Electrolyte, battery and power utilization system
By adding specific additives to the lithium ion electrolyte, a SEI interface layer rich in lithium sulfide and lithium sulfonate is solved, the problem of electrolyte instability in high temperature environments is improved, the high temperature stability and cycle life of the battery are improved, and the high temperature stability and cycle life are ensured. The safety performance of the battery.
Patent Information
- Application Number
- CN202411088114.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-29
AI Technical Summary
The electrolyte instability of the lithium-ion battery cell in high temperature environments leads to performance degradation and safety hazards, especially in the accumulation of heat in large-capacity battery cells, which leads to an increase in the internal pressure of the battery cell, which may cause a fire or explosion.
The first additive and the second additive are added simultaneously to the electrolyte. The first additive generates a flexible polysulfonate SEI film to enhance the chemical stability of the interface layer. The second additive generates polysulfide anions through the S-S bond homozygation to improve the interface. The ionic conductivity is combined to make lithium sulfide and lithium sulfonate the SEI interface layer mainly enhance high temperature stability and lithium ion transport characteristics.
It effectively improves the cycle life and safety performance of the battery in a high-temperature environment, reduces the charge transfer impedance of the battery cell, and enhances the high-temperature stability and normal high-temperature circulation performance of the battery.
Smart Images

Figure CN119050474A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of batteries, and specifically relates to an electrolyte, a battery and an electricity system. Background Art
[0002] With the development of the energy storage industry, lithium-ion battery technology has continued to develop and is widely used in electric vehicles, mobile devices, energy storage systems and other fields. However, lithium-ion batteries have the problem of electrolyte instability in high temperature environments, which not only affects the performance and life of the battery, but may also cause safety hazards. However, with the increasing energy density and increasing integration of battery cells in current large-scale energy storage batteries, the challenge of maintaining safety is becoming increasingly difficult.
[0003] In order to increase the energy density of energy storage cells and reduce production costs, higher electrode coatings and higher compaction densities are generally used. At the same time, the capacity of a single cell is getting larger and larger. On the basis of the same active material capacity, the amount of current collector and electrolyte used needs to be reduced. While these strategies bring high energy density and reduce costs, the stability of the cells under high temperature conditions is also becoming increasingly prominent. In large-capacity cells, the cells generate high heat and have poor heat dissipation. During operation, heat is easily accumulated, causing the electrolyte to easily decompose and evaporate, resulting in increased pressure inside the cell, and may even cause the cell to catch fire or explode. Summary of the invention
[0004] The present application aims to solve at least one of the technical problems in the related art to a certain extent. To this end, one purpose of the present application is to provide an electrolyte, a battery and an electricity system. The present application adds a first additive and a second additive to the electrolyte at the same time, which can effectively improve the high temperature stability and normal high temperature cycle performance of the battery, thereby effectively improving the cycle life and safety performance of the battery in a high temperature environment.
[0005] In a first aspect, the present application provides an electrolyte. According to an embodiment of the present application, the electrolyte includes an electrolyte salt, an organic solvent and an additive, the additive includes a first additive and a second additive, the first additive includes at least one of the compounds shown in Formula I, and the second additive includes at least one of the compounds shown in Formula II;
[0006]
[0007] Among them, R1, R2, R3 and R4 are each independently selected from at least one of hydrogen, fluorine, vinyl and methyl, R5 and R6 are each independently selected from at least one of methyl, ethyl, propyl, vinyl, propenyl and (triethoxysilyl)propyl, and n is an integer of 3 to 6.
[0008] According to the electrolyte of the above embodiment of the present application, the first additive and the second additive are added to the electrolyte at the same time. During the battery cycle, the first additive can effectively improve the high temperature stability of the battery cell, and the second additive can effectively improve the ionic conductivity of the SEI film at the interface, thereby reducing the charge transfer impedance of the battery cell. In addition, the first additive and the second additive are used together to increase the inorganic components mainly composed of lithium sulfide and lithium sulfonate in the SEI interface layer. The inorganic-rich interface layer can combine the high temperature stability of the sulfonate and the fast active ion (such as lithium ion) transmission characteristics of the sulfide, effectively improve the high temperature stability and normal high temperature cycle performance of the battery, thereby effectively improving the cycle life and safety performance of the battery in a high temperature environment.
