defects may lead to poor contact between the electrolyte and the electrode, which will further affect the efficiency and stability of ion transmission, and even cause safety problems such as electrolyte leakage or internal short circuit of the battery. In this scheme, the positive and negative active materials are in situ cast on the surface of the three-dimensional electrolyte in the form of slurry. This surface in situ casting method can form a closer contact between the electrolyte and the electrode, reducing the gaps and defects at the interface. At the same time, the protruding columns in the columnar array layer can significantly increase the direct contact area between the positive and negative active materials and the electrolyte, improve the adhesion of the positive and negative electrodes on the electrolyte, thereby reducing the interface impedance and improving the ion transmission efficiency at the interface, thereby improving the overall performance of the battery.

[0051] Example 1

[0052] This embodiment 1 provides a solid electrolyte and a sodium metal battery including the solid electrolyte, wherein:

[0053] 1. Preparation of the first slurry:

[0054] Take Na3Zr2Si2PO4 with a mass ratio of 15:45:30 12 , polyethylene glycol diacrylate (PEGDA) and sodium bis(trifluoromethylsulfonyl)imide (NaTFSI) are placed in a 10 mL glass bottle, and a photoinitiator is added, and the mixture is mixed and stirred at 25° C. for 6 hours to obtain a first slurry; wherein the photoinitiator is dibenzoyl peroxide (BPO) and the amount of BPO is 1% of the mass of PEGDA; based on the mass of the first slurry being 100%, the content of NZSP C1 is 15%;

[0055] In some other embodiments, PEGDA can also be replaced by other materials, including but not limited to ethoxylated trimethylolpropane triacrylate (ETPTA) and 3-cyclohexene-1-methyleneacrylate (CEA); NaTFSI can also be replaced by other materials, including but not limited to NaPF6, NaFSI, NaClO4, and NaBF4.

[0056] 2. Preparation of the second slurry:

[0057] Take Na3Zr2Si2PO4 with a mass ratio of 35:35:30 12 , PEGDA and NaTFSI are put into a 10 mL glass bottle, and a photoinitiator is added, and the mixture is mixed and stirred at 25° C. for 6 hours to obtain a second slurry; wherein the photoinitiator is dibenzoyl peroxide (BPO) and the amount of BPO is 1% of the mass of PEGDA; based on the mass of the second slurry being 100%, the content C2 of NZSP is 35%.

[0058] 3. 3D printing of solid electrolytes:

[0059] Place the prepared second slurry into the 3D printer tank, set the printing height to 25um, and the columnar printing surface density N to 15 / 2.545cm 2 , a plurality of solid electrolytes with a columnar structure arranged in an array are printed on a glass slide by a 3D printer to obtain a columnar array layer; in the printing step, the second slurry needs to be continuously stirred at a speed of 300r / min in the 3D printer material tank throughout the process, and the printing temperature is maintained at 25°C; and in the printing step, ultraviolet light with a wavelength of 405nm is used for irradiation throughout the process, so that the second slurry is quickly UV-cured and formed after being squeezed onto the glass slide;

[0060] The second slurry in the 3D printer material tank is replaced with the prepared first slurry, the printing layer height is set to 20um, and a solid electrolyte with a thin film structure is printed on the surface of the columnar array layer by a 3D printer to obtain a thin film layer located above the columnar array layer; in this printing step, the first slurry needs to be continuously stirred at a speed of 300r / min in the 3D printer material tank throughout the process, and the printing temperature is maintained at 25°C; and in this printing step, ultraviolet light with a wavelength of 405nm is used for irradiation throughout the process, so that the first slurry is squeezed onto the surface of the columnar array layer and quickly UV-cured and formed;

[0061] Replace the first slurry in the 3D printer tank with the second slurry, set the printing height to 25um, and the printing surface density N of the columnar body to 15 / 2.545cm 2 , a solid electrolyte having a plurality of columnar structures arranged in an array is printed on the surface of the thin film layer by a 3D printer, so as to obtain a columnar array layer located above the thin film layer; in this printing step, the second slurry needs to be continuously stirred at a speed of 300r / min in the 3D printer material tank throughout the process, and the printing temperature is maintained at 25°C; and in this printing step, ultraviolet light with a wavelength of 405nm is used for irradiation throughout the process, so that the second slurry is quickly UV-cured and formed after being squeezed onto the surface of the thin film layer;

[0062] After printing is completed, a solid electrolyte is obtained, which includes a columnar array layer, a thin film layer and a columnar array layer arranged in sequence from bottom to top.