[0009] In addition, the electrolyte according to the above embodiment of the present application may also have the following additional technical features:
[0010] In some embodiments of the present application, R5 and R6 are the same.
[0011] In some embodiments of the present application, n is 3 or 4.
[0012] In some embodiments of the present application, the first additive includes at least one of the following compounds:
[0013]
[0014] In some embodiments of the present application, the second additive includes at least one of the following compounds:
[0015]
[0016] In some embodiments of the present application, the mass proportion of the first additive in the electrolyte is a, satisfying 0.2%≤a≤5%; and / or, the mass proportion of the second additive in the electrolyte is b, satisfying 0.2%≤b≤5%.
[0017] In some embodiments of the present application, the ratio of a to b is 1:(0.5-1.5).
[0018] In some embodiments of the present application, the additive includes a third additive, and the third additive includes at least one of fluorovinylene carbonate, 2-fluoro-pyridine and 2-fluoro-5-aminopyridine.
[0019] In some embodiments of the present application, the mass proportion of the third additive in the electrolyte is c, satisfying 0.2%≤c≤3%.
[0020] In some embodiments of the present application, the electrolyte salt accounts for 5% to 20% by mass in the electrolyte; and / or, the electrolyte salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, lithium bis(oxalatoborate), lithium difluoroborate and lithium bis(trifluoromethanesulfonyl)imide; and / or, the organic solvent includes cyclic carbonates and chain carbonates.
[0021] The second aspect of the present application provides a battery. According to an embodiment of the present application, the battery includes the electrolyte of the first aspect. As a result, the high temperature stability and normal high temperature cycle performance of the battery are effectively improved, thereby effectively improving the cycle life and safety performance of the battery in a high temperature environment.
[0022] The third aspect of the present application proposes an electric power system. According to an embodiment of the present application, the electric power system includes: electric equipment, and an energy storage device, the energy storage device supplies power to the electric equipment, and the energy storage device includes the electrolyte described in the above embodiment or the lithium-ion battery described in the above embodiment. As a result, the energy storage device of the electric power system has excellent normal and high temperature cycle performance, service life and safety performance. It should be noted that the above-mentioned features and advantages described for the battery are also applicable to the electric device and will not be repeated here.
[0023] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. DETAILED DESCRIPTION
[0024] The embodiments of the present application are described in detail below, which are intended to be used to explain the present application but should not be construed as limiting the present application.
[0025] The first aspect of the present application provides an electrolyte. According to an embodiment of the present application, the electrolyte includes an electrolyte salt, an organic solvent and an additive, the additive includes a first additive and a second additive, including an electrolyte salt, an organic solvent and an additive, the additive includes a first additive and a second additive, the first additive includes at least one of the compounds shown in Formula I, and the second additive includes at least one of the compounds shown in Formula II;
[0026]
[0027] Among them, R1, R2, R3 and R4 are each independently selected from at least one of hydrogen, fluorine, vinyl and methyl, R5 and R6 are each independently selected from at least one of methyl, ethyl, propyl, vinyl, propenyl and (triethoxysilyl)propyl, n is an integer of 3 to 6, and n represents the number of S.
[0028] The beneficial effects of the electrolyte proposed in this application are described in detail below:
[0029] In order to solve the problem of electrolyte failure under high temperature environment, the present application adds a first additive and a second additive to the electrolyte at the same time. During the battery cycle, the first additive can undergo a reduction reaction on the negative electrode surface to generate a flexible polysulfonate SEI film. The polysulfonate SEI film has excellent high temperature stability, which can effectively improve the chemical stability of the interface layer. However, the polysulfonate SEI film has a low ionic conductivity at the interface, resulting in a rapid increase in the initial impedance of the battery cell, causing degradation of the room temperature performance. In order to solve this problem, the present application also adds a second additive to the electrolyte. The second additive undergoes homolytic cleavage of the SS bond during the reduction process, and the generated polysulfide anions have a strong interaction with active ions (such as lithium ions). At the same time, it has a low solubility in the electrolyte, so that it can be deposited on the graphite surface, so that it can be preferentially adsorbed on the damaged interface, promoting the desolvation process of active ions (such as lithium ions) at the interface, and improving the ionic conductivity of the SEI film at the interface, thereby reducing the charge transfer impedance of the battery cell. In addition, when the first additive and the second additive are used in combination, the polysulfide formed by the homolytic cleavage of the SS bond of the second additive can increase the concentration of active ions (such as lithium ions) on the interface, thereby promoting the degradation of the cyclic sulfate of the first additive, so that the inorganic components mainly composed of lithium sulfide and lithium sulfonate in the SEI interface layer become more. The inorganic-rich interface layer can combine the high temperature stability of the sulfonate and the fast active ion (such as lithium ion) transport characteristics of the sulfide, effectively improving the high temperature stability and normal high temperature cycle performance of the battery, thereby effectively improving the cycle life and safety performance of the battery in a high temperature environment.