[0063] 4. Preparation of positive and negative electrode materials:

[0064] Na3V2(PO4)3 active material, acetylene black and polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1 were put into a 5 ml small jar to obtain a mixed solution, 5% of the total mass of the mixed solution was added with NMP solvent, and ball milling was performed in a ball mill at a speed of 300 rpm for 2 hours to obtain a positive electrode slurry; the positive electrode slurry was directly coated on one side surface of the solid electrolyte, and vacuum dried at 120°C for 12 hours to obtain a positive electrode with a positive electrode loading of 15 mg / cm 2 .

[0065] In a glove box, sodium metal is melted into liquid at 200°C, and the liquid sodium metal is poured onto the other surface of the solid electrolyte. After the temperature is completely cooled, the solid electrolyte with positive and negative electrode materials on both sides is taken out and assembled into a button-type sodium metal full battery.

[0066] Example 2-12

[0067] The procedure of Example 1 was repeated according to the parameters specified in Examples 2 to 12 in Table 1.

[0068] Comparative Examples 1-10

[0069] The steps of Example 1 were repeated according to the parameters specified in Comparative Examples 1 to 10 in Table 1.

[0070] Table 1. Some process parameters for preparing solid electrolytes in Examples 2 to 12 and Comparative Examples 1 to 10

[0071]

[0072]

[0073] Performance Test:

[0074] The sodium metal batteries prepared in Examples 1 to 12 and Comparative Examples 1 to 10 were subjected to a charging cycle test, and the test method was as follows:

[0075] Using the Blue Electric tester system provided by Blue Electric Electronics Co., Ltd., the sodium metal full battery was first charged to 4.1V at a rate of 0.2C, and then charged to 2.5V at a rate of 0.2C; the sodium metal full battery was charged to 4.1V at a rate of 0.2C, and then charged to 2.5V at a rate of 1.0C; the sodium metal full battery was charged to 4.1V at a rate of 0.2C, and then charged to 2.5V at a rate of 2.0C; the sodium metal full battery was charged to 4.1V at a rate of 0.2C, and then charged to 2.5V at a rate of 3.0C.

[0076] The calculation formula is as follows:

[0077] Rate capacity retention rate = discharge capacity at different rates / first 0.2C discharge capacity * 100%;

[0078] The sodium metal batteries prepared in Examples 1 to 12 and Comparative Examples 1 to 10 were subjected to charge and discharge cycle tests, and the test method was as follows:

[0079] Using the Blue Electric tester system provided by Blue Electric Electronics Co., Ltd., the sodium metal full battery was first charged to 4.1V at a rate of 1.0C, and then charged to 2.5V at a rate of 1.0C. After 500 cycles, the 500-week capacity retention rate was calculated; the calculation formula is as follows:

[0080] Cycle capacity retention rate = 500 cycle discharge capacity / first discharge capacity*100%;

[0081] The test results are shown in Table 2.

[0082] Table 2. Test results of Examples 1 to 12 and Comparative Examples 1 to 11

[0083]

[0084]

[0085] Result analysis:

[0086] It can be seen from the data in Table 1 and Table 2 that, compared with Example 1, the surface density N of the columns of the columnar array layer of the electrolyte in Example 2 remains unchanged, the content C1 of NZSP in the thin film layer and the single-sided coating amount C2 of NZSP in the columnar array layer are both increased, and the cycle performance of the sodium battery is also improved; this is because when the NZSP content in the thin film layer and the columnar array layer is increased, the filler content of the electrolyte is increased, which can improve its ionic conductivity to a certain extent; in Comparative Examples 1 and 2, there is no NZSP filler in the columnar array layer of the electrolyte in Comparative Example 1, and there is no NZSP filler in the thin film layer of Comparative Example 2. The mechanical properties of the electrolytes in the two comparative examples are extremely poor, and there are almost no ion transport channels with high ion conductivity inside the electrolyte, which interrupts the sodium ion transport inside the thick electrode and the battery cannot exert its normal capacity; it is easy to know that when the thin film layer and the columnar array layer are filled with an appropriate amount of NZSP, the contact between the thick electrode and the electrolyte and the ionic conductivity inside the thick electrode can be optimized.

[0087] In Example 3 and Example 4, Example 4 increases the content C1 of NZSP in the thin film layer compared with Example 3. When the content of NZSP in the thin film layer is increased to 35%, micro-agglomeration will begin, which will affect the migration and conduction of ions, and the cycle performance will show a downward trend compared with Example 3; while the battery performance obtained in Comparative Examples 3 and 4 is not ideal, among which, the C1 of Comparative Example 3 is less than 10%, the content of NZSP in the thin film layer is low, the transmission of sodium ions is slow, and the ion deposition is not uniform, which may cause sodium dendrites to penetrate the electrolyte and cause micro-short circuits; C1 in Comparative Example 4 is increased to 65%, but the battery cycle performance is reduced. This is because when the filler content is too high, although the ion conductivity is improved, the flexibility of the middle thin film layer is greatly reduced. During the assembly process of the battery, the solid electrolyte is easily broken or damaged by external forces, which will affect the overall stability and safety of the battery; and during the charge and discharge process of the battery, the poor flexibility will cause the solid electrolyte to be unable to withstand the stress caused by the volume change, resulting in separation or damage between the electrolyte layer and the electrode, thereby affecting the cycle stability of the battery.

[0088] In Examples 5, 6, 7, and 8, the single-sided coating amount C2 of NZSP in the columnar array layer is gradually increased, and the other parameters remain unchanged. The discharge capacity and capacity retention of the obtained multiple batteries are first gradually increased, and then show a downward trend after C2 exceeds 80%; while in Comparative Examples 5 and 6, C2 in Comparative Example 5 is as high as 95%, which is far more than 80%, and the obtained battery performance is poor; This shows that although the content of NZSP in the columnar array layer can improve ionic conductivity when it is increased in the early stage, it will have a counter-effect after it is increased to a certain extent; this is mainly because the filler with too high a content is easy to gather together and agglomerate, which not only affects the ion conductivity of the electrolyte, but also affects the ionic conductivity of the electrolyte. The ion conductivity may be reduced, and the mechanical properties of the electrolyte may be reduced during the application process, thereby affecting the overall performance and safety of the battery and causing the mechanical properties of the electrolyte to decrease. In addition, if C2 is too high, the columns in the columnar array layer are too dense. When the battery is assembled, the columns are easily squeezed and broken, thereby interrupting the continuous ion transmission path, causing the ion transmission inside the thick electrode to deteriorate and the performance becomes worse. In Comparative Example 6, C2 is lower than 35%, and the performance of the battery is reduced. This is mainly due to the fact that the NZSP content in the columnar array layer cannot form a dense and continuous ion transmission channel, so that the sodium ions cannot be transmitted to the inside of the thick electrode over a long distance.

[0089] In Examples 9, 10, 11, and 12, the surface density N of the columnar bodies is gradually increased, and the other parameters remain unchanged. The discharge capacity and capacity retention of the obtained multiple batteries are gradually increased.

[0090] / 2.545cm 2 Then there is a downward trend; while in Comparative Examples 7 and 8, N in Comparative Example 7 exceeds 35 / 2.545cm 2 , the performance of the battery is reduced; although the densely arranged columnar electrolyte slurry rods in the columnar array layer can make the electrolyte and the electrode fit firmly and tightly, the large contact area between the two will also lead to a reduction in the active material per unit volume. In addition, a large number of close contact sites will cause the solid electrolyte interface phase change, resulting in increased interface resistance and increased battery polarization, affecting battery performance and service life; while N in Comparative Example 8 is less than 15 / 2.545cm 2 There are fewer ion transmission pathways inside the thick electrode, and the contact between the electrode and the electrolyte is also poor. The electrolyte and the electrode are easy to loosen and fall off, which will cause the battery performance to deteriorate and affect the stability of the battery.

[0091] In Comparative Examples 9 and 10, although the NZSP content C1 in the thin film layer, the single-sided coating amount C2 of the NZSP in the columnar array layer, and the surface density N of the columns are all within the preferred range of this scheme, C1, C2, and N do not satisfy the relationship of 2<(C1+C2) / N<7, and the overall performance of the batteries obtained in Comparative Examples 9 and 10 still does not meet the requirements; this further proves the superiority of the parameter selection of this scheme. Only when the NZSP content C1 of the thin film layer in the solid electrolyte is within 10% to 50%, the NZSP content C2 of the columnar array layer is within 35% to 85%, and the surface density N of the columns is 15 / 2.545cm 2 ~35 pieces / 2.545cm 2 Within, and C1, C2 and N satisfy 2<(C1+C2) / N<7, the mechanical properties of the solid electrolyte can achieve sufficient strength, the ion transmission performance can achieve a better effect, the solid electrolyte and the electrode are closely fitted, and the problem of poor solid-solid contact in the solid-state battery is solved. At the same time, the mechanical properties of the solid electrolyte are improved, which is sufficient to inhibit the growth of dendrites, and a large number of continuously arranged high-speed ion transmission channels are formed inside the electrolyte, so that sodium ions can be transmitted to the inside of the thick electrode over a long distance, thereby improving the electrochemical kinetics of the battery, so that the discharge capacity of the solid-state battery and the room temperature cycle capacity retention rate are improved, thereby improving the overall performance of the solid-state battery; in addition, according to the comparison of the rate and long-term cycle performance data of Examples 1 to 12, under the premise of satisfying the relationship 2<(C1+C2) / N<7, C1 is in a small range of 20% to 35%, C2 is in a small range of 60% to 80%, or N is 20 to 35 / 2.545cm 2 When the C1 is in the range of 15% to 35%, C2 is in the range of 35% to 85%, or N is in the range of 15 to 35 / 2.545 cm 2 When the temperature is within the range of , the performance of the solid electrolyte is better.