[0030] In the embodiments of the present application, n is an integer of 3 to 6. The inventors have found that n should not be too large because when the SS bonds in the long polysulfide chains are homolytically cleaved, more short-chain lithium sulfide products of Li2S4 to Li4S4 are easily generated. Such products are slightly soluble in the electrolyte and shuttle between the positive and negative electrodes, which will significantly deteriorate the electrical performance. Preferably, n is 3 or 4.
[0031] In the embodiments of the present application, R5 and R6 are each independently selected from at least one of methyl, ethyl, propyl, vinyl, propenyl, and (triethoxysilyl)propyl. Preferably, R5 and R6 are the same.
[0032] According to some specific embodiments of the present application, the first additive includes at least one of the following compounds:
[0033]
[0034] Therefore, the first additive of the above structure can undergo a reduction reaction on the surface of the negative electrode to generate a flexible polysulfonate SEI film, thereby further effectively improving the chemical stability of the interface layer, and the first additive of the above structure can be effectively used in combination with the second additive to further effectively improve the high temperature stability and normal high temperature cycle performance of the battery.
[0035] According to some further specific embodiments of the present application, the second additive includes at least one of the following compounds:
[0036]
[0037] Thus, the second additive of the above structure can undergo homolytic cleavage of SS bonds during the reduction process, and the generated polysulfide anions have a strong interaction with active ions (such as lithium ions), and can further promote the desolvation process of active ions (such as lithium ions) at the interface, thereby improving the ionic conductivity of the SEI film at the interface, thereby reducing the charge transfer impedance of the battery cell. The second additive of the above structure can be effectively used in combination with the first additive to further effectively improve the high temperature stability and normal high temperature cycle performance of the battery.
[0038] During the battery cycle, the first additive shown in Formula I-1 and the second additive shown in Formula II-2 will undergo the following reaction:
[0039]
[0040] According to some other specific embodiments of the present application, the mass proportion of the first additive in the electrolyte is a, satisfying 0.2%≤a≤5%. As an example, it can be 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc. By limiting the mass proportion of the first additive in the electrolyte to the above range, the chemical stability of the interface layer can be further effectively improved. At the same time, it can further ensure that the first additive is used in combination with the second additive, which can further effectively improve the high temperature stability and normal high temperature cycle performance of the battery.
[0041] According to some other specific embodiments of the present application, the mass proportion of the second additive in the electrolyte is b, satisfying 0.2%≤b≤5%. As an example, it can be 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc. By limiting the mass proportion of the second additive in the electrolyte to the above range, the desolvation process of active ions (such as lithium ions) at the interface can be further promoted, and the ionic conductivity of the SEI film at the interface can be improved, thereby reducing the charge transfer impedance of the battery cell. At the same time, it can further ensure that the second additive is used in combination with the first additive to further effectively improve the high temperature stability and normal high temperature cycle performance of the battery.
[0042] According to some other specific embodiments of the present application, the ratio of a to b is 1:(0.5~1.5), and as examples can be 1:0.5, 1:0.8, 1:1, 1:1.2, 1:1.5, etc. By limiting the ratio of a to b within the above range, the combined use of the first additive and the second additive can be further promoted, thereby improving the chemical stability of the interface layer and improving the ionic conductivity of the SEI film at the interface, thereby reducing the charge transfer impedance of the battery cell; at the same time, the high temperature stability and normal high temperature cycle performance of the battery can be further effectively improved.
[0043] According to some other specific embodiments of the present application, the additive includes a third additive, and the third additive includes a fluorine-containing additive. After the above-mentioned sulfur-rich SEI layer is introduced with an appropriate amount of the fluorine-containing additive, the cycle performance of the battery cell is further improved. This is because the fluorine-containing additive can be reduced at the interface in the early stage of film formation to produce an interface layer rich in lithium fluoride (lithium fluoride has high voltage stability and thermal stability). The interface layer has good electrochemical stability, thereby further improving the normal and high temperature cycle performance and high temperature storage performance of the battery cell.
[0044] In the embodiments of the present application, the specific types of the above-mentioned fluorine-containing additives are not particularly limited, and those skilled in the art can select them according to actual needs. As some preferred embodiments, the third additive includes at least one of fluorovinylene carbonate (FEC), 2-fluoro-pyridine (2FP), and 2-fluoro-5-aminopyridine (5A-2FP). 2-Fluoro-5-aminopyridine (5A-2FP) is preferred. The 5A-2FP additive promotes the occurrence of defluorination reaction due to the amination at the fluorine para position, thereby increasing the content of lithium fluoride at the interface, and thus has the best improvement effect.
[0045] According to some other specific embodiments of the present application, the mass proportion of the third additive in the electrolyte is c, satisfying 0.2%≤c≤3%. As an example, it can be 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, etc. By limiting the mass proportion of the third additive in the electrolyte to the above range, the cycle performance and high-temperature storage performance of the battery cell can be further improved.
[0046] In the embodiments of the present application, the specific types of the above-mentioned electrolyte salts are not particularly limited, and those skilled in the art can select them according to actual needs. As some specific examples, the above-mentioned electrolyte salts include at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(fluorosulfonyl)imide (LiFSI), lithium difluorophosphate (LiDFP), lithium dioxalate borate (LiBOB), lithium difluorooxalate borate (LiODFB) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI). At least one of lithium hexafluorophosphate (LiPF6) and lithium bis(fluorosulfonyl)imide (LiFSI) is preferred.
[0047] According to some other specific embodiments of the present application, the mass of the electrolyte salt in the electrolyte accounts for 5% to 20%, which can be 5%, 8%, 10%, 12%, 15%, 17%, 20%, etc., preferably 6% to 15%.
[0048] In the embodiments of the present application, the above-mentioned organic solvent is a non-aqueous organic solvent, wherein the non-aqueous organic solvent is the main component of the electrolyte and should have a high solubility of the electrolyte salt so that the electrolyte has a high ionic conductivity. Its specific type is not particularly limited, and those skilled in the art can select it according to actual needs. As some preferred embodiments, the above-mentioned organic solvent includes cyclic carbonates and chain carbonates. Among them, the cyclic carbonate includes at least one of ethylene carbonate and propylene carbonate, and the chain carbonate includes at least one of dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate. More preferably, the above-mentioned organic solvent includes a mixed solvent of ethylene carbonate, dimethyl carbonate and methyl ethyl carbonate.
[0049] The second aspect of the present application provides a battery. According to an embodiment of the present application, the battery includes the electrolyte of the first aspect. As a result, the high temperature stability and normal high temperature cycle performance of the battery are effectively improved, thereby effectively improving the cycle life and safety performance of the battery in a high temperature environment.
[0050] In the embodiments of the present application, the above electrolyte can be used for both lithium-ion batteries and sodium-ion batteries. The following is an example of lithium-ion batteries:
[0051] Generally, lithium-ion batteries include a positive electrode, a negative electrode, an electrolyte, and a separator. During the battery charging and discharging process, lithium ions are inserted and removed back and forth between the positive electrode and the negative electrode. The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The separator is set between the positive electrode and the negative electrode, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing lithium ions to pass through.
[0052] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material. The specific type of the positive electrode active material is not particularly limited. As some specific embodiments, the positive electrode active material includes at least one of lithium iron phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium nickel oxide, lithium cobalt phosphate, lithium manganese phosphate, lithium nickel phosphate, lithium manganese oxide, binary materials, and ternary materials.
[0053] In some embodiments of the present application, the positive electrode current collector may include a metal foil or a composite positive electrode current collector. For example, the metal foil may be aluminum foil. The composite positive electrode current collector may include a polymer material base and a metal layer formed on at least one side of the polymer material base. For example, the composite negative electrode current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT) and other substrates).
[0054] In some embodiments of the present application, the positive electrode active material layer may further optionally include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0055] In some embodiments of the present application, the positive electrode active material layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polyamide (PA), polyacrylonitrile (PAN), polyacrylate, polyvinyl ether, polymethyl methacrylate (PMMA), polyhexafluoropropylene, and styrene-butadiene rubber (SBR).