[0092] The above are only partial or preferred embodiments of the present invention, and the scope of protection of the present invention cannot be limited therefrom. All equivalent structural changes made by using the specification of the present invention under the concept of an overall concept of the present invention, or direct / indirect application in other related technical fields are included in the scope of protection of the present invention.

Claims

1. A solid electrolyte, characterized in that include Thin film layer; Two columnar array layers are respectively arranged on the two side surfaces of the film layer; The columnar array layer includes a plurality of columns arranged in an array on the surface of the film layer, and the plurality of columns are all extended outward from the film layer; The solid-state electrolyte also includes a sodium superion conductor.

2. The solid electrolyte according to claim 1, characterized in that In the thin film layer, based on the total mass of the thin film layer being 100%, the content of the sodium superion conductor is C1; in the columnar array layer, the surface density of the columns is N; based on the total mass of the columnar array layer being 100%, the content of the sodium superion conductor is C2; Wherein, the value of C1 is 10% to 50%, and / or the value of C2 is 35% to 85%, and / or the value of N is 15 / 2.545 cm 2 ~35 pieces / 2.545cm 2 .

3. The solid electrolyte according to claim 2, characterized in that The C1, the C2 and the N all satisfy 2<(C1+C2) / N<7.

4. The solid electrolyte according to claim 2, characterized in that The layer height of the thin film layer is 20um-50um, and / or the layer height of the columnar array layer is 20um-30um.

5. The solid electrolyte according to claim 2 or 4, characterized in that: The thin film layer and the columnar array layer are both printed by a 3D printer.

6. The solid electrolyte according to claim 5, characterized in that The sodium superion conductor includes at least one of sodium zirconium silicon phosphorus oxide, β-aluminum oxide, and sodium antimonite sulfide.

7. A method for preparing a solid electrolyte, characterized in that: The steps include: preparing a first slurry and a second slurry both containing a sodium superion conductor; Printing the second slurry into a solid electrolyte having a plurality of columnar structures arranged in an array by a 3D printer to obtain a first columnar array layer; On the surface of the first columnar array layer, the first slurry is printed into a solid electrolyte with a thin film structure by a 3D printer to obtain a thin film layer; On the outer surface of the thin film layer, the second slurry is printed into a solid electrolyte having a plurality of columnar structures arranged in an array by a 3D printer to obtain a second columnar array layer.

8. The method for preparing a solid electrolyte according to claim 7, characterized in that: In the thin film layer, based on the total mass of the thin film layer being 100%, the content of the sodium superion conductor is C1; in the first columnar array layer and the second columnar array layer, the surface density of the columns is N; based on the total mass of the first columnar array layer or the second columnar array layer being 100%, in the first columnar array layer or the second columnar array layer, the content of the sodium superion conductor is C2; Wherein, the value of C1 is 10% to 50%, and / or the value of C2 is 35% to 85%, and / or the value of N is 15 / 2.545 cm 2 ~35 pieces / 2.545cm 2 .

9. The method for preparing a solid electrolyte according to claim 8, characterized in that: The C1, the C2 and the N all satisfy 2<(C1+C2) / N<7.

10. The method for preparing a solid electrolyte according to claim 7 or 8, characterized in that: The obtained film layer has a layer height of 20 um to 50 um, and / or the obtained first columnar array layer and the obtained second columnar array layer have a layer height of 20 um to 30 um.

11. The method for preparing a solid electrolyte according to claim 10, characterized in that: The following steps are also included: While the first slurry or the second slurry is printed by the 3D printer, ultraviolet light with a wavelength of 360nm to 420nm is used for irradiation throughout the whole process, so that the thin film layer, the first columnar array layer and the second columnar array layer are UV cured and formed.

12. The method for preparing a solid electrolyte according to claim 11, characterized in that: The following steps are also included: During the printing of the first slurry and the second slurry by the 3D printer, the first slurry or the second slurry in the 3D printer tank is continuously stirred at a speed of 200 r / min to 300 r / min, and the temperature of the first slurry or the second slurry is maintained in the range of 25° C. to 35° C.

13. A sodium metal battery, characterized in that: A solid electrolyte comprising any one of claims 1 to 6, further comprising a positive electrode material and a negative electrode material respectively arranged on both side surfaces of the solid electrolyte; the positive electrode material and the negative electrode material are both obtained by in-situ casting on the surface of the solid electrolyte.