[0056] In some embodiments of the present application, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet (such as positive electrode active material, conductive agent, binder) are dispersed in an organic solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0057] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one side surface of the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode active material.
[0058] In some embodiments of the present application, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc.).
[0059] In some embodiments of the present application, the negative electrode active material may be a negative electrode active material for a battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, etc. The silicon-based material may include at least one of elemental silicon, silicon-oxygen compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may include at least one of elemental tin, tin-oxygen compounds, and tin alloys.
[0060] In some embodiments of the present application, the negative electrode active material layer may further optionally include a binder. The binder may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0061] In some embodiments of the present application, the negative electrode active material layer may further include a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0062] In some embodiments of the present application, the negative electrode active material layer may further optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0063] In some embodiments of the present application, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet (such as negative electrode active material, conductive agent, binder and any other components) are dispersed in an organic solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0064] The present application has no particular restrictions on the type of isolation membrane, and any known porous isolation membrane with good chemical stability and mechanical stability can be selected. In some embodiments of the present application, the isolation membrane may be made of at least one of glass fiber, non-woven fabric, polyethylene, polypropylene or polyvinylidene fluoride.
[0065] The lithium-ion battery of the present application may include a battery cell form, a battery module form and a battery pack form. In some embodiments, the battery cells may be assembled into a battery module, and the number of battery cells contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module. In some embodiments, the battery modules may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.
[0066] The third aspect of the present application proposes an electric power system. According to an embodiment of the present application, the electric power system includes: electric equipment, and an energy storage device, the energy storage device supplies power to the electric equipment, and the energy storage device includes the electrolyte described in the above embodiment or the lithium-ion battery described in the above embodiment. As a result, the energy storage device of the electric power system has excellent normal and high temperature cycle performance, service life and safety performance. It should be noted that the above-mentioned features and advantages described for the battery are also applicable to the electric device and will not be repeated here.
[0067] The energy storage device can be used as a power source for electrical equipment or as an energy storage unit for electrical equipment. The electrical equipment can include but is not limited to mobile phones, tablet computers, laptop computers, desktop computers, smart bracelets, smart watches, e-readers, game consoles and other portable electronic devices. It can also include but is not limited to vehicles such as cars, trucks, cars, vans, motor vehicles, high-speed trains, electric vehicles, etc. In addition, it can also be various household appliances, such as but not limited to refrigerators, electric lights, air conditioners, etc.
[0068] In addition, the energy storage device of the present application may include at least one of an energy storage device for the power generation side of the power system, an energy storage device for the distribution side of the power system (such as an electrochemical energy storage device), and an energy storage device for the user side of the power system.
[0069] The embodiments of the present application are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. In addition, unless otherwise explicitly stated, all reagents used in the following embodiments are commercially available or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.
[0070] Example 1
[0071] 1) Preparation of positive electrode
[0072] The positive electrode active material lithium iron phosphate, conductive carbon black (SP), and adhesive polyvinylidene fluoride (PVDF) were dispersed in an organic solvent N-methylpyrrolidone (NMP) and mixed evenly to obtain a positive electrode slurry, wherein the mass ratio of lithium iron phosphate, conductive carbon black, and PVDF was 97:0.7:2.3, and the solid content of the positive electrode slurry was 50wt%. The positive electrode slurry was coated on the positive electrode current collector aluminum foil, and the positive electrode slurry unit area (1540.25mm 2 ) The coating weight is 330 mg. After drying, cold pressing, slitting and cutting, the positive electrode sheet is obtained.
[0073] 2) Preparation of negative electrode
[0074] The negative electrode active material artificial graphite, conductive carbon SP, thickener CMC and binder SBR were dispersed in deionized water in a mass ratio of 96.5:0.5:1:2 and mixed evenly to obtain a negative electrode slurry, the solid content of which was 50wt%. The negative electrode slurry was coated on the negative electrode current collector copper foil, and the negative electrode slurry unit area (1540.25mm 2 ) The coating weight is 144 mg. After drying, cold pressing, slitting and cutting, the negative electrode sheet is obtained.
[0075] 3) Preparation of electrolyte
[0076] In an argon atmosphere glove box with a moisture content of ≤1ppm, ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) are mixed in a mass ratio of 2:1:2, and then dried lithium hexafluorophosphate is dissolved in an organic solvent, and the mass proportion of lithium hexafluorophosphate in the electrolyte is 13%. After the lithium hexafluorophosphate is stirred until it is completely dissolved, a first additive as shown in formula I-3 and a second additive as shown in formula II-1 are added and mixed evenly to obtain an electrolyte, wherein the mass proportion of the first additive as shown in formula I-3 in the electrolyte is 1%, and the mass proportion of the second additive as shown in formula II-1 in the electrolyte is 1%.
[0077] 4) Isolation film
[0078] A polyethylene film with a thickness of 16 microns was selected as the diaphragm.
[0079] 5) Battery assembly
[0080] The prepared positive electrode sheet, separator, and negative electrode sheet are stacked in order so that the separator is in the middle of the positive and negative electrodes to separate the positive and negative electrode sheets, and are wound to form a bare battery cell. After welding the pole ears, the bare battery cell is assembled into an outer package, and after injecting the prepared electrolyte, the battery cell is packaged, left to stand, formed, shaped, and capacity tested, etc., to finally prepare a lithium-ion battery.
[0081] Example 2
[0082] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0083] The first additive represented by formula I-3 is replaced by the first additive represented by formula I-1.
[0084] Example 3
[0085] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0086] The first additive represented by formula I-3 is replaced by the first additive represented by formula I-2.
[0087] Example 4
[0088] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0089] The second additive represented by formula II-1 is replaced by the second additive represented by formula II-2.
[0090] Example 5
[0091] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0092] The second additive represented by formula II-1 is replaced by the second additive represented by formula II-3.
[0093] Example 6
[0094] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0095] The mass proportion of the first additive in the electrolyte is 0.2%.
[0096] Example 7
[0097] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0098] The mass proportion of the first additive in the electrolyte is 1.5%.
[0099] Example 8
[0100] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0101] The mass proportion of the first additive in the electrolyte is 2.5%.
[0102] Example 9
[0103] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0104] The mass proportion of the first additive in the electrolyte is 3.5%.
[0105] Example 10
[0106] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0107] The mass proportion of the first additive in the electrolyte is 5%.
[0108] Embodiment 11
[0109] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0110] The mass proportion of the second additive in the electrolyte is 0.2%.
[0111] Example 12
[0112] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0113] The mass proportion of the second additive in the electrolyte is 1.5%.
[0114] Embodiment 13
[0115] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0116] The mass proportion of the second additive in the electrolyte is 2.5%.
[0117] Embodiment 14
[0118] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0119] The mass proportion of the second additive in the electrolyte is 3.5%.
[0120] Embodiment 15
[0121] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0122] The mass proportion of the second additive in the electrolyte is 5%.
[0123] Example 16
[0124] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0125] The mass proportion of the first additive in the electrolyte is 0.1%, and the mass proportion of the second additive in the electrolyte is 0.1%.
[0126] Embodiment 17
[0127] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0128] The mass proportion of the first additive in the electrolyte is 7%, and the mass proportion of the second additive in the electrolyte is 7%.
[0129] Embodiment 18
[0130] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0131] Fluorovinylene carbonate (FEC) is also included, and the mass proportion of fluorovinylene carbonate (FEC) in the electrolyte is 0.2%.
[0132] Embodiment 19
[0133] The preparation methods of this embodiment are basically the same as those of embodiment 18, the only difference being the additive in the electrolyte:
[0134] Fluorovinylene carbonate (FEC) is also included, and the mass proportion of fluorovinylene carbonate (FEC) in the electrolyte is 1%.
[0135] Embodiment 20
[0136] The preparation methods of this embodiment are basically the same as those of embodiment 18, the only difference being the additive in the electrolyte:
[0137] Fluorovinylene carbonate (FEC) is also included, and the mass proportion of fluorovinylene carbonate (FEC) in the electrolyte is 2.5%.
[0138] Embodiment 21
[0139] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0140] The electrolyte also includes 2-fluoro-pyridine (2FP), and the mass proportion of 2-fluoro-pyridine (2FP) in the electrolyte is 1%.
[0141] Embodiment 22
[0142] The preparation method of this embodiment is basically the same as that of embodiment 1, the only difference being the additive in the electrolyte:
[0143] It also includes 2-fluoro-5-aminopyridine (5A-2FP), and the mass proportion of 2-fluoro-5-aminopyridine (5A-2FP) in the electrolyte is 1%.
[0144] Comparative Example 1
[0145] The preparation method of this comparative example is basically the same as that of Example 1, except that the electrolyte does not contain the first additive shown in Formula I-3 and the second additive shown in Formula II-1.
[0146] Comparative Example 2
[0147] The preparation method of this comparative example is basically the same as that of Example 1, the only difference being the additive in the electrolyte:
[0148] Only the first additive shown in formula I-3 is added to the electrolyte, and the second additive shown in formula II-1 is not added.
[0149] Comparative Example 3
[0150] The preparation method of this comparative example is basically the same as that of Example 1, the only difference being the additive in the electrolyte:
[0151] Only the second additive as shown in formula II-1 is added to the electrolyte, and the first additive as shown in formula I-3 is not added.
[0152] The parameters of Examples 1-22 and Comparative Examples 1-3 are shown in Table 1.
[0153] Table 1
[0154]
[0155]
[0156] The 25°C 500 cycle 1C capacity retention rate, 45°C 500 cycle 1C capacity retention rate and 60°C storage 60 days volume expansion rate of the lithium ion batteries obtained in Examples 1-22 and Comparative Examples 1-3 were tested respectively, and the results are shown in Table 2.
[0157] The test method for 25℃ 500 cycles 1C capacity retention rate is as follows:
[0158] The lithium-ion battery is subjected to a charge and discharge cycle test on a charge and discharge instrument, the test temperature is 25°C, the cycle rate is 1C (i.e., both the charge rate and the discharge rate are 1C), the charging voltage is 2.5V to 3.65V, and the capacity retention rate after the cycle is calculated. The capacity retention rate calculation formula for the 25°C cycle is: Capacity retention rate after the 500th cycle = (discharge capacity after the 500th cycle / discharge capacity of the first cycle) * 100%.
[0159] The test method for 45℃ 500 cycles 1C capacity retention rate is as follows:
[0160] The lithium-ion battery was subjected to a charge and discharge cycle test on a charge and discharge instrument, the test temperature was 45°C, the cycle rate was 1C (i.e., both the charge rate and the discharge rate were 1C), the charging voltage was 2.5V to 3.65V, and the capacity retention rate after the cycle was calculated. The capacity retention rate calculation formula for the 45°C cycle is: capacity retention rate after the 500th cycle = (discharge capacity after the 500th cycle / discharge capacity of the first cycle) * 100%.
[0161] The test method for volume expansion rate after storage at 60°C for 60 days is as follows:
[0162] Adjust the temperature of the constant temperature box to 25℃, let it stand for 10min, charge at 0.33C constant current to 3.65V, then charge at 3.65V constant voltage to 0.05C cutoff, let it stand for 30min, and test the initial fully charged volume V0 of the battery cell; adjust the temperature of the constant temperature box to 60℃, let it stand for 30min, charge at 0.33C constant current to 3.65V, let it stand for 1h, cycle twice for recharging, store for 60 days, cool the battery cell, and test the fully charged volume V1 of the battery cell at this time; the volume expansion rate of the battery cell stored at 60℃ for 60 days = (V1 / V0-1)×100%.
[0163] Table 2
[0164]
[0165]
[0166] As can be seen from Table 2, compared with Comparative Examples 1-3, the 25°C 500 cycle 1C capacity retention rate and 45°C 500 cycle 1C capacity retention rate of Example 1-22 are significantly improved, and the 60°C storage 60-day volume expansion rate of Example 1-22 is significantly reduced. It can be seen that when the first additive and the second additive are added to the electrolyte at the same time, the normal high temperature protection effect on the battery cell is excellent. This is because the polysulfide compound (i.e., the second additive) has a higher reduction potential and electrostatic potential than the cyclic sulfate compound (i.e., the first additive). The polysulfide can increase the concentration of lithium ions at the interface, thereby promoting the degradation of the cyclic sulfate, and ultimately increasing the inorganic components mainly composed of lithium sulfide and lithium sulfonate in the SEI interface layer. At high temperatures, the addition of polysulfides can make up for the rate-limiting process of cyclic lithium sulfate on the interface. At the same time, since lithium ions have a strong dipole effect on the sulfonic acid group in the first additive, the ring opening of the first additive can be promoted, inducing the formation of a more solid SEI layer, thereby ensuring the stable performance of high temperature performance.
[0167] It can also be seen from Table 2 that, compared with Example 16, the 500 cycle 1C capacity retention rate and 45°C 500 cycle 1C capacity retention rate of Examples 1 and 6-15 are further improved, and the volume expansion rate of 60 days storage at 60°C of Examples 1 and 6-15 is further reduced. Compared with Example 17, the 500 cycle 1C capacity retention rate and 45°C 500 cycle 1C capacity retention rate of Examples 1 and 6-15 are further improved, and the volume expansion rate of 60 days storage at 60°C of Examples 1 and 6-15 is further reduced. It can be seen that when the mass proportion of the first additive in the electrolyte is in the range of 0.2% to 5%, and the mass proportion of the second additive in the electrolyte is in the range of 0.2% to 5%, the normal high temperature cycle performance and high temperature storage performance of the lithium-ion battery are excellent.
[0168] Compared with Example 1, the 25°C 500 cycle 1C capacity retention rate and 45°C 500 cycle 1C capacity retention rate of Examples 18-22 are further improved, and the 60-day storage volume expansion rate of Examples 18-22 is further reduced. It can be seen that adding the third additive to the electrolyte can further improve the normal high temperature cycle performance and high temperature storage performance of the lithium-ion battery.
[0169] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0170] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. An electrolyte, characterized in that: It includes an electrolyte salt, an organic solvent and an additive, wherein the additive includes a first additive and a second additive, the first additive includes at least one of the compounds shown in Formula I, and the second additive includes at least one of the compounds shown in Formula II; Among them, R1, R2, R3 and R4 are each independently selected from at least one of hydrogen, fluorine, vinyl and methyl, R5 and R6 are each independently selected from at least one of methyl, ethyl, propyl, vinyl, propenyl and (triethoxysilyl)propyl, and n is an integer of 3 to 6.
2. The electrolyte according to claim 1, characterized in that R5 and R6 are the same.
3. The electrolyte according to claim 1, characterized in that n is 3 or 4.
4. The electrolyte according to claim 1, characterized in that The first additive comprises at least one of the following compounds:
5. The electrolyte according to claim 1, characterized in that The second additive includes at least one of the following compounds:
6. The electrolyte according to claim 1, characterized in that The mass proportion of the first additive in the electrolyte is a, satisfying 0.2%≤a≤5%; And / or, the mass proportion of the second additive in the electrolyte is b, satisfying 0.2%≤b≤5%.
7. The electrolyte according to claim 6, characterized in that The ratio of a to b is 1:(0.5~1.5).
8. The electrolyte according to any one of claims 1 to 7, characterized in that The additive includes a third additive including at least one of fluorovinylene carbonate, 2-fluoro-pyridine, and 2-fluoro-5-aminopyridine.
9. The electrolyte according to claim 8, characterized in that The mass proportion of the third additive in the electrolyte is c, satisfying 0.2%≤c≤3%.
10. The electrolyte according to any one of claims 1 to 7, characterized in that The electrolyte salt accounts for 5% to 20% by mass in the electrolyte; and / or, the electrolyte salt comprises at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, lithium bisoxalatoborate, lithium difluorooxalatoborate and lithium bis(trifluoromethanesulfonyl)imide; And / or, the organic solvent includes cyclic carbonate and chain carbonate.
11. A battery, characterized in that: The electrolyte comprising the electrolyte according to any one of claims 1 to 10.
12. An electricity system, characterized in that: include: Electrical equipment, and An energy storage device, wherein the energy storage device supplies power to the electrical equipment, and the energy storage device comprises the electrolyte according to any one of claims 1 to 10 or the battery according to claim 11.
Citation Information
Patent Citations
Electrolyte, electrochemical device and electronic device
CN116544503A
Electrolyte, secondary battery containing electrolyte, battery pack and electric equipment
CN117728035A
Electrolyte for Lithium Secondary Battery and Lithium Secondary Battery Including the Same
US20200127333A1
Nonaqueous electrolytic solution additive, nonaqueous electrolytic solution including same, and nonaqueous electrolytic solution secondary battery
US20230091033A1
Electrolyte, secondary battery comprising same, battery module, battery pack, and electric apparatus
WO2023220857A1
Cited By
Electrolyte, battery containing electrolyte, energy storage device and electric equipment
CN119481286A
Electrolyte, battery and electric system
WO2026031895A1